Double-active-metal dehydrogenation catalyst as well as preparation method and application thereof

By loading dual-active metals and alkali metals or alkaline earth metals on the modified carrier, a highly active and stable addition and dehydrogenation catalyst is prepared, which solves the problems of cumbersome preparation process and poor stability of the existing catalyst, and achieves low-cost, high-efficiency hydrogenation hydrogen storage reaction.

CN118807754APending Publication Date: 2024-10-22WUHAN HYNERTECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310390750.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing hydrogenation and dehydrogenation catalyst preparation processes are cumbersome, have poor stability, and have many side reactions, resulting in high costs for organic liquid hydrogen storage technology and limiting the development of the hydrogen energy industry chain.

Method used

A dual-active metal addition and dehydrogenation catalyst is used to prepare a catalyst with high activity and stability by loading active metals A and B on a modified carrier, combined with alkali metal, alkaline earth metal or non-metal atoms modified carrier, to reduce the activity The dosage of component metals can reduce side reactions and improve the dispersion and stability of the catalyst.

Benefits of technology

It is possible to improve the activity and stability of the catalyst at a lower cost, reduce the occurrence of side reactions, extend the service life of the catalyst, and improve the circulation and efficiency of the hydrogenation hydrogen storage system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004175639420000081
    Figure BDA0004175639420000081
  • Figure BDA0004175639420000082
    Figure BDA0004175639420000082
Patent Text Reader

Abstract

The invention discloses a double-active-metal dehydrogenation catalyst as well as a preparation method and application thereof. The double-active-metal dehydrogenation catalyst mainly comprises active metals A and B which are jointly loaded on a modified carrier. The prepared double-active-metal dehydrogenation catalyst can be used for hydrogenation of a reversible hydrogenation hydrogen storage system and dehydrogenation of hydrogenation products of the reversible hydrogenation hydrogen storage system. The double-metal component of the double-active-metal dehydrogenation catalyst shows a synergistic effect and has more excellent catalytic activity than a single-metal-component catalyst, the dosage of the active component metal can be greatly reduced, and meanwhile, the dispersity of the double-component active metal is improved, so that by properly reducing the content of the active component metal, the catalytic activity of the dehydrogenation catalyst is improved, and the dehydrogenation effect of the dehydrogenation catalyst is improved. The preparation process of the catalyst can be further simplified; the alkali metal, alkaline earth metal or non-metal atom modified carrier is adopted, so that active metal atom sites can be better fixed, the phenomena of active metal agglomeration and powder removal are effectively inhibited, the stability and the cyclicity of the catalyst are improved, and the service life of the catalyst is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and particularly relates to a dual-active metal dehydrogenation catalyst and a preparation method and application thereof. Background Art

[0002] The basis of the "hydrogen economy" is to use hydrogen as a new clean energy for storage, transportation, and power generation. Therefore, hydrogen needs to be produced in tons. Traditional hydrogen storage and transportation technologies such as high-pressure gaseous hydrogen storage, low-temperature liquefied hydrogen storage, and solid hydrogen storage restrict the application of hydrogen energy due to high costs and safety requirements. Organic liquid hydrogen storage materials (LOHCs) are a type of hydrogen storage material with a fully reversible hydrogenation-dehydrogenation cycle. In recent years, they have become the focus of hydrogen research due to their reversibility and zero CO2 emissions. The principle is to achieve hydrogen storage (chemical bonding) through the reversible reaction and hydrogenation reaction of unsaturated liquid organic matter such as olefins, alkynes or aromatic hydrocarbons and hydrogen, and to achieve hydrogen release through dehydrogenation reactions, making hydrogen storage and release safe and efficient. Since the hydrogenated Hn-LOHCs compounds have similar properties to crude oil derivatives (such as diesel and gasoline), they can be transported over long distances using existing liquid fuel transportation logistics (such as pipelines, ships, and trucks). Therefore, it is very feasible to transition to the "hydrogen economy" with existing infrastructure.

