Preparation method of catalyst for hydrogenation reaction of methyl acrylate
By using alumina carrier and non-noble metal nickel and molybdenum catalysts, combined with equal volume impregnation method and fixed bed reaction technology, the problems of insufficient catalyst activity and difficult product separation in the hydrogenation reaction of methyl acrylate are solved, and an efficient and low-cost process is achieved. Industrial production.
Patent Information
- Application Number
- CN202410926263.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-22
AI Technical Summary
The existing technology has problems such as insufficient catalyst activity, easy polymerization, and difficulty in product separation in the hydrogenation reaction of methyl acrylate. In addition, industrial production has high costs and complex process problems.
Alumina is used as a carrier, non-noble metal nickel and molybdenum are used as active components, and boron is used as an auxiliary agent. The catalyst is prepared by an equal volume impregnation method, and hydrogen pretreatment and hydrogenation reaction under mild conditions are performed in a fixed bed reaction to solve the problem. Catalyst stability and continuity of industrial production.
It achieves a highly active and stable hydrogenation catalyst under mild conditions, reduces the cost of the catalyst, simplifies the process flow, solves the problems of easy polymerization of methyl acrylate and difficult product separation, and is suitable for industrial continuous production.
Smart Images

Figure CN118807765A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst for methyl acrylate hydrogenation reaction, in particular to a nickel-based hydrogenation catalyst used in a mild environment. The invention also relates to a method for hydrogenating methyl acrylate using the catalyst. Background Art
[0002] Methyl methacrylate (MMA) is an important organic chemical raw material and polymer monomer. It is an indispensable monomer for the production of aerospace glass, optical fiber, high-performance optical lenses, electronic information devices, robots and other major national strategic materials. At present, my country's MMA is still heavily dependent on imports and is one of the top ten products with the highest import dependence in organic fine chemicals. At the same time, with the rapid development of my country's economy, downstream markets such as special high-end coatings, precision equipment, and sound insulation panels are also developing actively, which will further stimulate the overall demand for domestic MMA.
[0003] At present, the main production methods of MMA in China are acetone cyanohydrin method (ACH), isobutylene method and ethylene method. The ACH method has a simple process and mature and reliable technology, but it uses cyanic acid as raw material, which causes great pollution to the environment. At the same time, my country has expressly prohibited the construction of traditional hydrocyanic acid process equipment since 2010. The industrial production of the emerging isobutylene method is currently mainly monopolized by foreign joint ventures. Although the domestic industrial production equipment of the isobutylene method has been newly built, the production is still unstable. The more mature process of the ethylene method is mainly mastered by companies such as BASF and Lucite. It is very difficult for my country to achieve full localization of industrial production of MMA by the ethylene method in the short term; the catalyst of the isobutylene method is expensive, the investment in equipment construction is large, and the catalyst is easy to deactivate. Based on the characteristics of my country's rich coal, poor oil and little gas, the process of synthesizing MMA by methyl acetate method is of great significance. The methyl acetate method obtains MMA products by three steps of aldol condensation, hydrogenation and aldol condensation of methyl acetate and formaldehyde. Among them, the second step of methyl acrylate hydrogenation reaction has problems such as methyl acrylate is easy to polymerize and difficult to separate from the product methyl propionate. Therefore, the methyl acrylate hydrogenation reaction requires high catalyst hydrogenation activity under mild conditions.
[0004] Patent CN107626344A discloses a catalyst for industrial naphthalene hydrogenation, wherein the active components are Ni, Mo, and W, the organic additive is citric acid or urea, and the inorganic additive is one or more of P, B, and F. The metal composite oxide is obtained by hydrothermal reaction, and then the hydrogenation catalyst is obtained by extrusion. The active component content of the catalyst is high, accounting for 35%-90% of the total mass of the catalyst, and the preparation process is complicated, which is not suitable for industrial production.
[0005] Patent CN1579624A discloses a Ni-MB catalyst for benzene hydrogenation, wherein the active components are Ni, B, M (Fe, Mo, La, Cr), and the Ni-M / N (carrier) catalyst is prepared by an impregnation method. + The aqueous solution of ions reduces Ni and M on the carrier, introducing B into the Ni-M / N (carrier) catalyst, which has good catalytic activity and strong sulfur resistance. However, this preparation method has a large limitation on the loading amount of B, containing BH4 + The reducing agent is not easy to store, and a large amount of wastewater is produced during the reduction, and the preparation process is relatively complicated.
[0006] Reaction patent CN109232247A discloses a method of hydrogenating methyl acrylate in an intermittent reactor using a palladium catalyst, wherein the hydrogenation conversion rate of methyl acrylate is greater than 95% and the selectivity is greater than 95%. The intermittent reactor is not conducive to the continuous operation of industrialization, and the active component of the catalyst is a precious metal, so the catalyst cost is relatively high. Summary of the invention
[0007] The object of the present invention is to provide a hydrogenation catalyst with high activity and stability under mild reaction conditions. At the same time, the present invention also provides a method for producing methyl propionate which can continuously, stably and effectively solve the problems of temperature rise.
