Catalyst for synthesizing 2, 6-dimethylphenol as well as preparation method and application of catalyst

By using activated alumina pellet carriers and Fe and Mg metal salts to prepare a bimetallic oxide catalyst during the synthesis of 2,6-dimethylphenol, the problems of low activity and short life of the existing catalysts were solved, and efficient Catalytic performance and long life enhance the value of industrial applications.

CN118807746APending Publication Date: 2024-10-22SHANDONG JUCAI POLYMER MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410794565.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the process of synthesizing 2,6-dimethylphenol, existing catalysts have high reaction temperature, low activity, poor selectivity, easy carbon deposition and short life, making it difficult to meet the needs of industrial production.

Method used

Activated alumina pellets are used as carriers, combined with Fe and Mg metal salts, and a bimetallic oxide catalyst is prepared through programmed temperature heating and alkali solution dripping, and the reaction conditions are optimized to improve catalytic performance.

Benefits of technology

It achieves high conversion rate and selectivity, extends the catalyst life, reduces the carbon deposition rate, and improves the economy and production efficiency of the reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807746A_ABST
    Figure CN118807746A_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst for synthesizing 2, 6-dimethylphenol as well as a preparation method and application of the catalyst, and belongs to the technical field of catalyst materials. Through screening of a series of catalysts, the efficient catalyst which takes the bimetallic oxide as the active component is prepared by taking the activated alumina pellets as the carrier, taking Fe and Mg metal salts as key components and adopting a special catalyst synthesis process, and the catalyst shows excellent catalytic performance under specific process conditions, and can be used for preparing the catalyst with the bimetallic oxide as the active component. The conversion rate of phenol is 92% or above, the selectivity of 2, 6-dimethylphenol is 76% or above, the selectivity of 2, 6-dimethylphenol and o-cresol reaches nearly 90%, the activity of a small-scale test catalyst is not inactivated within 300 hours, the catalyst is simple to prepare and convenient for industrial production, the activity of the catalyst and the selectivity of a 2, 6-dimethylphenol product are improved, the carbon deposition rate of the catalyst is reduced, and the catalyst is suitable for industrial production. The service life of the catalyst is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst materials, and specifically relates to a catalyst for synthesizing 2,6-dimethylphenol and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] 2,6-Dimethylphenol is an important fine chemical intermediate and polymer material monomer. It is mainly used in the synthesis of polyphenylene ether (PPO). In addition, it can also be used to synthesize 2,6-dimethylaniline (pesticide, dye intermediate) and antioxidant. At present, the mainstream route for synthesizing 2,6-dimethylphenol is the gas phase phenol alkylation method, which uses phenol as raw material and methanol as methylation agent. Methylation is carried out under the catalytic action of a catalyst to synthesize 2,6-dimethylphenol. The key to synthesizing 2,6-dimethylphenol by the gas phase phenol alkylation method is the catalyst. Metal oxides are the most widely studied catalysts in the alkylation reaction of phenol and methanol. For example, General Motors has researched and developed magnesium oxide catalysts, Asahi Kasei and URBK have developed V-Fe catalysts, Beijing Research Institute of Chemical Industry is committed to the development of MgO series catalysts, and Hunan Changling Petrochemical Technology Development Co., Ltd. has prepared Fe-based composite catalysts using a coprecipitation method. The common problems of the above catalysts are that the reaction temperature is relatively high (400-450°C), the activity is relatively low (the conversion rate is about 80%), the selective carbon deposition is serious, and the catalyst life is relatively short. Therefore, the development of a new catalyst system is the key to research and development.

[0004] The catalytic performance of simple metal oxides is generally poor. For example, aluminum oxide catalysts will produce anisole, o-cresol and other C-alkylation products, and the product selectivity is poor; oxide catalysts such as titanium dioxide and magnesium oxide have high selectivity for ortho-alkylation, but relatively low reaction activity. At the same time, the required reaction temperature is high (above 450°C), carbon deposition is easy, and the service life is short. Compared with single metal oxides, the reaction performance of two-component and multi-component metal oxide composite catalysts is generally higher, and it is also the focus of research by scientific researchers. For example, under the same reaction conditions, a small amount of vanadium pentoxide-modified zirconium oxide catalyst can increase the conversion rate of phenol from 30% to 91%, and the selectivity of 2,6-dimethylphenol from 38% to 60%. Therefore, it is urgent to develop new and efficient bimetallic and multimetallic composite oxide catalysts, change the acid-base strength and type of the catalyst, and optimize the synergy between the two metals to improve the activity of the catalyst, the selectivity of the product, and the life of the catalyst. Summary of the invention