[0003] Organic liquid hydrogen storage materials mainly include traditional organic liquid hydrogen storage materials and new organic liquid hydrogen storage materials. Traditional organic liquid hydrogen storage molecules are mainly aromatic benzene-cyclohexane, toluene-methylcyclohexane, naphthalene-decalin, dibenzyltoluene-perhydrodibenzyltoluene systems. Such traditional organic liquid hydrogen storage molecules can change the properties of organic compounds by changing the number of substituents, bridging methods, etc. At present, there are still problems such as high temperature required for the dehydrogenation process and easy occurrence of side reactions such as cracking and disproportionation, resulting in reduced purity of the generated hydrogen. New organic liquid hydrogen storage materials are mainly condensed aromatic molecules containing heteroatoms (O, N, S), among which N-heterocyclic systems such as quinoline and its derivatives, indole and its derivatives, carbazole and its derivatives are the most studied new organic liquid hydrogen storage materials. The hydrogen storage capacity is usually expressed in mass fraction (wt%), and the reaction enthalpy ΔH in kJ / mol H2 represents the energy value released in the hydrogenation reaction, and the energy value required in the dehydrogenation reaction. For example, the dehydrogenation temperature of methylcyclohexane used by Chiyoda in Japan is as high as 350℃~400℃. The selection of LOHCs with more than 4wt% hydrogen storage and low reaction enthalpy (-15kcal / mol H2≤ΔH≤-10kcal / mol H2) has low external energy demand, and the hydrogen storage capacity can meet most of the actual needs, thereby improving the overall efficiency of the dehydrogenation process and facilitating the industrial application of the hydrogen energy industry chain.

[0004] The key to realizing the hydrogenation and dehydrogenation of LOHCs is to add dehydrogenation catalysts. Catalysts can not only reduce the reaction temperature, but also improve the reaction rate of chemical hydrogen storage technology. The hydrogenation and dehydrogenation of LOHCs are reversible reactions. They follow Le Chatelier's principle. Hydrogenation releases heat and dehydrogenation absorbs heat. By changing the temperature, pressure and concentration of the reactants, the equilibrium direction of the reaction can be effectively controlled to move toward hydrogenation or dehydrogenation. Under pressurized conditions, the catalyst adsorbs LOHCs, causing the unsaturated bonds to vibrate and break, and H2 is added; under normal pressure conditions, the catalyst adsorbs Hn-LOHCs, CH vibrates and breaks, and H2 is removed.

[0005] The essence of the hydrogenation and dehydrogenation process is the bond vibration breaking to achieve H2 storage and release. In theory, it can catalyze hydrogenation and dehydrogenation at the same time, but because the hydrogenation and dehydrogenation reaction pathways are opposite, based on cost, yield and other considerations, the choice of catalyst is generally different. Hydrogenation catalysts mainly include nickel catalysts, palladium and platinum catalysts, ruthenium catalysts and rhodium catalysts. Conventional hydrogenation catalysts are nickel metal catalysts with aluminum as the carrier, while for deep aromatics catalysis, precious metal catalysts are the first choice. Dehydrogenation catalysts are mainly precious metal catalysts, non-precious metal catalysts and mixed catalysts. Precious metal catalysts have high activity and can improve the dehydrogenation efficiency of organic liquid hydrogen storage materials. In theory, catalysts that can be used for hydrogenation can also be used for dehydrogenation, but in fact, the reaction pathways of hydrogenation and dehydrogenation processes are opposite, so it is very demanding to meet the requirements of catalysts for both hydrogenation and dehydrogenation processes. Most of the applicable bifunctional catalysts are based on precious metals as the main components, mostly for the research of Pt, Pd, and Ir, and are rarely used in practice. Hydrogenation and dehydrogenation bifunctional catalysts based on non-precious metal elements have not been used.

[0006] Current dehydrogenation catalysts generally use non-precious metal catalysts with active component metals such as Cr, Fe, Co, Ni, Cu or Zn. Such catalysts usually use higher loadings and often have disadvantages such as complicated preparation process, poor stability, and high side reactions, which increases the cost of organic liquid hydrogen storage technology and greatly limits the development of organic liquid hydrogen storage technology. Summary of the invention

[0007] The purpose of the present invention is to provide a dual-active metal dehydrogenation catalyst and a preparation method and application thereof in view of the defects of the prior art.

[0008] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a dual-active metal dehydrogenation catalyst, wherein the catalyst is active metals A and B co-loaded on a modified carrier; the active metal A is Cr, Fe, Co, Ni, Cu or Zn, accounting for 15% to 25% of the total mass of the catalyst; the active metal B is Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Y, Mo or W, accounting for 5% to 15% of the total mass of the catalyst; the modified carrier is made of silicon aluminum oxide, transition metal oxide, rare earth metal oxide, carbon material or MOFs through modification.

[0009] Furthermore, the silicon aluminum oxide carrier is Al2O3, SiO2, SBA-15, KIT-6, MCM-41 or ZSM-5; the transition metal oxide carrier is ZnO2, CeO2, TiO2, WO3, MoO3, Cr2O3 or Co3O4; the rare earth metal oxide carrier is La2O3 or CeO2; the carbon material carrier is activated carbon, graphite, graphene or carbon nanotubes; and the MOFs are ZIF, MIL, UIO, Nu, PCN or CPL series.

