Method for pre-activating industrial catalyst Cu-ZnO-Al2O3 by using supercritical fluid technology
By controlling the migration dynamics of ZnO and forming dual-channel reaction sites through supercritical fluid technology, the problem of low selectivity and stability of the Cu-ZnO-Al2O3 catalyst when catalyzing the hydrogenation of CO2 to methanol at high temperatures has been solved, significantly improving the performance of the catalyst. activity and stability.
Patent Information
- Application Number
- CN202411023100.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-22
AI Technical Summary
When the existing Cu-ZnO-Al2O3 catalyst catalyzes the hydrogenation of CO2 to methanol at high temperatures, there are problems such as low methanol selectivity, catalyst deactivation, and difficulty in identifying active sites. A single reaction path leads to the accumulation of intermediates and reduces conversion efficiency.
Supercritical fluid technology is used to clean the Cu-ZnO-Al2O3 catalyst with acetone and ethanol. After ultrasonic dispersion, it is treated in a supercritical CO2-ethanol system to regulate the migration dynamics of ZnO to form the ZnxAl2O4 spinel phase and CuxO surface active sites. , realizing a dual-channel reaction strategy.
The methanol generation activity and selectivity are significantly improved, the stability of the catalyst is enhanced, the dual-channel reaction of CO2 hydrogenation is realized, and the performance and sustainability of the catalyst are improved.
Smart Images

Figure CN118807757A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preactivation, and in particular to a method for preactivating industrial catalyst Cu-ZnO-Al2O3 by using supercritical fluid technology. Background Art
[0002] Catalytic CO2 hydrogenation to methanol is an effective way to convert greenhouse gases into high-value-added chemicals and alleviate the pressure of climate warming and fossil fuel depletion. The currently widely studied industrial catalysts are composed of Cu (> 50 mol%) / ZnO composites and amorphous Al2O3 (10 mol%), which have many advantages such as high activity and low cost. However, the catalytic reaction is carried out at 150-300℃ and 5-10 MPa, which is a relatively harsh condition. In addition, the main problem of this catalyst is the low methanol selectivity (< 70%) caused by the reverse water gas shift side reaction (RWGS: CO2 + H2 → CO + H2O) at high temperature, and the generated water will also accelerate the sintering of Cu active components, resulting in catalyst deactivation. More importantly, the high reactivity of the three-phase components of Cu, ZnO, and Al2O3 to high pressure and reaction atmosphere makes it difficult to distinguish the actual active sites of this multiphase catalyst. Although the Cu gradually induced by dynamic metal support interaction (SMSI) under reaction conditions is + -O v -Zn δ+ (1 < δ < 2) The interfacial active sites have been recognized by more and more scholars, but the adsorption and activation of CO2 on the active sites follow a single formate pathway. This single reaction pathway cannot effectively utilize reaction intermediates (such as CO*), which will cause them to accumulate in large quantities and occupy the active sites, reducing the conversion efficiency of methanol. In addition, although SMSI-induced ZnO coating of Cu particles can create an active interface and inhibit Cu sintering, the thickness and porosity of the coating are usually uncontrollable, which will reduce the permeability of the reaction gas and the available Cu. + Number of active sites. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preactivating an industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology to solve multiple technical problems existing in the application of the above industrial catalyst in CO2 thermal catalytic reduction.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A method for preactivating industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology comprises the following steps: The purchased Cu-ZnO-Al2O3 industrial catalyst was washed with acetone and ethanol in sequence to remove organic impurities, and then placed in a H2 / N2 atmosphere at 200-300 °C for 1-5 h for reduction, which was recorded as CZA catalyst; The CZA catalyst is ultrasonically dispersed in ethanol to form a suspension, and then the suspension is transferred to a supercritical reactor, the reactor is heated to 40-100°C, CO2 is introduced into the reactor to 8-20 MPa, and magnetic stirring is performed for 1-6 h; The mixture was naturally cooled to room temperature, and then CO2 was slowly released to relieve the pressure. The suspension after supercritical treatment was separated by centrifugation to obtain a precipitate, which was washed and dried to obtain a pre-activated Cu-ZnO-Al2O3 catalyst.
[0005] In some embodiments, the shaped industrial catalyst Cu—ZnO—Al 2 O 3 includes a copper-based methanol synthesis catalyst suitable for high pressure, medium pressure and low pressure.
[0006] In some embodiments, the volume ratio of H2 to N2 in the H2 / N2 atmosphere is 10%-60%, and the flow rate is 10-60 mLmin -1 .
[0007] In some embodiments, the reaction temperature of the supercritical CO2 is 40-100°C and the pressure is 8-20 MPa.