[0005] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a catalyst for synthesizing 2,6-dimethylphenol and a preparation method and application thereof. The present invention provides a highly active and highly selective 2,6-dimethylphenol catalyst, which exhibits good catalytic performance.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] The first aspect of the present invention provides a method for preparing a catalyst for synthesizing 2,6-dimethylphenol, comprising the following steps:

[0008] Dissolve iron salt and magnesium salt in water, add activated alumina ball carrier to obtain solution A;

[0009] Adding an alkaline solution containing sodium carbonate dropwise to solution A until the pH of solution A is 9-10, and allowing the solution to stand to obtain a catalyst precursor;

[0010] The catalyst precursor is subjected to programmed temperature heating to obtain a catalyst for synthesizing 2,6-dimethylphenol.

[0011] In some embodiments of the present invention, solution A is prepared based on the maximum water absorption capacity of the activated alumina bead carrier, the mass loading of metallic iron on the activated alumina bead carrier is 0.5-1.2%, and the molar ratio of iron salt to magnesium salt is (1-3):1.

[0012] In some embodiments of the present invention, the particle size of the activated alumina spherical carrier is 3-4 mm, and the specific surface area is 240-250 m 2 / g, and the saturated water absorption capacity is 0.60-0.70g / g.

[0013] In some embodiments of the present invention, the base in the alkaline solution containing sodium carbonate is an inorganic base;

[0014] The concentration of the inorganic base is 0.05-0.1 mol / L, and the molar ratio of sodium carbonate to the inorganic base is 2:1.

[0015] In some embodiments of the present invention, the standing is 2-3 hours.

[0016] In some embodiments of the present invention, the programmed temperature heating is first kept at 78-82°C for 3.8-4.2 hours, then heated to 275-285°C, kept for 1.8-2.2 hours, and then heated to 545-555°C, kept for 3.8-4.2 hours.

[0017] The second aspect of the present invention provides a catalyst for synthesizing 2,6-dimethylphenol, wherein the catalyst is prepared by the above-mentioned preparation method.

[0018] The third aspect of the present invention provides a use of the above catalyst in catalyzing the synthesis of 2,6-dimethylphenol from phenol and methanol by a gas phase process.

[0019] A fourth aspect of the present invention provides a method for synthesizing 2,6-dimethylphenol, comprising the following steps:

[0020] The catalyst is loaded into a fixed bed reactor, wherein the catalyst is the above-mentioned catalyst for synthesizing 2,6-dimethylphenol;

[0021] The starting reaction raw materials are prepared in a molar ratio of phenol:methanol:water=1:2.5-3:0.2-0.5 and added into the fixed bed reactor, and reacted at 370-380° C. and 0.1-0.75 MPa to obtain 2,6-dimethylphenol.

[0022] In some embodiments of the present invention, the reaction space velocity is controlled at 0.5-1.3h -1 .

[0023] The beneficial effects of the present invention are:

[0024] The invention develops a catalyst with activated alumina beads as carriers, Fe and Mg metal salts as key components, and a special catalyst synthesis process to prepare a high-efficiency catalyst with bimetallic oxide as active components. The catalyst shows excellent catalytic performance under specific process conditions, with a phenol conversion rate of more than 92%, a 2,6-dimethylphenol selectivity of more than 76%, and a selectivity of 2,6-dimethylphenol and o-cresol of nearly 90%. The activity of the catalyst in a small test is as high as 300 hours without deactivation. The catalyst is simple to prepare and is convenient for industrial production. The activity of the catalyst and the selectivity of the 2,6-dimethylphenol product are improved, the carbon deposition rate of the catalyst is reduced, and the service life of the catalyst is improved, thereby improving the economy of the reaction and the production efficiency of the enterprise, and having good industrial application value.