[0010] Furthermore, the modified carrier has a diameter of 0.3-0.8 mm, a pore size of 15-30 nm, and a specific surface area of ​​400-1200 m 2 / g, pore volume is 0.75-2.0cm 3 / g; strength is 5-100N / grain, abrasion is 0.01%-0.05%, and bulk density is 0.3-0.7g / cm 3 .

[0011] A method for preparing the above-mentioned dual-active metal dehydrogenation catalyst comprises the following steps:

[0012] (1) A modifier and a surfactant are prepared into a mixed solution, carrier powder C is poured into the mixed solution, stirred and ultrasonically subjected to 0.5 to 2 h, completely dried in a drying oven, and then calcined in a muffle furnace at 350 to 550° C. for 2 to 8 h, with a heating rate of 2 to 10° C. / min. After calcination, the powder is crushed and ground into 300 to 500 mesh, a binder and a solvent are added, kneaded, extruded and spheronized, and the modified carrier is obtained after calcination;

[0013] (2) preparing an aqueous solution of metal salts of metals A and B, adding the modified carrier, stirring and co-impregnating, the impregnation temperature is 30-50° C., ultrasonicating for 0.5-2 h, then taking out, aging overnight and drying;

[0014] (3) The dried catalyst is placed in a muffle furnace for calcination, and then placed in a tubular furnace for reduction. After reduction, the catalyst is purged with nitrogen gas, and after cooling to room temperature, it is passivated to obtain the target catalyst.

[0015] Furthermore, the modifier in step (1) is a soluble salt of one or more alkali metals or alkaline earth metals selected from the group consisting of Na, K, Mg and Ca, specifically potassium carbonate, potassium nitrate, magnesium nitrate and calcium nitrate; or a soluble organic substance selected from the group consisting of one or more non-metallic substances selected from the group consisting of B, C, N, P, S and Se, specifically urea, dicyandiamide, melamine or cross-linked linear poly(diaryloxyphosphazene).

[0016] Furthermore, the surfactant in step (1) is one or a mixture of two or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyethylene glycol, P123, and F127.

[0017] Furthermore, the binder in step (1) is one or a mixture of two or more of pseudo-boehmite, glass fiber, sesbania powder, microcrystalline cellulose, and polyvinyl alcohol.

[0018] Furthermore, the solvent in step (1) is aluminum sol or silica sol.

[0019] Furthermore, the reaction conditions in step (3) are as follows: calcination temperature is 350-550°C for 2-8h, and the heating rate is 2-10°C / min; reduction temperature is 300-600°C, time is 4-12h, reducing gas is 5%-15% H2 / Ar mixed gas, hydrogen flow rate is 50-250mL / min, and heating rate is 2-10°C / min; nitrogen purge time is 0.5-2h; room temperature is 15-25°C; passivation time is 6-12h, mixed gas is 0.5-1.5% O2 / Ar, and flow rate is 50-250mL / min.

[0020] An application of the above-mentioned dual-active metal dehydrogenation catalyst in a reversible hydrogenation hydrogen storage system.

[0021] Furthermore, the reversible hydrogenation hydrogen storage system includes one or a mixture of two or more π-conjugated reversible hydrogenation hydrogen storage materials; the π-conjugated reversible hydrogenation hydrogen storage material, at 25°C and 1atm, releases 10 to 15 kcal of heat per 1 mol of H2 stored, that is, -15 kcal / mol H2≤ΔH≤-10 kcal / mol H2; and the hydrogen storage density after complete hydrogenation is greater than 4% of the mass of the hydrogen storage material; the π-conjugated reversible hydrogenation hydrogen storage material is solid or liquid, and has a melting point of less than 80°C.

[0022] The prepared dual-active metal dehydrogenation catalyst can be used for the hydrogenation of a reversible hydrogenation hydrogen storage system and the dehydrogenation of its hydrogenation product.

[0023] Application example: Taking fixed bed and reactor applications as examples, the hydrogenation raw material and dehydrogenation raw material are respectively N-propylcarbazole and fully hydrogenated N-propylcarbazole as examples. The actual application is not limited to this:

[0024] Fixed bed hydrogenation reaction conditions: catalyst filling height 10 ~ 30cm, liquid space velocity: 0.3 / h ~ 2.0 / h, reaction temperature: 140 ~ 240 ° C, reaction pressure: 3M ~ 9MPa, hydrogenation conversion rate can reach more than 99%, complete hydrogenation product 60% ~ 98%, stable cycle time can reach 5000h.

