Utilization method of waste hydrogenation bulk phase catalyst
Through the extraction, oil removal, sulfur removal, carbon removal of the waste phase hydrogenation catalyst and the treatment of the ternary alkali solution and organic additives, combined with the co-flow gelation reaction and pH value decreasing aging, the problems in the existing technology have been solved. The problem of low recovery rate of active metals and high impurities in the finished catalyst is used to prepare a catalyst with excellent performance and stability.
Patent Information
- Application Number
- CN202310434210.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-21
AI Technical Summary
The existing technology has a low recovery rate of active metals when recovering bulk phase hydrogenation catalysts. The finished catalyst has many impurities and poor adhesion, which affects the molding effect and activity stability of the catalyst.
Through extraction, oil removal, sulfur removal, carbon removal, and pulverization, the catalyst powder is mixed and dissolved with a ternary alkali solution and an organic additive to obtain a solution containing tungsten, molybdenum, and nickel and aluminum, which is then co-flowed into a gel, and The catalyst is prepared through multiple pH decline aging, and finally drying and roasting.
It achieves efficient recovery of active metals in waste phase hydrogenation catalysts, reduces metal impurities, improves the crushing strength and pore volume of the catalyst, enhances activity stability, and reduces production costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste recycling and utilization, and specifically relates to a method for utilizing a waste hydrogenation bulk catalyst. Background Art
[0002] With the development of the chemical industry, especially the development of chemical industries such as oil refining and chemical industry that use a large amount of catalysts, a large amount of waste catalysts will be generated. At the same time, with the increasingly stringent environmental regulations, the treatment of these waste catalysts has become an important issue. In particular, bulk catalysts have a high content of active metals. If they are directly discarded, it will bring great losses both in terms of economy and environment. Bulk catalysts are often used in the processing of heavy oil due to their high activity. The high impurity content in the waste catalysts further increases the difficulty of reusing bulk catalysts. An environmentally friendly method for reusing waste catalysts is needed.
[0003] CN108067245A discloses a method for recycling a hydroprocessing catalyst. The method comprises extracting, roasting and crushing molybdenum-nickel waste catalyst, mixing the catalyst powder with alkali to obtain an aluminate solution and nickel oxide solid, preparing pseudo-boehmite from the aluminate solution by carbonization to prepare a carrier, preparing basic nickel carbonate from the nickel oxide, preparing molybdenum-nickel-phosphorus solution from the obtained basic nickel carbonate, and then impregnating the carrier. The method is particularly suitable for recycling molybdenum and nickel waste catalysts to prepare new catalysts, and has the characteristics of simple process and low processing cost.
[0004] CN112619658A discloses a method for recycling a waste hydrogenation catalyst, which comprises extracting and removing oil from the waste hydrogenation catalyst, roasting, crushing, mixing with alkali, roasting, soaking with hot water, filtering, obtaining a filtrate and a residue, then adding a polymer monomer to the filtrate to obtain a solution I and a solution II for a parallel gelation reaction, aging, solid-liquid separation of the aged material, extrusion molding, and then drying and roasting to obtain a hydrogenation catalyst.
[0005] CN108620083A discloses a method for recycling and reusing waste hydrogenation catalyst materials, comprising: crushing the waste catalyst materials, sieving and beating to obtain a slurry with a solid content of 15wt% to 55wt%, adding nitric acid, phosphoric acid and an organic acid solution under stirring conditions, heating to 65 to 100°C, cooling to room temperature, adding an organic amine and mixing evenly to obtain a sol slurry of the waste materials, mixing the waste sol slurry, a modified macroporous alumina powder, a small-pore alumina powder mixture and an extrusion aid evenly, kneading, forming, drying and calcining to obtain an alumina carrier, and loading active components to obtain a hydrogenation catalyst.
[0006] The metal content of the catalyst involved in the above method is relatively small. When the bulk hydrogenation catalyst with an active metal content of more than 60m% is treated, the active metal recovery rate is poor. At the same time, the recovered active metal solution contains more impurities. When the active metal is used again, the adhesion of the gelled material is poor, which affects the molding effect of the recovered catalyst. The crushing strength of the finished catalyst is poor, and the catalyst contains more impurities, which reduces the activity of the catalyst and its activity stability (lifespan). Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a method for utilizing waste bulk hydrogenation catalysts. The method can efficiently recover active metals in waste bulk hydrogenation catalysts, and the re-prepared catalysts have fewer metal impurities, good active metal utilization rate and crushing strength. At the same time, the catalyst has large pore volume and specific surface area, excellent hydrogenation performance and activity stability, thus realizing the transformation of waste into treasure and greatly reducing the production cost of the catalyst.