[0008] The object of the present invention is achieved through the following technical solutions:
[0009] The catalyst consists of a carrier, an active component group and an auxiliary agent. The carrier is alumina, the active components are non-noble metals Ni and Mo, and the auxiliary agent is non-metallic B.
[0010] The loading amount of the active components is 20-25wt% of the total mass of the catalyst, wherein the nickel oxide content is 10wt%, the second component molybdenum oxide content is 10wt%, and the third component boron oxide content is 0-5wt%, excluding zero point.
[0011] As a limitation of the above method, the catalyst is prepared by an equal volume impregnation method.
[0012] The present invention discloses a catalyst for methyl acrylate hydrogenation reaction and a method thereof. The preparation method of the catalyst comprises the following steps:
[0013] (1) The carrier used needs to be calcined at 500-700℃ for 3-6h before use.
[0014] (2) impregnating the alumina support obtained in (1) into an impregnation solution containing an active component by an equal volume impregnation method, leaving the solution at room temperature for 8-12 hours, and drying the solution at 100-120° C. for 8-12 hours to obtain a catalyst precursor.
[0015] (3) The catalyst precursor obtained in (2) is calcined at 400-600° C. for 3-6 hours to obtain a catalyst.
[0016] At the same time, the present invention discloses a catalyst for methyl acrylate hydrogenation reaction and a method thereof, wherein the use method comprises the following steps:
[0017] (1) The hydrogenation catalyst needs to be pre-treated with hydrogen at a temperature of 400-600°C before use.
[0018] (2) At the reaction temperature and pressure, a certain proportion of hydrogen and liquid raw materials are introduced into a fixed bed, wherein the liquid is a mixture of methyl acrylate, methyl propionate and a polymerization inhibitor.
[0019] (3) After the reaction is completed, the reaction temperature is lowered to room temperature to release the unreacted hydrogen. After nitrogen purging, the catalyst is unloaded.
[0020] The catalyst and method for hydrogenation reaction of methyl acrylate of the present invention have the following characteristics: reaction temperature is 80-120°C, reaction pressure is 0.6-1.2MPa, molar ratio of methyl acrylate to hydrogen is 3-10, mass space velocity is 0.5-2h -1 .
[0021] The invention discloses a catalyst for hydrogenation reaction of methyl acrylate and a method thereof. The molar ratio of methyl acrylate to methyl propionate in the feed liquid is 0.5-2.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The catalyst of the present invention has high activity under mild conditions, good stability, and low hydrogen consumption. At the same time, it uses non-precious metals as active components, has low catalyst cost, and a simple preparation method, which is conducive to industrial production.
[0024] 2. The present invention solves the problems of easy polymerization of methyl acrylate, difficulty in separation of product methyl propionate and heat release during hydrogenation. The process is simple and the operating cost is low. At the same time, the fixed bed is used for reaction, which is conducive to industrial continuous production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram of the element content of a catalyst used in the hydrogenation reaction of methyl acrylate, in which the number in front of the element represents the mass fraction of the element.
[0026] Figure 2 These are the experimental conditions and results of the fixed bed methyl acrylate hydrogenation method.
[0027] Figure 3These are the experimental conditions and results of the life experiment of the fixed bed methyl acrylate hydrogenation method. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with specific examples, but it should not be understood that the subject scope of the present invention is limited to the following examples. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to common technical knowledge and customary means in the art, which should all be included in the scope of the present invention. The following γ-Al2O3 carrier is provided by Liaoning Haitai Technology Development Co., Ltd.
[0029] Embodiment 1
[0030] This example relates to a group of catalyst preparations for the hydrogenation reaction of methyl acrylate, as shown in the following table:
[0031] Active ingredient 1 Active ingredient 2 Active ingredient 3 Example 1.1 10Ni 10Mo 0B Example 1.2 10Ni 10Mo 1B Example 1.3 10Ni 10Mo 2B Example 1.4 10Ni 10Mo 4B Example 1.5 10Ni 10Mo 5B
[0032] Table 1 Schematic table of element contents in the catalyst preparation for methyl acrylate hydrogenation reaction
[0033] Example 1.1:
[0034] The carrier was pretreated, the γ-Al2O3 balls were crushed into 20-40 mesh particles, and calcined at 600°C for 4 hours. The impregnation solution was prepared by dissolving 4.87g nickel nitrate hexahydrate and 1.53g ammonium molybdate tetrahydrate in 10.66g distilled water. 10g of the calcined alumina carrier was weighed and impregnated in the impregnation solution containing the active component, left to stand at room temperature for 4 hours, dried at 120°C for 12 hours, and calcined at 450°C in an air atmosphere for 4 hours. A 10wt% Ni-10wt% Mo-0wt% B / γ-Al2O3 catalyst was obtained.