[0025] Reactor hydrogenation conditions: the ratio of catalyst to reversible hydrogenation hydrogen storage system is 1:5-1:500, reaction temperature is 140-240°C, reaction pressure is 3M-9MPa, reaction time is 1-2h, hydrogenation conversion rate can reach more than 99%, and complete hydrogenation product is 90%-99%.

[0026] Fixed bed dehydrogenation reaction conditions: dehydrogenation raw materials: catalyst filling height 10 ~ 30cm, liquid space velocity: 0.3 / h ~ 2.0 / h, reaction temperature 160 ~ 260 ℃, reaction pressure less than 3MPa, dehydrogenation conversion rate can reach more than 99%, complete dehydrogenation product 60% ~ 98%, stable cycle time can reach 5000h, if needed, longer use.

[0027] Reactor dehydrogenation conditions: the ratio of catalyst to reversible hydrogenation hydrogen storage system is 1:5-1:20, reaction temperature is 160-240°C, reaction pressure is normal pressure, reaction time is 1-10h, hydrogenation conversion rate can reach more than 99%, and complete dehydrogenation product is 70%-99%.

[0028] The dual-active metal dehydrogenation catalyst prepared in this application has the following advantages:

[0029] (1) Since the non-metallic catalyst has a high loading of active components, it usually requires multiple impregnations to achieve the required loading. After adding a metal promoter, the bimetallic component exhibits a synergistic effect and has better catalytic activity than the single metal component catalyst. It can greatly reduce the amount of active component metal and improve the dispersion of the bicomponent active metal. Therefore, by appropriately reducing the active component metal content, the catalyst preparation process can be further simplified;

[0030] (2) At higher reduction temperatures, the active component metals on the carrier surface tend to agglomerate. Adding an easily reducible auxiliary metal can also lower the reduction temperature of the active component metals that are more difficult to reduce, thereby reducing the occurrence of agglomeration and sintering.

[0031] (3) After adding another active metal, the metal content of the active component is greatly reduced, which can reduce the occurrence of side reactions, further improve product selectivity, and improve the recyclability and service life of the hydrogen storage material;

[0032] (4) Using alkali metals, alkaline earth metals or non-metallic atoms to modify the carrier can better fix the active metal atomic sites, effectively inhibit the occurrence of active metal agglomeration and de-powdering, and improve the stability, cyclability and service life of the catalyst. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiment of the present application will be clearly and completely described below in combination with the embodiment of the present application. Obviously, the described embodiment is only a part of the embodiment of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present application.

[0034] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but includes other steps or units that are not explicitly listed or are inherent to these processes, methods, products or apparatuses.

[0035] Example 1

[0036] (1) Weigh 5 g of sodium carbonate and 3 g of hexadecyltrimethylammonium bromide, add them into 100 mL of deionized water, stir for 30 min, then weigh 100 g of homemade macroporous silica powder and pour it into the mixed solution, stir and ultrasonicate for 1 h, completely dry in a drying oven, grind to 400 mesh, place in a muffle furnace and calcine at 450 ° C for 4 h, with a heating rate of 2 ° C / min, and obtain a SiO2-Al2O3 modified carrier after calcination.

[0037] (2) Weigh 30 g of pseudo-boehmite (alumina content 70%) and place it in a kneader, then add 100 g of Na-SiO2-Al2O3 carrier and 2 g of microcrystalline cellulose, and knead for 20 min. Then, mix 3 g of concentrated nitric acid with 70 g of deionized water and add them to the kneader. After kneading for 30 min, extrude and roll into strips using an extruder, and calcine to obtain a Na-SiO2-Al2O3 spherical carrier.

[0038] (3) Weigh 50 g of nickel chloride and 43 g of copper chloride and dissolve them in 100 mL of deionized water. Stir and ultrasonicate at 40°C until they are completely dissolved. Then weigh 100 g of Na-SiO2-Al2O3 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry. Place it in a muffle furnace and calcine it at 450°C for 4 h, with a heating rate of 2°C / min.

[0039] (4) After calcination, the mixture was placed in a tubular furnace and reduced at 400°C for 4 hours. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, the mixture was purged with nitrogen for 0.5 hours. After the mixture was cooled to room temperature (25°C), the mixture was passivated for 6 hours. The mixed gas was 0.5% O2 / Ar at a flow rate of 100 mL / min. 20% Ni-Cu / Na-SiO2-Al2O3 was obtained.

[0040] Example 2

[0041] (1) Weigh 3 g of potassium nitrate and 2 g of dodecyl dimethyl benzyl ammonium chloride and add them into 100 mL of deionized water, stir for 30 min, then weigh 100 g of homemade macroporous carbon powder and pour it into the mixed solution, stir and ultrasonicate for 1 h, completely dry in a drying oven, grind to 500 mesh, place in a muffle furnace and calcine at 400 ° C for 6 h, with a heating rate of 2 ° C / min, and obtain the KC modified carrier after calcination.