[0025] The present invention also optimizes the reaction process of synthesizing 2,6-dimethylphenol, optimizes the reaction process by adjusting parameters such as the distribution ratio of reaction raw material components, reaction temperature, reaction pressure, etc., further improves the activity and selectivity of the catalyst, reduces the carbon deposition rate, increases the service life, and improves the economy of the reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0027] Figure 1This is a diagram of the catalyst life evaluation of the A1 catalyst prepared in Example 1 of the present invention under the R0 reaction condition. DETAILED DESCRIPTION

[0028] The first typical embodiment of the present invention provides a method for preparing a catalyst for synthesizing 2,6-dimethylphenol, comprising the following steps:

[0029] Dissolve iron salt and magnesium salt in water, add activated alumina ball carrier to obtain solution A;

[0030] Adding an alkaline solution containing sodium carbonate dropwise to solution A until the pH of solution A is 9-10, and allowing the solution to stand to obtain a catalyst precursor;

[0031] The catalyst precursor is subjected to programmed temperature heating to obtain a catalyst for synthesizing 2,6-dimethylphenol.

[0032] The present invention uses activated alumina beads as carriers, Fe and Mg metal salts as key components, and prepares efficient catalysts with bimetallic oxides as active components through a special catalyst synthesis process. The catalyst exhibits excellent catalytic performance under specific process conditions. Specifically, the present invention tests the saturated water absorption capacity of the activated alumina bead carrier before loading, prepares a salt solution containing bimetallic cations with the maximum water absorption capacity, and in order to improve the binding force of metal ions on the catalyst surface, adopts an equal volume impregnation method and a method of dripping a low concentration composite alkali solution to prepare a catalyst precursor, and then adopts a programmed temperature rise method to prepare a composite metal oxide catalyst. In the preparation process of the present invention, by optimizing the carrier of the catalyst, the type of key active components, the content of the components and the preparation process, a highly active and highly selective 2,6-dimethylphenol catalyst is developed. The catalyst exhibits good catalytic performance, the phenol conversion rate is above 92%, the selectivity of 2,6-dimethylphenol is above 76%, the selectivity of 2,6-dimethylphenol and o-cresol reaches nearly 90%, and the activity of the small test catalyst is up to 300 hours without deactivation, which has excellent industrialization prospects.

[0033] In some examples of this embodiment, solution A is prepared based on the maximum water absorption capacity of the activated alumina bead carrier, the mass loading of metallic iron on the activated alumina bead carrier is 0.5-1.2%, and the molar ratio of iron salt to magnesium salt is (1-3):1.

[0034] The said preparation of solution A based on the maximum water absorption capacity of the activated alumina bead carrier specifically means that during the preparation of solution A, the mass of water is equal to the mass of the activated alumina bead carrier multiplied by its maximum water absorption capacity. The said mass loading amount of metallic iron on the activated alumina bead carrier specifically means the mass of metallic iron as a percentage of the mass of the activated alumina bead carrier, 0.5-1.2% means that the mass of metallic iron is 0.5-1.2% of the mass of the activated alumina bead carrier, specifically 0.5%, 0.8%, 1.0% or 1.2%.

[0035] The molar ratio of the iron salt to the magnesium salt is (1-3):1, specifically 1:1, 1.5:1, 2:1 or 3:1.

[0036] In some embodiments of this embodiment, the particle size of the activated alumina spherical carrier is 3-4 mm; the specific surface area is 240-250 m 2 / g, specifically 240m 2 / g, 241m 2 / g, 242m 2 / g, 243m 2 / g, 244m 2 / g, 245m 2 / g, 246m 2 / g, 247m 2 / g, 248m 2 / g, 249m 2 / g or 250m 2 / g; the saturated water absorption capacity is 0.60-0.70g / g, specifically 0.60g / g, 0.61g / g, 0.62g / g, 0.65g / g, 0.66g / g, 0.68g / g or 0.70g / g.

[0037] The activated alumina bead carrier of the present invention is a conventional commercially available product and can be purchased, for example, from Zibo Beige Industry and Trade Co., Ltd. or other manufacturers.

[0038] In some examples of this embodiment, the base in the alkaline solution containing sodium carbonate is an inorganic base;

[0039] The concentration of the inorganic base is 0.05-0.1 mol / L, and the molar ratio of sodium carbonate to the inorganic base is 2:1.

[0040] Wherein, the inorganic base can be sodium hydroxide.