[0008] The method for utilizing the waste bulk hydrogenation catalyst of the present invention comprises the following contents: (1) The waste tungsten-molybdenum-nickel bulk hydrogenation catalyst is extracted, deoiled, desulfurized, decarbonized and crushed to obtain catalyst powder; (2) mixing and dissolving the catalyst powder, the ternary mixed alkali solution and the first organic auxiliary agent, and after the reaction is completed, obtaining a solution containing tungsten and molybdenum and a solid phase containing nickel and aluminum through solid-liquid separation; (3) mixing and dissolving the nickel-aluminum-containing solid phase, the inorganic acid, and the second organic auxiliary agent to obtain a nickel-aluminum-containing solution after the reaction is completed; (4) The tungsten- and molybdenum-containing solution and the nickel- and aluminum-containing solution are subjected to a parallel gelation reaction, and the obtained gelation product is subjected to multiple pH value decreasing aging processes in succession. The aged product is dried, formed, washed, and then dried and calcined to obtain a catalyst product.
[0009] In the method of the present invention, the waste tungsten-molybdenum-nickel bulk hydrogenation catalyst described in step (1) comprises, by weight, 70% to 90% of catalyst solids and 10% to 30% of petroleum fractions. Based on the weight of the extracted catalyst, tungsten oxide is 20% to 50%, nickel oxide is 10% to 35%, molybdenum oxide is 10% to 50% of aluminum oxide, iron oxide is 0.7% to 1.8%, vanadium oxide is 0.6% to 1.3%, arsenic oxide is 0.6% to 1.5%, and sodium oxide is 0.6% to 1.1%.
[0010] The organic solvent used for the extraction is toluene, petroleum ether, ethanol, etc., and the extraction temperature is 80-110°C. The desulfurization and decarbonization process is: desulfurization at a constant temperature of 300-350°C for 2-7 hours, and then decarbonization at a constant temperature of 500-600°C for 2-6 hours; the particle size of the catalyst powder after crushing is 200-400 mesh, preferably 250-390 mesh.
[0011] In the method of the present invention, the ternary mixed alkaline solution in step (2) is a mixed alkaline solution containing sodium carbonate, sodium phosphate and ammonia water, wherein the molar ratio of the total molar number of sodium carbonate, sodium phosphate and ammonia to the catalyst powder calculated as oxide is 2.0:1 to 6.0:1, preferably 2.2:1 to 5.5:1; the molar ratio of the sum of the molar numbers of sodium carbonate and sodium phosphate to ammonia is 0.8:1 to 8:3, and the molar ratio of sodium carbonate to sodium phosphate is 4:6 to 3:1.
[0012] In the method of the present invention, the first organic auxiliary agent in step (2) is one or more of sodium polyaspartate, sodium polyepoxysuccinate, acrylic acid-hydroxypropyl acrylate copolymer, pentasodium aminotrimethylenephosphonic acid, sodium polypropionate, pentasodium ethylenediaminetetramethylenephosphonic acid, tetrasodium hydroxyethylidene diphosphonic acid, sodium diethylenetriamine penta(methylenephosphonic acid), and 2-hydroxyphosphonic acid acylacetic acid, preferably one or more of sodium polyaspartate, sodium polyepoxysuccinate, pentasodium aminotrimethylenephosphonic acid, sodium polypropionate, pentasodium ethylenediaminetetramethylenephosphonic acid, tetrasodium hydroxyethylidene diphosphonic acid, and sodium diethylenetriamine penta(methylenephosphonic acid).
[0013] In the method of the present invention, in step (2), the molar ratio of the first organic auxiliary agent to Mo in the catalyst powder is 0.8:1 to 3.8:1, preferably 1:1 to 3.5:1.
[0014] In the method of the present invention, the mixing and dissolving time in step (2) is 2 to 10 hours, generally carried out under stirring conditions. The solid-liquid separation can be carried out by centrifugation, filtration, etc.