[0042] (2) Weigh 30 g of pseudo-boehmite (alumina content 70%) and place it in a kneader, then add 100 g of KC carrier and 2 g of sesbania powder, and knead for 20 min. Then, mix 4 g of concentrated nitric acid with 70 g of deionized water and add them to the kneader. After kneading for 30 min, extrude and roll into strips using an extruder, and calcine to obtain a KC-Al2O3 spherical carrier.

[0043] (3) Weigh 50 g of nickel nitrate and 50 g of cobalt nitrate and dissolve them in 100 mL of deionized water. Stir and ultrasonicate at 40 °C until they are completely dissolved. Then weigh 100 g of KC-Al2O3 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry. Place it in a muffle furnace and calcine it at 450 °C for 6 h, with a heating rate of 2 °C / min.

[0044] (4) After calcination, the mixture was placed in a tube furnace and reduced at 550°C for 4 hours. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, the mixture was purged with nitrogen for 0.5 hours. After the mixture was cooled to room temperature (25°C), the mixture was passivated for 6 hours. The mixed gas was 0.5% O2 / Ar at a flow rate of 100 mL / min. 20% Ni-Co / KC-Al2O3 was obtained.

[0045] Example 3

[0046] (1) Weigh 3 g of dicyandiamide and 2 g of sodium dodecylbenzene sulfonate, add them into 100 mL of deionized water, stir for 30 min, then weigh 100 g of homemade macroporous silica powder and pour it into the mixed solution, stir and ultrasonicate for 1 h, completely dry in a drying oven, and grind to 500 mesh, place in a muffle furnace and calcine at 400 ° C for 8 h, with a heating rate of 2 ° C / min, and obtain the N-CNTs modified carrier after calcination.

[0047] (2) Weigh 30 g of pseudo-boehmite (alumina content 70%) and place it in a kneader, then add 100 g of N-CNTs carrier and 3 g of glass fiber, and knead for 20 min. Then, mix 5 g of concentrated nitric acid with 70 g of deionized water and add them to the kneader. After kneading for 30 min, extrude and roll into strips using an extruder, and calcine to obtain a N-CNTs-Al2O3 spherical carrier.

[0048] (3) Weigh 49 g of cobalt nitrate hexahydrate and 43 g of copper nitrate trihydrate and dissolve them in 100 mL of deionized water, stir and ultrasonicate at 40 °C until they are completely dissolved, then weigh 100 g of N-CNTs-Al2O3 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry, and place it in a muffle furnace and calcine it at 450 °C for 8 h, with a heating rate of 2 °C / min.

[0049] (4) After calcination, the mixture was placed in a tube furnace and reduced at 400°C for 4 hours. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, it was switched to nitrogen purge for 0.5 hours. After the temperature dropped to room temperature (25°C), it was passivated for 6 hours. The mixed gas was 0.5% O2 / Ar, and the flow rate was 100 mL / min. 20% Cu-Co / N-CNTs-Al2O3 was obtained.

[0050] Example 4

[0051] (1) Weigh 3 g of melamine and 2 g of P123 and add them into 100 mL of deionized water, stir for 30 min, then weigh 100 g of homemade macroporous tungsten trioxide powder and pour it into the mixed solution, stir and ultrasonicate for 1 h, completely dry in a drying oven, and grind to 500 mesh, place in a tubular furnace and calcine at 500 ° C for 4 h in a nitrogen atmosphere, with a heating rate of 2 ° C / min, and the NC-WO3 modified carrier is obtained after calcination.

[0052] (2) Weigh 100 g of NC-WO3 carrier and 5 g of glass fiber, knead for 20 min, then add 70 g of aluminum sol into a kneader, knead for 30 min, extrude and roll into a spherical shape using an extruder, and calcine to obtain a NC-Al2O3 spherical carrier.

[0053] (3) Weigh 73 g of ferric nitrate nonahydrate and 49 g of nickel nitrate hexahydrate and dissolve them in 100 mL of deionized water. Stir and ultrasonicate at 40 °C until they are completely dissolved. Then weigh 100 g of NC-WO3-Al2O3 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry. Place it in a tubular furnace and calcine it at 500 °C for 4 h under a nitrogen atmosphere with a heating rate of 2 °C / min.