[0041] In some examples of this implementation manner, the standing is for 2-3 hours.

[0042] In some examples of this embodiment, the programmed temperature heating is first kept at 78-82°C for 3.8-4.2 hours, then heated to 275-285°C, kept for 1.8-2.2 hours, and then heated to 545-555°C, kept for 3.8-4.2 hours.

[0043] Preferably, the programmed temperature heating is aimed at removing moisture in stages and carrying out decomposition reaction of metal compounds. The programmed temperature heating process is to keep warm at 80°C for 4 hours to ensure that the surface of the precursor is fully dried; then heat to 280°C and keep warm for 2 hours to ensure the removal of internal crystallization water; then heat to 550°C and keep warm for 4 hours to ensure that the metal salt compound is completely decomposed into a composite metal oxide, thereby obtaining an Fe-Mg composite oxide catalyst loaded with activated alumina beads.

[0044] A second typical embodiment of the present invention provides a catalyst for synthesizing 2,6-dimethylphenol, wherein the catalyst is prepared by the above-mentioned preparation method.

[0045] A third typical embodiment of the present invention provides a use of the above catalyst in catalyzing the synthesis of 2,6-dimethylphenol from phenol and methanol by a gas phase process.

[0046] A fourth typical embodiment of the present invention provides a method for synthesizing 2,6-dimethylphenol, comprising the following steps:

[0047] The catalyst is loaded into a fixed bed reactor, wherein the catalyst is the above-mentioned catalyst for synthesizing 2,6-dimethylphenol;

[0048] The starting reaction materials were prepared according to the molar ratio of phenol:methanol:water=1:2.5-3:0.2-0.5 and added to the fixed bed reactor. The air velocity was controlled at 0.5-1.3h -1 , react at 370-380°C and 0.1-0.75Mpa to obtain 2,6-dimethylphenol.

[0049] The present invention optimizes the reaction process of the prepared catalyst, optimizes the molar ratio of each component in the raw material, the reaction temperature and the reaction pressure, obtains good catalytic reaction results, reduces the carbon deposition rate of the catalyst, increases the life span, improves the economy of the reaction, and increases the profit of the enterprise.

[0050] The reaction product obtained by the present invention enters a product collection tank after being air-cooled or water-cooled, and is used for testing and analyzing the reaction product.

[0051] In some embodiments of the present invention, the amount of the catalyst is...

[0052] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0053] The raw materials used in the present invention are all conventional commercial products and can be purchased. For example, the particle size of the activated alumina ball carrier used is 3-4 mm, and the specific surface area is 242 m 2 / g, purchased from Zibo Beige Industry and Trade Co., Ltd.

[0054] Example 1

[0055] A method for preparing a catalyst for synthesizing 2,6-dimethylphenol comprises the following steps:

[0056] Firstly, the saturated water absorption capacity of the activated alumina bead carrier was measured to be 0.62 g / g. Three portions of 124 mL of deionized water were measured and poured into beakers ①, ②, and ③ respectively. Three portions of 4.32 g of ferric nitrate were weighed and added into beakers ①, ②, and ③ respectively. 1.32 g of magnesium nitrate, 2.65 g of zinc nitrate, and 3.86 g of lanthanum nitrate were weighed and added into beakers ①, ②, and ③ respectively. After the metal salt was completely dissolved, 200 g of alumina beads (particle size 3-4 mm, purchased from Zibo Berg Industry and Trade Co., Ltd.) were added.

[0057] A dilute alkaline solution was prepared, wherein the concentration of sodium hydroxide in the solution was 0.1 mol / L, and the molar ratio of the amount of sodium carbonate substance to sodium hydroxide in the solution was 2:1.

[0058] Add dilute alkali solution dropwise into beakers ①, ②, and ③ until the pH of the solution in the beaker is 9-10, and let it stand for 2-3 hours to obtain three catalyst precursors. Put the obtained catalyst precursors into a muffle furnace and perform programmed temperature heating to remove moisture and decomposition reactions of metal compounds in stages. The programmed temperature heating process is to keep the temperature at 80°C for 4 hours to ensure that the surface of the precursor is fully dried, then heat it to 280°C and keep it for 2 hours to ensure that the internal crystal water is removed, and then heat it to 550°C and keep it for 4 hours to ensure that the metal salt compound is completely decomposed to form a composite metal oxide, thereby obtaining three composite oxide catalysts loaded with activated alumina beads, among which the catalysts prepared in beakers ①, ②, and ③ are marked as A1, A2, and A3, respectively.