[0015] In the method of the present invention, the inorganic acid in step (3) is nitric acid, sulfuric acid or hydrochloric acid, preferably sulfuric acid or nitric acid, and the molar ratio of the inorganic acid to the nickel in the catalyst after extraction is 0.8:1 to 2.9:1, preferably 0.9:1 to 2.7:1.
[0016] In the method of the present invention, the second organic auxiliary agent in step (3) is one or more of octadecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride and dodecyltrimethylammonium chloride.
[0017] In the method of the present invention, the molar ratio of the amount of the second organic auxiliary agent added in step (3) to the Ni in the catalyst powder is 0.6:1 to 2.5:1, preferably 0.8:1 to 2.2:1.
[0018] In the method of the present invention, the mixing and dissolving time in step (3) is 1 to 8 hours, generally carried out at room temperature.
[0019] In the method of the present invention, the conditions of the gelling reaction in step (4) are as follows: the reaction temperature is 30 to 95°C, preferably 40 to 95°C, the pH value is controlled at 6.5 to 9.5 at the end, and the reaction time is 0.5 to 3.5 hours.
[0020] In the method of the present invention, the aging temperature in step (4) is 60 to 98°C, preferably 65 to 92°C.
[0021] In the method of the present invention, the pH value in step (4) is gradually reduced and the number of aging times is 2 to 8 times.
[0022] In the method of the present invention, the pH value of step (4) is gradually decreased during the aging process: a portion of sodium aluminate solution is added dropwise to the reaction slurry to control the pH value at 11.5-13.5, and the aging is performed for 0.05-0.5 hours; then the pH value is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; finally, the pH value is adjusted to 4.0-6.5, and the aging time is 0.05-0.5 hours.
[0023] In the method of the present invention, the sodium aluminate solution in step (4) is divided into 2 to 8 parts by volume according to the number of aging times, preferably divided equally by volume. The Al added through the sodium aluminate solution accounts for 5% to 48% of the total Al of the obtained catalyst in terms of Al2O3, preferably 6% to 45%.
[0024] Among them, except for the use of sodium aluminate solution in the first stage pH value adjustment during the aging process, the acids and alkalis used for adjusting the pH value can be inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements. The inorganic acid can be hydrochloric acid and acetic acid, and the inorganic alkali can be one or more of sodium carbonate, sodium bicarbonate, ammonia water, and sodium hydroxide. The concentration and dosage of the acid and alkali solutions can be adjusted according to the actual preparation needs.
[0025] In the method of the present invention, the drying, molding and washing described in step (4) can be carried out by conventional methods in the art. The drying conditions are as follows: drying at 40-150°C for 1-48 hours, preferably drying at 50-120°C for 4-36 hours. During the molding process, conventional molding aids, such as one or more of peptizers, extrusion aids, etc., can be added as needed. The peptizer is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the extrusion aid refers to a substance that is conducive to extrusion molding, such as one or more of sesbania powder, carbon black, graphite powder, citric acid, etc., and the amount of the extrusion aid accounts for 1wt% to 10wt% of the total material dry basis. It can be prepared into flakes, spheres, cylindrical strips and special-shaped strips (three-leaf clover, four-leaf clover) and the like as needed. Washing is generally done with deionized water or a solution containing decomposable salts (such as ammonium acetate, ammonium chloride, ammonium nitrate, etc.) until neutral.
[0026] In the method of the present invention, the calcination conditions in step (4) are as follows: calcination at 350-650° C. for 1-24 hours, preferably calcination at 400-600° C. for 2-12 hours.
[0027] The catalyst obtained by the method of the present invention can be applied to ultra-deep hydrodesulfurization, denitrogenation reaction and hydrodearomatization reaction of heavy diesel fraction.
[0028] Compared with the prior art, the present invention has the following advantages: 1. The method of the present invention can maximize the recovery and utilization of active metals and alumina of waste bulk catalysts by combining a ternary alkaline solution and an organic auxiliary agent, while removing metallic impurity ions dissolved in the active metal solution.
[0029] The present invention adds Al-containing solution in batches during aging, dissolves amorphous oxides in oxide particles by swinging the pH value, and re-modifies the size of oxide particles by adding Al-containing solution. After the pH value swings n times, the growth of oxide particles is controlled, making the oxide particles more uniform, exposing more active metals to the surface phase and dispersing them uniformly. At the same time, the aluminum introduced by the Al-containing solution increases the surface hydroxyl groups, further enhancing the adhesion of the oxide, which is beneficial to the formation of the bulk catalyst.