[0008] In some embodiments, the solid-to-liquid ratio of the CZA catalyst to the ethanol is 2.5-5 mg / mL.
[0009] In some embodiments, the washing step comprises washing with deionized water for more than 3 times, and the drying step comprises drying under vacuum at 50-80° C. for 2-8 h.
[0010] The present invention utilizes the solvent characteristics of the supercritical CO2-ethanol system to effectively increase the number of surface active sites, wherein CO2 can regulate the migration kinetics of ZnO, promote the uniform deposition of ZnO clusters on the catalyst surface, and obtain the optimized Cu + -O v -Zn δ+ At the same time, Zn will migrate to the amorphous Al2O3 support to form Zn x Al2O4 spinel phase can effectively inhibit Zn δ+ The reduction of active components can also act as Lewis acid sites to stabilize reaction intermediates. 0 Can be oxidized into amorphous Cu by supercritical CO2 x O, Cu x O surface active sites can cooperate with Cu +-O v -Zn δ+ The interfacial active sites realize a dual-channel reaction strategy for CO2 hydrogenation (RWGS-CO hydrogenation and formate pathway). As a result, the preactivated industrial catalyst exhibits significantly enhanced methanol production activity, selectivity, and stability.
[0011] Compared with the prior art, the present invention has the following advantages: At present, the catalytic active sites of industrial catalysts Cu-ZnO-Al2O3 are mainly formed by SMSI under reaction conditions, which is inseparable from harsh reaction conditions such as high temperature and high pressure. This single interfacial active site cannot effectively utilize reaction intermediates, resulting in low methanol selectivity (<70%). In addition, uncontrollable SMSI action may reduce the permeability of the reaction gas and the available Cu + Number of active sites.
[0012] This project can effectively control the migration kinetics of ZnO by simply adjusting the external thermodynamic parameters of supercritical CO2, so as to achieve the purpose of optimizing the active sites on the interface. At the same time, the rapid migration of ZnO at low temperature will lead to the x The formation of Al2O4 spinel phase also provides new insights into the stability of catalysts under actual working conditions. In addition, CO2 can also induce the creation of new Cu x O surface active sites, thereby unlocking a new strategy for synthesizing methanol via a dual-channel pathway. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The XRD patterns of the target products obtained in Examples 1 and 2 and Comparative Example 1 of the present invention are as follows; Figure 2 TEM comparison diagrams of the target products obtained in Example 1 of the present invention and Comparative Example 1: a, b) supercritical reaction 12MPa, 4 h pre-activated Cu-ZnO-Al2O3 catalyst, c, d) non-pre-activated commercial catalyst CZA; Figure 3 The comparison diagram of Cu and Zn Auger spectra of the target products obtained in Examples 1 and 2 of the present invention and Comparative Example 1 after reacting at 21 bar and 210° C. for 4 hours: a) Auger spectrum of Cu, b) Auger spectrum of Zn; Figure 4 The performance comparison chart of CO2 hydrogenation to methanol of the target catalyst obtained in Examples 1-4 of the present invention and Comparative Example 1 is as follows: a) product STY (methanol, CO) data of Examples 1, 2 and Comparative Example 1 at ambient pressure and 210°C and the corresponding methanol selectivity; b); product STY (methanol, CO) data of Examples 1-4 and Comparative Example 1 at 21 bar and 210°C and the corresponding methanol selectivity; Figure 5 The stability test data of Example 1 at 21 bar and 210°C for 30 h; Figure 6 This is the in-situ infrared spectrum of the target product CO2 hydrogenation reaction obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0014] The present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the performance of the present invention, and are not limited to the following examples.
[0015] Example 1: Supercritical reaction 12 MPa, 4 h pre-activated Cu-ZnO-Al2O3 catalyst 1 g of Cu-ZnO-Al2O3 catalyst (purchased from Sichuan Shutai Chemical Technology Co., Ltd.) was washed with acetone and ethanol to remove organic impurities, and then heated at 250 °C in H2 / N2 (10% H2, 50 mL min -1 ) atmosphere for 3 h, denoted as CZA; 100 mg of CZA powder was ultrasonically dispersed in 30 mL of ethanol, and then the suspension was transferred to a supercritical reactor. The reactor was heated to 40 °C, CO2 was introduced into the reactor to 12 MPa, and magnetic stirring was performed for 4 h. After naturally cooling to room temperature, CO2 was slowly released to relieve the pressure. The suspension after supercritical treatment was separated by centrifugation to obtain the precipitate. The product was collected by centrifugation at 8000 rpm for 10 min; it was washed with water three times and then dried under vacuum at 333 K for 6 h to obtain the target product, which was recorded as 12 MPa (4h).