[0035] Catalyst performance test: The test was carried out using the conditions in Example 2.1.
[0036] Example 1.2:
[0037] The carrier was pretreated, the γ-Al2O3 balls were crushed into 20-40 mesh particles, and calcined at 600°C for 4 hours. The impregnation solution was prepared by dissolving 4.93g nickel nitrate hexahydrate, 1.55g ammonium molybdate tetrahydrate, and 0.22g boric acid in 10.66g distilled water. 10g of the calcined alumina carrier was weighed and impregnated in the impregnation solution containing the active component, left to stand at room temperature for 4 hours, dried at 120°C for 12 hours, and calcined at 450°C in an air atmosphere for 4 hours. A 10wt% Ni-10wt% Mo-1wt% B / γ-Al2O3 catalyst was obtained.
[0038] Catalyst performance test: The test was carried out using the conditions in Example 2.2.
[0039] Example 1.3:
[0040] The carrier was pretreated, the γ-Al2O3 balls were crushed into 20-40 mesh particles, and calcined at 600°C for 4 hours. The impregnation solution was prepared by dissolving 4.99g nickel nitrate hexahydrate, 1.57g ammonium molybdate tetrahydrate, and 0.46g boric acid in 10.66g distilled water. 10g of the calcined alumina carrier was weighed and impregnated in the impregnation solution containing the active component, left to stand at room temperature for 4 hours, dried at 120°C for 12 hours, and calcined at 450°C in an air atmosphere for 4 hours. A 10wt% Ni-10wt% Mo-2wt% B / γ-Al2O3 catalyst was obtained.
[0041] Catalyst performance test: The test was carried out using the conditions in Example 2.3.
[0042] Example 1.4:
[0043] The carrier was pretreated, the γ-Al2O3 balls were crushed into 20-40 mesh particles, and calcined at 600°C for 4 hours. The impregnation solution was prepared by dissolving 5.12g nickel nitrate hexahydrate, 1.61g ammonium molybdate tetrahydrate, and 0.93g boric acid in 10.66g distilled water. 10g of the calcined alumina carrier was weighed and impregnated in the impregnation solution containing the active component, left to stand at room temperature for 4 hours, dried at 120°C for 12 hours, and calcined at 450°C in an air atmosphere for 4 hours. A 10wt% Ni-10wt% Mo-4wt% B / γ-Al2O3 catalyst was obtained.
[0044] Catalyst performance test: The test was carried out using the conditions in Example 2.4.
[0045] Example 1.5:
[0046] The carrier was pretreated, the γ-Al2O3 balls were crushed into 20-40 mesh particles, and calcined at 600°C for 4 hours. The impregnation solution was prepared by dissolving 5.19g nickel nitrate hexahydrate, 1.63g ammonium molybdate tetrahydrate, and 1.18g boric acid in 10.66g distilled water. 10g of the calcined alumina carrier was weighed and impregnated in the impregnation solution containing the active component, left to stand at room temperature for 4 hours, dried at 120°C for 12 hours, and calcined at 450°C in an air atmosphere for 4 hours. A 10wt% Ni-10wt% Mo-5wt% B / γ-Al2O3 catalyst was obtained.
[0047] Embodiment 2
[0048] This embodiment relates to a fixed bed methyl acrylate hydrogenation method:
[0049] Example 2.1
[0050] 5 g of the hydrogenation catalyst prepared in Example 1.1 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction, the temperature was lowered to 80°C and the pressure was 1 MPa. The molar ratio of methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 6, and the mass space velocity was 1 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0051] Example 2.2
[0052] 5 g of the hydrogenation catalyst prepared in Example 1.2 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction was completed, the temperature was lowered to 80°C and the pressure was 1 MPa. The molar ratio of methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 5, and the mass space velocity was 1 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0053] Example 2.3
[0054] 5 g of the hydrogenation catalyst prepared in Example 1.3 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction, the temperature was lowered to 80°C and the pressure was 1 MPa. The molar ratio of methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 5, and the mass space velocity was 1 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0055] Example 2.4
[0056] 5 g of the hydrogenation catalyst prepared in Example 1.4 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction, the temperature was lowered to 80°C and the pressure was 1 MPa. The molar ratio of methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 5, and the mass space velocity was 1 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0057] Example 2.5
[0058] 5 g of the hydrogenation catalyst prepared in Example 1.5 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction, the temperature was lowered to 80°C and the pressure was 1 MPa. The molar ratio of methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 5, and the mass space velocity was 1 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0059] Example 2.6
[0060] 5 g of the hydrogenation catalyst prepared in Example 1.1 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction was completed, the temperature was lowered to 50°C and the pressure was 0.5 MPa. The molar ratio of methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 5, and the mass space velocity was 1 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0061] Example 2.7
[0062] 5 g of the hydrogenation catalyst prepared in Example 1.1 was loaded into a reaction tube with an inner diameter of 7 mm. The catalyst was reduced with 10% H2 at 450°C for 4 h. After the reduction, the temperature was lowered to 80°C and the pressure was 1 MPa. The molar ratio of the methyl acrylate to methyl propionate was 1, the molar ratio of hydrogen to methyl acrylate was 5, and the mass space velocity was 2 h -1 , n-hexane was used as the internal standard, and the addition amount was 10%; hydroquinone was used as the inhibitor, and the addition amount was 100ppm. After the reaction, the reaction product was checked by chromatography. After the reaction was completed, the fixed bed temperature was lowered to room temperature, the unreacted hydrogen was released, and the catalyst was unloaded. The results are shown in the figure.