[0030] 3. The catalyst obtained by the method of the present invention has less metal impurities and good crushing strength, which realizes the circular economic utilization of the catalyst, greatly reduces the production cost of the catalyst, and improves the recovery efficiency of the bulk phase waste catalyst. DETAILED DESCRIPTION
[0031] The technical scheme and technical effects of the present invention are further illustrated below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, the specific surface area and pore volume are determined by low-temperature liquid nitrogen adsorption method, and the mechanical strength is determined by lateral pressure method. The active metal content of the catalyst surface phase is determined by X-ray photoelectron spectroscopy (XPS), and the active metal content of the catalyst bulk phase is determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES). The impurity content of the waste catalyst is determined by X-ray fluorescence spectrometer. In the present invention, wt% is the mass fraction and v% is the volume fraction.
[0032] The waste bulk catalyst used in the present invention is discarded after the operation of a hydrocracking unit of a refinery of Sinopec. The bulk catalyst after industrial operation is extracted and deoiled at 90°C, dried at 120°C for 3 hours, calcined at 500°C for 2 hours, and sieved and crushed to 300 meshes. The mass content of active metals and impurities after desulfurization and decarbonization of the waste bulk catalyst used in the present invention is: MoO3 is 18.4%, NiO is 20.5%, WO3 is 34.6%, Al2O3 is 23.6, Fe2O3 is 0.987%, V2O5 is 0.746%, As2O3 is 0.487%, and Na2O is 0.680%. Example 1
[0033] The crushed catalyst powder is mixed with a mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water, wherein the molar ratio of sodium carbonate, sodium phosphate and ammonia to the active metal (in terms of oxide) in the mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water is 3.5, the molar ratio of the sum of the moles of sodium carbonate and sodium phosphate to ammonia is 1.2, and the molar ratio of sodium carbonate to sodium phosphate is 1.5. Sodium polyaspartate is added, wherein the molar ratio of sodium polyaspartate to Mo in the catalyst powder is 2.5, and the mixture is reacted and dissolved under stirring for 6 hours, and then filtered to obtain a tungsten-molybdenum solution and a filter residue containing nickel and aluminum; the obtained residue is mixed with nitric acid, and the molar ratio of nitric acid to nickel in the catalyst powder is 2.0:1. Octadecyl trimethyl ammonium bromide is added, wherein the molar ratio of octadecyl trimethyl ammonium bromide to Ni in the catalyst powder is 1.3, and the mixture is reacted and dissolved under stirring for 5 hours, and filtered to obtain a solution containing nickel and aluminum. The Al in the sodium aluminate solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrogenation catalyst, and it is divided into 5 equal parts by volume. Deionized water is added to the reaction tank, and the W, Mo solution and the Ni, Al solution are added to the reaction tank in parallel to perform a gelling reaction. The reaction pH is controlled at 8.3, and the reaction temperature is 60°C. After 1.0 hour of reaction, a precipitate slurry containing nickel, molybdenum, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 76°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 13.1. After aging for 0.2 hours, the aging pH value is controlled to 9.5. After aging for 0.15 hours, the pH value is then controlled to 5.2, and the aging time is 0.2 hours. The above operation process is repeated 5 times to end aging. The aged slurry is filtered, and the filter cake is dried at 100°C for 8 hours, rolled, and extruded. Wash with deionized water at room temperature until neutral. The dried material was dried at 100°C for 8 hours, and the dried material was calcined at 530°C for 5 hours to obtain Catalyst A. The composition and main properties of the catalyst are shown in Table 1. Example 2
[0034] The crushed catalyst powder is mixed with a mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water, wherein the molar ratio of sodium carbonate, sodium phosphate and ammonia to the active metal (in terms of oxide) in the mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water is 4.0, the molar ratio of the sum of the moles of sodium carbonate and sodium phosphate to ammonia is 1.6, and the molar ratio of sodium carbonate to sodium phosphate is 1.6. Sodium polyepoxysuccinate is added, wherein the molar ratio of sodium polyepoxysuccinate to Mo in the catalyst powder is 1.8, and the mixture is reacted and dissolved under stirring for 6 hours, and then filtered to obtain a tungsten-molybdenum solution and a filter residue containing nickel and aluminum; the obtained residue is mixed with nitric acid, and the molar ratio of nitric acid to nickel in the catalyst powder is 1.8:1. Octadecyl trimethyl ammonium bromide is added, wherein the molar ratio of octadecyl trimethyl ammonium bromide to Ni in the catalyst powder is 1.7, and the mixture is reacted and dissolved under stirring for 4 hours, and filtered to obtain a solution containing nickel and aluminum. The Al in the sodium aluminate solution accounts for 35% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 6 equal parts by volume. Deionized water is added to the reaction tank, and the W, Mo solution and the Ni, Al solution are added to the reaction tank in parallel to perform a gelling reaction. The reaction pH is