[0016] Example 2: Supercritical reaction 16 MPa, 4 h pre-activated Cu-ZnO-Al2O3 catalyst 100 mg of CZA powder was ultrasonically dispersed in 20 mL of ethanol, and then the suspension was transferred to a supercritical reactor. The reactor was heated to 40 °C, CO2 was introduced into the reactor to 16 MPa, and magnetic stirring was performed for 4 h. After naturally cooling to room temperature, CO2 was slowly released to relieve the pressure. The suspension after supercritical treatment was separated by centrifugation to obtain the precipitate. The product was collected by centrifugation at 8000 rpm for 10 min; it was washed with water three times and then dried under vacuum at 333 K for 6 h to obtain the target product, which was recorded as 16 MPa (4h).
[0017] Example 3: Supercritical reaction 12 MPa, 2 h pre-activated Cu-ZnO-Al2O3 catalyst 50 mg of CZA powder was ultrasonically dispersed in 20 mL of ethanol, and then the suspension was transferred to a supercritical reactor. The reactor was heated to 40 °C, CO2 was introduced into the reactor to 12 MPa, and magnetic stirring was performed for 2 h. After naturally cooling to room temperature, CO2 was slowly released to relieve the pressure. The suspension after supercritical treatment was separated by centrifugation to obtain the precipitate. The product was collected by centrifugation at 8000 rpm for 10 min; it was washed with water three times and then dried under vacuum at 333 K for 6 h to obtain the target product, which was recorded as 12 MPa (2h).
[0018] Example 4: Supercritical reaction 12 MPa, 6 h pre-activated Cu-ZnO-Al2O3 catalyst 200 mg of CZA powder was ultrasonically dispersed in 40 mL of ethanol, and then the suspension was transferred to a supercritical reactor. The reactor was heated to 40 °C, CO2 was introduced into the reactor to 12 MPa, and magnetic stirring was performed for 6 h. After naturally cooling to room temperature, CO2 was slowly released to relieve the pressure. The suspension after supercritical treatment was separated by centrifugation to obtain the precipitate. The product was collected by centrifugation at 8000 rpm for 10 min; it was washed with water three times and then dried under vacuum at 333 K for 6 h to obtain the target product, which was recorded as 12 MPa (6h).
[0019] Comparative Example 1: Unactivated Commercial Catalyst CZA The difference from Example 1-4 is that the sample is directly used for CO2 hydrogenation catalytic reduction after reduction treatment in H2 / N2 mixed gas.
[0020] like Figure 1 As shown in the figure, the Cu-ZnO-Al2O3 activated under different supercritical CO2 pressures showed two obvious differences: (i) the Zn- x Al2O y The new diffraction peaks of the spinel phase indicate that Zn migrates to the Al2O3 support under supercritical CO2 reaction conditions. The formation of this spinel structure helps to suppress Zn under harsh reaction conditions. δ+ The reduction enhances the stability of the catalyst and acts as a Lewis acid site to stabilize formate and methoxy intermediates; (ii) the diffraction peak corresponding to the Cu (111) crystal plane at 43.58° is significantly reduced after supercritical CO2 treatment, generating Cu x O amorphous phase.
[0021] like Figure 2As shown in the figure, compared with the unactivated comparative case 1, in the 12 MPa (4 h) sample treated at supercritical pressure of 12 MPa for 4 h, ZnO is evenly dispersed on the surface of Cu particles without complete coating, which can avoid the reduction of surface active sites caused by transitional coating and optimize the interface active sites. At the same time, the increase in the surface Al content further proves that Zn x Al2O y The formation of new phases.
[0022] like Figure 3 As shown in the figure, after the pre-activated sample undergoes reduction reaction, the active site Cu + and Zn δ+ The content of is significantly higher than that of the unactivated sample, which means the high stability of the catalyst under harsh reaction conditions.
[0023] Performance test: CO2 hydrogenation to methanol performance test The performance test of CO2 hydrogenation to methanol was carried out using a stainless steel Harrick flow reactor with a 13×2 mm SiO2 window (HVC-MRA-5, USA). The reactor temperature was controlled by a thermocouple and heating system connected to the Harrick reactor. A gas chromatograph equipped with a TCD and FID detector was used to monitor the CO2 hydrogenation product online. Specifically, 20 mg of the product obtained in Examples 1-3 and Comparative Examples 1-4 was loaded into the Harrick flow reactor. Before the reaction, the mixture was heated at 10 mL min -1 20 mg of the catalyst was in situ reduced at 350 °C for 1 h under a H2 flow rate of 1.5 %. Then the H2 / CO2 mixed feed gas (20 mL min -1 ), hydrogenation performance tests were carried out at ambient pressure and 21 bar respectively. Gas samples were collected after 2 hours of reaction at each temperature stage to ensure that the reaction reached a steady state. A stainless steel gas line (120 °C) was used between the reactor and the GC system to avoid condensation of liquid products.