[0059] Example 2

[0060] A method for preparing a catalyst for synthesizing 2,6-dimethylphenol comprises the following steps:

[0061] Firstly, the saturated water absorption capacity of the activated alumina bead carrier was measured to be 0.62 g / g. Three portions of 124 mL of deionized water were measured and poured into beakers ①, ②, and ③ respectively. The catalyst was screened according to the mass loading of the metal Fe element of 0.8, 1, and 1.2%. 6.91 g of ferric nitrate and 2.12 g of magnesium nitrate were weighed and added to beaker ①, 8.63 g of ferric nitrate and 2.65 g of magnesium nitrate were weighed and added to beaker ②, 10.36 g of ferric nitrate and 3.17 g of magnesium nitrate were weighed and added to beaker ③. After the metal salt was completely dissolved, 200 g of alumina beads (particle size 3-4 mm, purchased from Zibo Berg Industry and Trade Co., Ltd.) were added.

[0062] A dilute alkaline solution was prepared, wherein the concentration of sodium hydroxide in the solution was 0.1 mol / L, and the molar ratio of the amount of sodium carbonate substance to sodium hydroxide in the solution was 2:1.

[0063] Add dilute alkali solution dropwise into beakers ①, ②, and ③ until the pH of the solution in the beaker is 9-10, and let it stand for 2-3 hours to obtain three catalyst precursors. Put the obtained catalyst precursors into a muffle furnace and perform programmed temperature heating to remove moisture and decomposition reactions of metal compounds in stages. The programmed temperature heating process is to keep the temperature at 80°C for 4 hours to ensure that the surface of the precursor is fully dried, then heat it to 280°C and keep it for 2 hours to ensure that the internal crystal water is removed, and then heat it to 550°C and keep it for 4 hours to ensure that the metal salt compound is completely decomposed to form a composite metal oxide, thereby obtaining three Fe-Mg composite oxide catalysts supported by activated alumina beads, among which the catalysts prepared in beakers ①, ②, and ③ are marked as B1, B2, and B3, respectively.

[0064] Example 3

[0065] A method for preparing a catalyst for synthesizing 2,6-dimethylphenol comprises the following steps:

[0066] Firstly, the saturated water absorption capacity of the activated alumina bead carrier was measured to be 0.62 g / g. Three portions of 124 mL of deionized water were measured and poured into beakers ①, ②, and ③. Three portions of 4.32 g of ferric nitrate were weighed and added to beakers ①, ②, and ③. 2.65 g, 1.76 g, and 0.88 g of magnesium nitrate were weighed and added to beakers ①, ②, and ③ respectively. After the metal salt was completely dissolved, 200 g of alumina beads (particle size 3-4 mm, purchased from Zibo Berg Industry and Trade Co., Ltd.) were added.

[0067] A dilute alkaline solution was prepared, wherein the concentration of sodium hydroxide in the solution was 0.1 mol / L, and the molar ratio of the amount of sodium carbonate substance to sodium hydroxide in the solution was 2:1.

[0068] Add dilute alkali solution dropwise into beakers ①, ②, and ③ until the pH of the solution in the beaker is 9-10, and let it stand for 2-3 hours to obtain three catalyst precursors. Put the obtained catalyst precursors into a muffle furnace and perform programmed temperature heating to remove moisture and decomposition reactions of metal compounds in stages. The programmed temperature heating process is to keep the temperature at 80°C for 4 hours to ensure that the surface of the precursor is fully dried, then heat it to 280°C and keep it for 2 hours to ensure that the internal crystal water is removed, and then heat it to 550°C and keep it for 4 hours to ensure that the metal salt compound is completely decomposed to form a composite metal oxide, thereby obtaining three Fe-Mg composite oxide catalysts supported by activated alumina beads, among which the catalysts prepared in beakers ①, ②, and ③ are marked as C1, C2, and C3, respectively.