controlled at 8.0 and the reaction temperature is 65°C. After 1.2 hours of reaction, a precipitate slurry containing nickel, molybdenum, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 82°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 12.7. After aging for 0.15 hours, the aging pH value is controlled to 9.2. After aging for 0.15 hours, the pH value is then controlled to 4.9, and the aging time is 0.15 hours. The above operation process is repeated 6 times to end aging. The aged slurry is filtered, and the filter cake is dried at 110°C for 7 hours, rolled, and extruded. Wash with deionized water at room temperature until neutral. The dried material was dried at 100°C for 7 hours, and the dried material was calcined at 520°C for 5 hours to obtain Catalyst B. The composition and main properties of the catalyst are shown in Table 1. Example 3
[0035] The crushed catalyst powder is mixed with a mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water. The molar ratio of sodium carbonate, sodium phosphate and ammonia in the mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia to the active metal (in terms of oxide) in the crushed catalyst is 3.8, the molar ratio of the sum of the moles of sodium carbonate and sodium phosphate to ammonia is 1.8, and the molar ratio of sodium carbonate to sodium phosphate is 1.9. Sodium polypropionate is added, and the molar ratio of sodium polypropionate to Mo in the catalyst powder is 2.0. The mixture is reacted and dissolved under stirring for 5.5 hours, and then filtered to obtain a tungsten-molybdenum solution and a filter residue containing nickel and aluminum; the obtained residue is mixed with nitric acid, and the molar ratio of nitric acid to nickel in the catalyst powder is 1.6:1. Octadecyl trimethyl ammonium chloride is added, and the molar ratio of octadecyl trimethyl ammonium chloride to Ni in the catalyst powder is 1.4. The mixture is reacted and dissolved under stirring for 4.5 hours, and filtered to obtain a solution containing nickel and aluminum. The Al in the sodium aluminate solution accounts for 25% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 7 equal parts by volume. Deionized water is added to the reaction tank, and the W, Mo solution and the Ni, Al solution are added to the reaction tank in parallel to perform a gelling reaction. The reaction pH is controlled at 7.8 and the reaction temperature is 55°C. After 1.3 hours of reaction, a precipitate slurry containing nickel, molybdenum, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 81°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 12.5. After aging for 0.15 hours, the aging pH value is controlled to 9.8. After aging for 0.2 hours, the pH value is then controlled to 5.5, and the aging time is 0.2 hours. The above operation process is repeated 7 times to end aging. The aged slurry is filtered, and the filter cake is dried at 120°C for 8 hours, rolled, and extruded. Wash with deionized water at room temperature until neutral. The dried material was dried at 90°C for 8 hours, and the dried material was calcined at 500°C for 5 hours to obtain Catalyst C. The composition and main properties of the catalyst are shown in Table 1. Example 4
[0036] The crushed catalyst powder is mixed with a mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water. The molar ratio of sodium carbonate, sodium phosphate and ammonia in the mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia to the active metal (in terms of oxide) in the crushed catalyst is 4.2, the molar ratio of the sum of the moles of sodium carbonate and sodium phosphate to ammonia is 1.4, and the molar ratio of sodium carbonate to sodium phosphate is 1.9. Add pentasodium ethylenediaminetetramethylenephosphonate, the molar ratio of pentasodium ethylenediaminetetramethylenephosphonate to Mo in the catalyst powder is 2.4, react and dissolve under stirring conditions for 6 hours, and then filter to obtain a tungsten-molybdenum solution and a filter residue containing nickel and aluminum; the obtained residue is mixed with nitric acid, and the molar ratio of nitric acid to nickel in the catalyst powder is 2.2:1. Add dodecyltrimethylammonium chloride, the molar ratio of dodecyltrimethylammonium chloride to Ni in the catalyst powder is 1.4, react and dissolve under stirring conditions for 6.5 hours, filter to obtain a solution containing nickel and aluminum. The Al in the sodium aluminate solution accounts for 33% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 5 equal parts by volume. Deionized water is added to the reaction tank, and the W, Mo solution and the Ni, Al solution are added to the reaction tank in parallel to perform a gelling reaction. The reaction pH is controlled at 8.1 and the reaction temperature is 68°C. After 1.1 hours of reaction, a precipitate slurry containing nickel, molybdenum, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 76°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 12.9. After aging for 0.2 hours, the aging pH value is controlled to 9.3. After aging for 0.15 hours, the pH value is then controlled to 5.3, and the aging time is 0.2 hours. The above operation process is repeated 5 times to end aging. The aged slurry is filtered, and the filter cake is dried at 90°C for 8 hours, rolled, and extruded. Wash with deionized water at room temperature until neutral. The dried material was dried at 80°C for 8 hours, and the dried material was calcined at 540°C for 4 hours to obtain catalyst D. The catalyst composition and main properties are shown in Table 1.