[0024] The experimental results are as follows Figure 4 and Figure 5 As shown in the figure, the samples pre-activated by supercritical CO2 showed significantly enhanced methanol space-time yield (STY) and selectivity at both ambient pressure and 21 bar. Specifically, when heated to 210°C, the methanol space-time yield of the 12 MPa (4h) sample at ambient pressure and 21 bar was 14.18 and 259.09 g Kg, respectively. cat -1 h -1, which is twice that of the unactivated sample. At the same time, the selectivity of methanol in the 12 MPa (4h) sample at 210℃ and 21 bar is as high as 89%. Even if the reaction temperature is reduced to 170℃, the methanol space-time yield can reach 55.96 g Kg cat -1 h -1 , and the selectivity is as high as 98%. In addition, it can be confirmed that the time of supercritical CO2 pre-activation is directly related to the activity of the product. The stability test of the 12 MPa (4h) sample under 210 and 21 bar conditions also fully demonstrated the excellence of the activated product. Within the reaction time of 30 h, the catalyst performance did not show a downward trend, while the methanol yield of the traditional commercial catalyst decreased by 7% within the reaction time of 30 h (Angew. Chem. Int. Ed. 2024, 63, e202316888).
[0025] Figure 6 This is the in-situ infrared spectrum of the target product CO2 hydrogenation reaction obtained in Example 1 of the present invention. 12 MPa (4h) In addition to the common intermediate Zn (bi-HCOO*) of the formic acid pathway on the active site of the interface, Cu (m-HOCO*) of the RWGS-CO hydrogenation pathway on the active site of the Cu surface and its further hydrogenation intermediate Cu (CH3O*) can also be observed, confirming that the supercritical activation technology can achieve a dual-channel reaction of CO2 hydrogenation.
[0026] In summary: The present invention provides a method for pre-activating an industrial catalyst Cu-ZnO-Al2O3. The solvent characteristics of the supercritical CO2-ethanol system can accelerate the migration kinetics of ZnO and promote the uniform deposition of ZnO clusters on the catalyst surface to obtain the optimal Cu δ+ -O v -Zn δ+ At the same time, Zn will migrate to the amorphous Al2O3 support to form Zn x Al2O y The spinel phase can effectively inhibit the Zn δ+ The reduction of active components can also act as Lewis acid sites to stabilize reaction intermediates. 0 Oxidation into amorphous Cu by supercritical CO2 x O, Cu x O surface active sites can cooperate with Cu δ+ -O v -Zn δ+ Interfacial active sites realize a dual-channel reaction strategy for CO2 hydrogenation.
[0027] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preactivating industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology, characterized in that: The following steps are involved: The Cu-ZnO-Al2O3 industrial catalyst was washed with acetone and ethanol in sequence to remove organic impurities, and then placed in a H2 / N2 atmosphere at 200-300 °C for reduction for 1-5 h h, which was recorded as CZA catalyst; Ultrasonic dispersion of the CZA catalyst in ethanol forms a suspension, the suspension is transferred to a supercritical reactor, the reactor is heated to 40-100° C., CO2 is introduced into the reactor to 8-20 MPa, and magnetic stirring is performed for 1-6 h; The mixture was naturally cooled to room temperature, and then CO2 was slowly released to relieve the pressure. The suspension after supercritical treatment was separated by centrifugation to obtain a precipitate, and the precipitate was washed and dried to obtain a pre-activated Cu-ZnO-Al2O3 catalyst.
2. A method for preactivating industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology according to claim 1, characterized in that: The industrial catalyst Cu-ZnO-Al2O3 includes copper-based methanol synthesis catalysts suitable for high pressure, medium pressure and low pressure.
3. The method for preactivating industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology according to claim 1, characterized in that: The volume ratio of H2 to N2 in the H2 / N2 atmosphere is 10%-60%, and the flow rate is 10-60 mL·min -1 .
4. The method for preactivating industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology according to claim 1, characterized in that: The solid-to-liquid ratio of the CZA catalyst to the ethanol is 2.5-5 mg / mL.
5. The method for preactivating industrial catalyst Cu-ZnO-Al2O3 using supercritical fluid technology according to claim 1, characterized in that: The washing step comprises washing with deionized water for more than 3 times, and the drying step comprises drying under vacuum at 50-80° C. for 2-8 h.