[0069] Example 4

[0070] A method for preparing a catalyst for synthesizing 2,6-dimethylphenol comprises the following steps:

[0071] First, the saturated water absorption capacity of the HZSM5 carrier was measured to be 0.87 g / g, and the saturated water absorption capacity of the silica ball carrier with the same particle size was 0.76 g / g. 174 mL and 152 mL of deionized water were respectively measured and poured into beakers ① and ②. Two portions of 4.32 g of ferric nitrate were weighed and added to beakers ① and ② respectively. Two portions of 1.32 g of magnesium nitrate were weighed and added to beakers ① and ②. After the metal salt was completely dissolved, 200 g of HZSM5 carrier was added to beaker ①, and 200 g of silica ball carrier was added to beaker ②.

[0072] A dilute alkaline solution was prepared, wherein the concentration of sodium hydroxide in the solution was 0.1 mol / L, and the molar ratio of the amount of sodium carbonate substance to sodium hydroxide in the solution was 2:1.

[0073] Add dilute alkali solution dropwise into beakers ① and ② until the pH of the solution in the beakers is 9-10, and let it stand for 2-3 hours to obtain three catalyst precursors. Put the obtained catalyst precursors into a muffle furnace and perform programmed temperature heating to remove moisture and decomposition reactions of metal compounds in stages. The programmed temperature heating process is to keep the temperature at 80°C for 4 hours to ensure that the surface of the precursor is fully dried, then heat it to 280°C and keep it for 2 hours to ensure that the internal crystal water is removed, and then heat it to 550°C and keep it for 4 hours to ensure that the metal salt compound is completely decomposed to form a composite metal oxide, thereby obtaining three composite oxide catalysts loaded with activated alumina beads, among which the catalysts prepared in beakers ① and ② are marked as D1 and D2, respectively.

[0074] Example 5

[0075] The catalyst prepared in Example 1-4 was used to evaluate the alkylation of phenol to prepare 2,6-dimethylphenol. This operating condition is defined as R0. Specifically, the catalyst prepared in Example 1-4 was loaded into a fixed bed reactor, and the reaction raw material ratio was n (phenol): n (methanol): n (water) = 1:2.5:0.2. The air velocity was controlled at 1 h -1 , reaction temperature 375℃, reaction pressure 0.25MPa, the reaction product enters the product collection tank after air cooling and water cooling, and is used for testing and analysis of the reaction product.

[0076] For the R0 reaction condition, the reaction effects of each catalyst are shown in Table 1.

[0077] Table 1 Reaction effects of different catalysts under RO conditions

[0078]

[0079] Figure 1 The catalyst evaluation life of A1 catalyst under R0 reaction conditions is shown in the figure. It can be seen from the figure that A1 catalyst has worked continuously for 300 hours and its catalytic activity is still very high without deactivation. After 300 hours, the selectivity of 2,6-dimethylphenol is above 84% and the phenol conversion rate is above 92%.

[0080] Example 6

[0081] The reaction process was optimized using A1 catalyst. The raw material ratios were n(phenol): n(methanol): n(water) = 1:2.8:0.2 and n(phenol): n(methanol): n(water) = 1:3:0.2, which were defined as reaction conditions R1 and R2, respectively. The air velocity was controlled at 1 h -1 , reaction temperature 375℃, reaction pressure 0.25MPa, the reaction product enters the product collection tank after air cooling and water cooling, and is used for testing and analysis of the reaction product.

[0082] Example 7

[0083] The reaction process was optimized with A1 catalyst. The raw material ratios were n(phenol): n(methanol): n(water) = 1:2.5:0.3, n(phenol): n(methanol): n(water) = 1:2.5:0.4, and n(phenol): n(methanol): n(water) = 1:2.5:0.5, which were defined as reaction conditions R3, R4, and R5, respectively. The space velocity was controlled at 1 h -1 , reaction temperature 375℃, reaction pressure 0.25MPa, the reaction product enters the product collection tank after air cooling and water cooling, and is used for testing and analysis of the reaction product.

[0084] Example 8

[0085] The reaction process was optimized using A1 catalyst. The raw material ratio was n(phenol): n(methanol): n(water) = 1:2.5:0.2. The air velocity was controlled at 0.5, 0.7, and 1.3 h -1 The three reaction conditions are defined as R6, R7, and R8, with a reaction temperature of 375°C and a reaction pressure of 0.25MPa. The reaction products are air-cooled and water-cooled before entering the product collection tank for testing and analysis of the reaction products.