[0037] Comparative Example 1 The same as Example 1, the reference agent E was prepared, and all the sodium aluminate solution was added at one time during the aging process of the precipitate slurry containing nickel, molybdenum, tungsten and aluminum, and the aging pH value was fixed (one aging). The specific preparation process is as follows: The crushed catalyst powder is mixed with a mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia water. The molar ratio of sodium carbonate, sodium phosphate and ammonia in the mixed alkaline solution of sodium carbonate, sodium phosphate and ammonia to the active metal (in terms of oxide) in the crushed catalyst is 3.5, the molar ratio of the sum of the moles of sodium carbonate and sodium phosphate to ammonia is 1.2, and the molar ratio of sodium carbonate to sodium phosphate is 1.5. Sodium polyaspartate is added, and the molar ratio of sodium polyaspartate to Mo in the extraction catalyst is 2.5. The reaction and dissolution are carried out under stirring for 6 hours, and then filtered to obtain a tungsten-molybdenum solution and a filter residue containing nickel and aluminum; the obtained residue is mixed with nitric acid, and octadecyl trimethyl ammonium bromide is added. The molar ratio of nitric acid to nickel in the catalyst powder is 2.0:1. The molar ratio of octadecyl trimethyl ammonium bromide to Ni in the extracted catalyst is 1.3. The reaction and dissolution are carried out under stirring for 5 hours, and filtered to obtain a nickel-aluminum solution. The Al in the sodium aluminate solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst. Deionized water was added to the reaction tank, and the tungsten-molybdenum solution and the nickel-aluminum solution were added to the reaction tank in parallel for gelation reaction. The reaction pH was controlled at 8.3, the reaction temperature was 60°C, and after 1.0 hour of reaction, a precipitate slurry containing nickel, molybdenum, tungsten and aluminum was generated. The obtained slurry was aged at 76°C. During aging, all sodium aluminate solution was added, and the pH was controlled at 8.0. After aging for 2 hours, the aging was terminated. The aged slurry was filtered, the filter cake was dried at 100°C for 8 hours, rolled, and extruded. Wash with deionized water at room temperature until neutral. Dry at 100°C for 8 hours, and roast the dried material at 530°C for 5 hours to obtain catalyst E. The catalyst composition and main properties are shown in Table 1.
[0038] Comparative Example 2 The same method as in Example 1 was used to prepare the reference agent F (which contained many impurities and could not be formed) without adding the organic reagent P1 during the catalyst preparation process.
[0039] Comparative Example 3 The same method as in Example 1 was used to prepare the reference agent G (which contained many impurities and could not be formed) without adding the organic reagent P2 during the catalyst preparation process.
[0040] Comparative Example 4 As in Example 1, the catalyst preparation process adopts a mixed dissolution reaction of sodium carbonate and ammonia, and the molar ratio of the total moles of sodium carbonate and ammonia to the catalyst powder calculated as oxide is 3.0:1; and reference agent H (with many impurities and unable to be formed) is prepared.