[0054] (4) After calcination, the mixture was placed in a tube furnace and reduced at 500°C for 4 hours. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, the mixture was switched to nitrogen purge for 0.5 hours. After the mixture was cooled to room temperature (25°C), the mixture was passivated for 6 hours. The mixed gas was 0.5% O2 / Ar at a flow rate of 100 mL / min. 20% Fe-Ni / NC-WO3-Al2O3 was obtained.

[0055] Example 5

[0056] (1) Weigh 3 g of cross-linked linear poly(diaryloxyphosphazene) and 2 g of F127, add them into 100 mL of deionized water, stir for 30 min, then weigh 100 g of homemade macroporous ZIF powder and pour it into the mixed solution, stir and ultrasonicate for 1 h, completely dry in a drying oven, and grind to 500 mesh, place in a tubular furnace and calcine at 400 °C for 4 h in a nitrogen atmosphere, with a heating rate of 2 °C / min, to obtain the NP-ZIF modified carrier after calcination.

[0057] (2) Weigh 100 g of NP-ZIF carrier and 5 g of polyvinyl alcohol, knead for 20 min, then add 70 g of silica sol into a kneader, knead for 30 min, extrude and roll into a round shape using an extruder, and calcine to obtain a spherical NC-ZIF-SiO2 carrier.

[0058] (3) Weigh 43 g of manganese carbonate and 73 g of basic copper carbonate and dissolve them in 100 mL of deionized water. Stir and ultrasonicate at 40 °C until completely dissolved. Then weigh 100 g of NP-ZIF-SiO2 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry. Place it in a tubular furnace and calcine it at 400 °C for 4 h under a nitrogen atmosphere with a heating rate of 2 °C / min.

[0059] (4) After calcination, the mixture was placed in a tubular furnace and reduced at 400°C for 4 h. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, the mixture was switched to nitrogen purge for 0.5 h. After the mixture was cooled to room temperature (25°C), the mixture was passivated for 6 h. The mixed gas was 0.5% O2 / Ar at a flow rate of 100 mL / min. 20% Mn-Cu / NP-ZIF-SiO2 was obtained.

[0060] Comparative Example 1

[0061] (1) Weigh 5 g of sodium carbonate and 3 g of hexadecyltrimethylammonium bromide, add them into 100 mL of deionized water, stir for 30 min, then weigh 100 g of homemade macroporous silica powder and pour it into the mixed solution, stir and ultrasonicate for 1 h, dry it completely in a drying oven, grind it into 400 mesh, place it in a muffle furnace and calcine it at 450 ° C for 4 h, with a heating rate of 2 ° C / min, and obtain the Na-SiO2-Al2O3 modified carrier after calcination.

[0062] (2) Weigh 30 g of pseudo-boehmite (alumina content 70%) and place it in a kneader, then add 100 g of Na-SiO2-Al2O3 carrier and 2 g of microcrystalline cellulose, and knead for 20 min. Then, mix 3 g of concentrated nitric acid with 70 g of deionized water and add them to the kneader. After kneading for 30 min, extrude and roll into strips using an extruder, and calcine to obtain a Na-Al2O3 spherical carrier.

[0063] (3) Weigh 100 g of nickel nitrate and dissolve it in 100 mL of deionized water. Stir and ultrasonicate at 40° C. until it is completely dissolved. Then weigh 100 g of Na-SiO2-Al2O3 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry. Place it in a muffle furnace and calcine it at 450° C. for 4 h, with a heating rate of 2° C. / min.

[0064] (4) After calcination, the mixture was placed in a tube furnace and reduced at 550°C for 4 hours. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, it was switched to nitrogen purge for 0.5 hours. After the temperature dropped to room temperature (25°C), it was passivated for 6 hours. The mixed gas was 0.5% O2 / Ar, and the flow rate was 100 mL / min. 20% Ni / Na-SiO2-Al2O3 was obtained.

[0065] Comparative Example 2

[0066] (1) Weigh 30 g of pseudo-boehmite (alumina content 70%) and place it in a kneader, then add 100 g of homemade macroporous silica powder and 2 g of microcrystalline cellulose, and knead for 20 min. Then, mix 3 g of concentrated nitric acid with 70 g of deionized water and add them to the kneader. After kneading for 30 min, extrude and roll into strips using an extruder, and calcine to obtain a SiO2-Al2O3 spherical carrier.

[0067] (2) Weigh 49 g of nickel nitrate and 43 g of copper nitrate and dissolve them in 100 mL of deionized water. Stir and ultrasonicate at 40°C until they are completely dissolved. Then weigh 100 g of SiO2-Al2O3 spherical carrier and pour it into the impregnation solution, stir for 30 min, ultrasonicate for 60 min, age overnight and dry. Place it in a muffle furnace and calcine it at 450°C for 4 h, with a heating rate of 2°C / min.