[0086] Example 9: (Effect of changes in process conditions on results)

[0087] The reaction process was optimized using A1 catalyst. The raw material ratio was n(phenol): n(methanol): n(water) = 1:2.5:0.2, and the space velocity was controlled at 1h -1 The two working conditions of reaction temperature of 370 and 380℃ are defined as R9 and R10, the reaction pressure is 0.25MPa, and the reaction products enter the product collection tank after air cooling and water cooling for the test and analysis of the reaction products.

[0088] Example 10: (Effect of changes in process conditions on results)

[0089] The reaction process was optimized using A1 catalyst. The raw material ratio was n(phenol): n(methanol): n(water) = 1:2.5:0.2, and the space velocity was controlled at 1h -1 The reaction temperature is 375°C, and the three working conditions of reaction pressure of 0.1, 0.5, and 0.75MPa are defined as working conditions R11, R12, and R13. The reaction products are air-cooled and water-cooled before entering the product collection tank for testing and analysis of the reaction products.

[0090] The effects under different reaction conditions R1-R13 under A1 catalyst are shown in Table 2.

[0091] Table 2 Reaction effects of A1 catalyst under different working conditions

[0092]

[0093]

[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a catalyst for synthesizing 2,6-dimethylphenol, It is characterized in that The steps include: Dissolve iron salt and magnesium salt in water, add activated alumina ball carrier to obtain solution A; Adding an alkaline solution containing sodium carbonate dropwise to solution A until the pH of solution A is 9-10, and allowing the solution to stand to obtain a catalyst precursor; The catalyst precursor is subjected to programmed temperature heating to obtain a catalyst for synthesizing 2,6-dimethylphenol.

2. The preparation method according to claim 1, It is characterized in that Solution A is prepared based on the maximum water absorption capacity of the activated alumina bead carrier, the mass loading of metallic iron on the activated alumina bead carrier is 0.5-1.2%, and the molar ratio of iron salt to magnesium salt is (1-3):

1.

3. The preparation method according to claim 1, It is characterized in that The particle size of the activated alumina ball carrier is 3-4 mm, and the specific surface area is 240-250 m 2 / g, and the saturated water absorption capacity is 0.60-0.70g / g.

4. The preparation method according to claim 1, It is characterized in that The alkali in the alkaline solution containing sodium carbonate is an inorganic alkali; The concentration of the inorganic base is 0.05-0.1 mol / L, and the molar ratio of sodium carbonate to the inorganic base is 2:

1.

5. The preparation method according to claim 1, It is characterized in that The step of leaving the mixture to stand is 2-3 hours.

6. The preparation method according to claim 1, It is characterized in that The programmed temperature heating is firstly kept at 78-82°C for 3.8-4.2h, then heated to 275-285°C, kept for 1.8-2.2h, then heated to 545-555°C, kept for 3.8-4.2h.

7. A catalyst for synthesizing 2,6-dimethylphenol, It is characterized in that The catalyst is prepared by the preparation method described in any one of claims 1 to 6.

8. Use of the catalyst according to claim 7 in catalyzing the synthesis of 2,6-dimethylphenol from phenol and methanol by a gas phase process.

9. A method for synthesizing 2,6-dimethylphenol, It is characterized in that The steps include: Loading a catalyst into a fixed bed reactor, wherein the catalyst is the catalyst for synthesizing 2,6-dimethylphenol as claimed in claim 7; According to Phenol: The starting reaction raw materials are prepared in a molar ratio of methanol: water = 1:2.5-3:0.2-0.5, added to the fixed bed reactor, and reacted at 370-380° C. and 0.1-0.75 MPa to obtain 2,6-dimethylphenol.

10. The method for synthesizing 2,6-dimethylphenol as claimed in claim 9, It is characterized in that The reaction space velocity is controlled at 0.5-1.3h -1 .

Citation Information

Patent Citations

  • Alkylation catalyst and method for making alkylated phenols

    CN101219930A

  • Catalyst for synthesizing 2,6-xylenol as well as preparation method of catalyst and method for synthesizing 2,6-xylenol

    CN103084213A

  • Method for improving selectivity of anisole, o-cresol and 2, 6-dimethylphenol

    CN118164828A