[0041] Comparative Example 5 The same as in Example 1, the catalyst preparation process adopts sodium carbonate, sodium phosphate and ammonia mixed dissolution reaction, the molar ratio of the total mole of sodium carbonate, sodium phosphate and ammonia to the catalyst powder as oxide is 1.1:1; the molar ratio of the sum of the moles of sodium carbonate and sodium phosphate to ammonia is 0.5, and the molar ratio of sodium carbonate to sodium phosphate is 0.4, and the reference agent I (more impurities and poor mechanical strength) is prepared. Example 5
[0042] This example is an activity evaluation experiment of the catalyst of the present invention, and is compared with the catalyst of the comparative example. The catalysts A, B, C, D of the present invention and the catalyst E of the comparative example were respectively used to conduct comparative evaluation tests on a 200mL small hydrogenation device. In order to further evaluate the ability of the catalyst to saturate aromatics, catalytic diesel with a high aromatic content was selected as the test raw material. The main properties of the raw materials are shown in Table 3. Process conditions for catalyst activity evaluation: hydrogen partial pressure of 6.4MPa, reaction temperature of 360℃, liquid hourly volume space velocity of 1.7h -1 , the hydrogen-oil volume ratio is 500:1, and the evaluation results are shown in Tables 4 to 6. As can be seen from Tables 1 to 2, compared with the comparative example catalyst, the catalyst prepared by the method of the present invention has less impurity content, larger pore volume and surface area, more surface active metals, and higher active metal utilization rate. As can be seen from Table 3, the catalyst activity evaluation uses a high aromatic content of the feedstock oil, which will also increase the difficulty of hydrogenation saturation, ultra-deep hydrodesulfurization and denitrogenation of the feedstock oil. As can be seen from the evaluation results of Tables 4 to 5, the catalyst prepared by the method of the present invention not only has excellent hydrodesulfurization activity and hydrodenitrogenation activity, but also has excellent hydrogenation saturation performance, which effectively reduces the aromatic content of heavy distillate oil. The catalyst prepared by the method of the present invention is used for processing heavy distillate oil, especially for processing inferior diesel fractions with high aromatic content and high processing difficulty. It has excellent hydrogenation saturation, hydrodesulfurization and hydrodenitrogenation performance, effectively reduces the content of polycyclic aromatic hydrocarbons, and improves the cetane number of diesel. Table 6 shows the activity evaluation results of the catalyst after running for 2000 hours under the unchanged evaluation conditions. It can be seen that the fresh catalyst prepared by the method of the present invention using the waste bulk catalyst has good activity stability due to its small amount of impurities.
[0043] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples Catalyst No. A B C D E F G H I NiO,wt% 18.2 18.8 17.9 17.6 18.3 10.2 13.4 14.7 15.2 <![CDATA[WO3,wt%]]> 30.4 29.6 30.1 30.7 30.1 19.4 20.8 18.9 22.4 <![CDATA[MoO3,wt%]]> 15.2 15.0 15.8 15.5 15.3 9.2 10.3 8.6 12.2 <![CDATA[Al2O3,wt%]]> margin margin margin margin margin margin margin margin margin <![CDATA[Fe2O3,wt%]]> 0.106 0.108 0.104 0.095 0.110 0.667 0.522 0.693 0.473 <![CDATA[V2O5,wt%]]> 0.084 0.088 0.079 0.093 0.092 0..476 0..414 0..505 0..383 <![CDATA[As2O3,wt%]]> 0.066 0.061 0.069 0.073 0.079 0.298 0.242 0.303 0.207 <![CDATA[Na2O,wt%]]> 0.052 0.043 0.048 0.040 0..051 0.401 0.352 0.423 0.241 <![CDATA[Specific surface area, m 2 / g]]> 292 283 297 304 197 - - - - Pore volume, mL / g 0.431 0.418 0.438 0.454 0.247 - - - - Mechanical strength, N / mm 19.3 19.6 19.9 19.5 19.0 Unable to form Unable to form Unable to form 5.5 Pore distribution <4nm 5.13 6.56 4.87 4,54 33.67 - - - - 4nm~6nm 6.75 7.93 5.37 5.01 25.51 - - - - 6nm~10nm 59.23 59.12 60.02 60.23 25.43 - - - - 10nm~15nm 19.56 18.01 19.86 19.90 8.09 - - - - >15nm 9,33 8.38 9.88 10.32 7.30 - - - - Table 2 Weight ratio of active metal oxides in the catalyst surface phase and bulk phase Catalyst No. A B C D E <