[0063] A fixed bed methyl acrylate hydrogenation method of this embodiment is verified by the following experiment to verify the effect of methyl acrylate hydrogenation. The limitation of reaction conditions and experimental results are shown in the following table:
[0064]
[0065]
[0066] Table 2 Experimental conditions and experimental results of fixed bed methyl acrylate hydrogenation method
[0067] Embodiment 3
[0068]
[0069] Table 3 Experimental conditions and results of fixed bed methyl acrylate hydrogenation process life test
[0070] The present invention relates to a nickel-based catalyst for a fixed-bed methyl acrylate hydrogenation reaction and a method thereof, which has a high yield for methyl propionate, solves the problem of difficult separation of methyl acrylate and methyl propionate, and effectively avoids the problem of easy polymerization of methyl acrylate. The invention is a hydrogenation method with simple process flow, low energy consumption and low operating cost, and has good industrial application prospects.
Claims
1. A catalyst for the hydrogenation reaction of methyl acrylate, characterized in that: The catalyst is composed of a carrier, an active component and an auxiliary agent, wherein the carrier is alumina, the active component is non-precious metals Ni and Mo, the auxiliary agent is non-metal B, the loading amount of the active component accounts for 20-25wt% of the total mass of the catalyst, wherein the content of nickel oxide is 10wt%, the content of molybdenum oxide of the second component is 10wt%, and the content of boron oxide of the third component is 0-5wt%, excluding zero point, and the use method comprises the following steps: (1) The hydrogenation catalyst needs to be pretreated with hydrogen at a temperature of 400-600°C before use; (2) At the reaction temperature and pressure, a certain ratio of hydrogen and liquid raw materials are introduced into a fixed bed, wherein the liquid is a mixture of methyl acrylate, methyl propionate and a polymerization inhibitor; (3) After the reaction is completed, the reaction temperature is lowered to room temperature to release the unreacted hydrogen. After nitrogen purging, the catalyst is unloaded.
2. A catalyst for hydrogenation of methyl acrylate according to claim 1, characterized in that: The content of nickel oxide is 10wt%, the content of molybdenum oxide, the second component, is 10wt%, and the content of boron oxide, the third component, is 0-5wt%, excluding zero point.
3. A catalyst and application for hydrogenation of methyl acrylate according to any one of claims 1 to 2, characterized in that: The catalyst was prepared by an isovolumetric impregnation method.
4. A catalyst and application for hydrogenation of methyl acrylate according to any one of claims 1 to 2, characterized in that: The preparation method of the catalyst comprises the following steps: (1) The carrier used needs to be calcined at 500-700℃ for 3-6h before use; (2) impregnating the alumina support obtained in (1) into an impregnation solution containing an active component by an equal volume impregnation method, leaving the solution at room temperature for 8-12 hours, and drying the solution at 100-120° C. for 8-12 hours to obtain a catalyst precursor; (3) The catalyst precursor obtained in (2) is calcined at 400-600°C for 3-6h to obtain a catalyst.
5. The catalyst and application for hydrogenation of methyl acrylate according to claim 1, characterized in that: The reaction temperature is 80-120°C, the reaction pressure is 0.6-1.2MPa, the molar ratio of methyl acrylate to hydrogen is 3-10, and the mass space velocity is 0.5-2 h -1 .
6. The catalyst for hydrogenation of methyl acrylate according to claim 1, characterized in that: The molar ratio of the methyl acrylate to the methyl propionate in the feed is 0.5-2.
Citation Information
Patent Citations
Catalyst for preparing tetrahydronaphthalene and decahydronaphthalene from technical naphthalene through hydrogenation, preparation and application
CN107626344A
Method for preparing methyl methacrylate by aldol condensation of methyl acetate and formaldehyde
CN109232247A
Benzene hydrogenation non-crystalline state nickel-base catalyst with high sulfidation resistance and its preparing method
CN1579624A