[0068] (3) After calcination, the mixture was placed in a tube furnace and reduced at 550°C for 4 hours. The reducing gas was 5% H2 / Ar mixed gas, the hydrogen flow rate was 100 mL / min, and the heating rate was 2°C / min. After reduction, it was switched to nitrogen purge for 0.5 hours. After the temperature dropped to room temperature (25°C), it was passivated for 6 hours. The mixed gas was 0.5% O2 / Ar, and the flow rate was 100 mL / min. 20% Ni-Cu / SiO2-Al2O3 was obtained.

[0069] The prepared modified carrier-loaded non-noble metal dehydrogenation catalyst can be used for hydrogenation of a reversible hydrogenation hydrogen storage system and dehydrogenation of its hydrogenation product.

[0070] Catalyst hydrogenation or dehydrogenation performance test: Weigh 20g of the catalyst prepared in the above Examples 1-5 and Comparative Examples 1-2 and load it into a fixed bed reactor, heat it to the reaction conditions to test the hydrogenation or dehydrogenation performance of N-methylindole. The hydrogenation reaction is carried out at 210°C and 7MPa, and the dehydrogenation reaction is carried out at 180°C and normal pressure. Unhydrogenated N-methylindole or fully hydrogenated 8-N-methylindole is added to the reactor at a rate of 0.6mL / min through a liquid delivery pump. The hydrogen inlet flow rate during the hydrogenation reaction is 1000mL / min, and the space velocity during the hydrogenation or dehydrogenation reaction is 1.2h -1 The catalyst can be used for cyclic addition and dehydrogenation reaction. The same raw material is first subjected to hydrogenation reaction, and the hydrogenated hydrogen oil is then subjected to dehydrogenation reaction. During the addition and dehydrogenation cycle reaction, real-time sampling is performed, and the composition of the sampled liquid and the generated gas is qualitatively and quantitatively analyzed by GC-MS and gas chromatography, respectively. The results are shown in Table 1 and Table 2, respectively.

[0071] Table 1

[0072]

[0073] Table 2

[0074]

[0075] It can be seen from the results of Table 1 and Table 2 that the embodiments of the present invention have high hydrogenation and dehydrogenation activities. The catalyst prepared in this embodiment has a conversion rate of about 99.9% in hydrogenation and dehydrogenation reactions, and a selectivity of about 99.8% in dehydrogenation reactions, while the selectivity of hydrogenation and dehydrogenation in Comparative Example 1 is 99.5% and 99.6%, respectively. By adding another active metal component, the content of the active component metal is reduced, the occurrence of side reactions is reduced, the dehydrogenation selectivity of the catalyst is further improved, and the cycle life of the raw material is improved. In the comparative example, the hydrogenation conversion rates of the catalysts prepared by impregnation of homemade macroporous carriers and commercial carriers are 95% and 99.9%, respectively, and the complete hydrogenation selectivity is 95% and 99%, respectively; while the dehydrogenation conversion rates are 91% and 99.9%, respectively, and the complete dehydrogenation selectivity is 91% and 95%, respectively. Therefore, it is explained that the addition of another active metal helps to improve the dispersibility of the two-component active metal on the carrier surface and improve the dehydrogenation activity of the catalyst. The long-term stable operation duration of the catalyst in the embodiments of the present invention and the comparative examples can reach 5000 hours and more than 500 hours, respectively, indicating that the carrier modified with alkali metals, alkaline earth metals and non-metal atoms can improve the stability of the catalyst dehydrogenation reaction and further improve the service life of the catalyst.

[0076] It should be noted that the various embodiments of the present application are only for the purpose of explaining the present invention and cannot limit the present invention. It should also be known to those skilled in the art that the present embodiment only uses specific examples to elaborate on the principles and implementation methods of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the principles of the present invention should all be within the scope of protection of the present invention.

Claims

1. A dual-active metal dehydrogenation catalyst, characterized in that: The catalyst is composed of active metals A and B loaded together on a modified carrier; the active metal A is Cr, Fe, Co, Ni, Cu or Zn, accounting for 15% to 25% of the total mass of the catalyst; the active metal B is Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Y, Mo or W, accounting for 5% to 15% of the total mass of the catalyst; the modified carrier is made of silicon aluminum oxide, transition metal oxide, rare earth metal oxide, carbon material or MOFs through modification.

2. The dual-active metal dehydrogenation catalyst according to claim 1, characterized in that: The silicon aluminum oxide carrier is Al2O3, SiO2, SBA-15, KIT-6, MCM-41 or ZSM-5; the transition metal oxide carrier is ZnO2, TiO2, WO3, MoO3, Cr2O3 or Co3O4; the rare earth metal oxide carrier is La2O3 or CeO2; the carbon material carrier is activated carbon, graphite, graphene or carbon nanotubes; and the MOFs are ZIF, MIL, UIO, Nu, PCN or CPL series.

3. The dual-active metal dehydrogenation catalyst according to claim 1, characterized in that: The modified carrier has a diameter of 0.3-0.8 mm, a pore size of 15-30 nm, and a specific surface area of ​​400-1200 m 2 / g, pore volume is 0.75-2.0cm 3 / g; strength is 5-100N / grain, abrasion is 0.01%-0.05%, and bulk density is 0.3-0.7g / cm 3 .

4. A method for preparing a dual-active metal dehydrogenation catalyst according to any one of claims 1 to 3, characterized in that The following steps are involved: (1) A modifier and a surfactant are prepared into a mixed solution, carrier powder C is poured into the mixed solution, stirred and ultrasonically subjected to 0.5 to 2 h, completely dried in a drying oven, and then calcined in a muffle furnace at 350 to 550° C. for 2 to 8 h, with a heating rate of 2 to 10° C. / min. After calcination, the powder is crushed and ground into 300 to 500 mesh, a binder and a solvent are added, kneaded, extruded and spheronized, and the modified carrier is obtained after calcination; (2) preparing an aqueous solution of metal salts of metals A and B, adding the modified carrier, stirring and co-impregnating, the impregnation temperature is 30-50° C., ultrasonicating for 0.5-2 h, then taking out, aging overnight and drying; (3) The dried catalyst is placed in a muffle furnace for calcination, and then placed in a tubular furnace for reduction. After reduction, the catalyst is purged with nitrogen gas, and after cooling to room temperature, it is passivated to obtain the target catalyst.

5. The preparation method according to claim 4, characterized in that: The modifier in step (1) is a soluble salt of one or more alkali metals or alkaline earth metals selected from the group consisting of Na, K, Mg and Ca, specifically potassium carbonate, potassium nitrate, magnesium nitrate and calcium nitrate; or a soluble organic substance selected from the group consisting of one or more non-metallic substances selected from the group consisting of B, C, N, P, S and Se, specifically urea, dicyandiamide, melamine or cross-linked linear polydiaryloxyphosphazene.

6. The preparation method according to claim 4, characterized in that: The surfactant in step (1) is one or a mixture of two or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyethylene glycol, P123, and F127.

7. The preparation method according to claim 4, characterized in that: The binder in step (1) is one or a mixture of two or more of pseudo-boehmite, glass fiber, sesbania powder, microcrystalline cellulose, and polyvinyl alcohol.

8. The preparation method according to claim 4, characterized in that: The solvent in step (1) is aluminum sol or silica sol.

9. The preparation method according to claim 4, characterized in that: The reaction conditions in the step (3) are as follows: calcination temperature is 350-550°C for 2-8h, and the heating rate is 2-10°C / min; reduction temperature is 300-600°C, the time is 4-12h, the reducing gas is 5%-15% H2 / Ar mixed gas, the hydrogen flow rate is 50-250mL / min, and the heating rate is 2-10°C / min; nitrogen purge time is 0.5-2h; room temperature is 15-25°C; passivation time is 6-12h, the mixed gas is 0.5-1.5% O2 / Ar, and the flow rate is 50-250mL / min.

10. Use of the dual-active metal dehydrogenation catalyst according to any one of claims 1 to 3 in a reversible hydrogenation hydrogen storage system, characterized in that: The reversible hydrogenation hydrogen storage system includes one or a mixture of two or more π-conjugated reversible hydrogenation hydrogen storage materials; the π-conjugated reversible hydrogenation hydrogen storage material, under the conditions of 25°C and 1atm, releases 10 to 15 kcal of heat per 1 mol of H2 stored, that is, -15 kcal / mol H2≤ΔH≤-10 kcal / mol H2; and the hydrogen storage density after complete hydrogenation is greater than 4% of the mass of the hydrogen storage material; the π-conjugated reversible hydrogenation hydrogen storage material is solid or liquid, and has a melting point of less than 80°C.

Citation Information

Patent Citations

  • Catalyst for preparing H2 by direct cracking of methanol, and preparation method and application of catalyst

    CN111167462A

  • Organic hydrogen storage system capable of automatically supplying heat for dehydrogenation

    CN115304023A

  • Carbon-supported bimetallic catalyst synthesized by low-cost self-reduction method and application of carbon-supported bimetallic catalyst

    CN115318294A

  • Method and apparatus for estimating network topology and voltage states of a distribution system

    KR1020230078486A