Ce modified Co-Mn material and preparation method and application thereof

By using Ce-modified Co-Mn catalyst in diesel engine exhaust, the deficiencies of the existing NOx removal catalysts in terms of low temperature and sulfur resistance are solved, achieving efficient and sulfur-tolerant NOx removal effects, improving the mine operating environment and Personnel health and safety.

CN118807769APending Publication Date: 2024-10-22SHANDONG UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410829418.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing NOx removal catalysts in diesel engine exhaust have deficiencies in low temperature and sulfur resistance. In particular, they are easily deactivated in environments containing sulfur dioxide, resulting in poor catalytic effect, high cost, low removal rate, and short lifespan.

Method used

Using PVP as a complexing agent, a Ce-modified Co-Mn catalyst was prepared through a hydrothermal method to form a cauliflower-like surface structure with a high specific surface area, improve the contact efficiency between active components and polluting gases, achieve efficient removal of NOx, and improve the catalyst sulfur resistance.

Benefits of technology

It achieves close to 100% NOx removal efficiency and high nitrogen selectivity at low temperatures, and can still maintain an 85% NO conversion rate in an environment containing sulfur dioxide, significantly improving the sulfur tolerance and service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807769A_ABST
    Figure CN118807769A_ABST
Patent Text Reader

Abstract

The invention discloses a Ce modified Co-Mn material as well as a preparation method and application thereof, and belongs to the technical field of catalytic treatment of tail gas pollutants of mining diesel vehicles. The preparation method of the Ce modified Co-Mn material comprises the following steps: mixing a cobalt salt, a manganese salt, a cerium salt, a dispersing agent and a complexing agent, and heating to obtain the Ce modified Co-Mn material, the complexing agent is polyvinylpyrrolidone. The PVP is adopted as the complexing agent, the cobalt salt, the manganese salt, the cerium salt and the complexing agent are dispersed in the dispersing agent, the formed product structure is a cauliflower-shaped surface structure with a high specific surface area, and the contact efficiency between the active component and the pollution gas is remarkably improved. According to the Ce modified Co-Mn material prepared by the invention, efficient removal of NO is realized, and the problems of high cost, easy generation of secondary pollution, low removal rate, short service life, poor sulfur resistance and the like of a traditional catalyst are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalytic treatment of exhaust pollutants of mining diesel vehicles, and in particular to a Ce-modified Co-Mn material and a preparation method and application thereof. Background Art

[0002] Diesel-powered machines play a vital role in coal mining and transportation. However, the working environment in the mine is relatively closed and the gas circulation is not smooth, which makes it difficult for toxic and harmful substances (such as nitrogen oxides and sulfur dioxide) in diesel engine exhaust to be quickly diluted and diffused, seriously affecting the health of workers. x , x = 1, 2) has a great impact on the respiratory and nervous systems of the human body. Therefore, NO in diesel exhaust is x The removal of NOx has become an important part of protecting the life and health of underground workers. At present, ammonia selective catalytic reduction (NH3-SCR) has become the main method to solve NOx emissions and is widely used in diesel engine exhaust emission devices. The only drawback is that the V2O5-WO3 (MoO3) / TiO2 catalyst used in the industrialized NH3-SCR technology has excellent SCR performance, but it is also accompanied by problems such as strong toxicity of V species and poor sulfur resistance. It is easy to deactivate in an environment containing sulfur dioxide, resulting in a deterioration of the catalytic effect, which has severely restricted its long-term application. Therefore, the development of new, efficient, water-resistant and sulfur-resistant, and environmentally friendly low-temperature (≤300°C) SCR catalysts has become the focus and difficulty of new catalysts.

[0003] So far, the main research direction of NH3-SCR is to use non-precious metal materials to replace precious metal materials in order to reduce costs while maintaining denitration performance. x 、CoO x ,FeO x 、MoO x , WO x Transition metal oxides such as MnO have been widely studied due to their excellent performance in low-temperature NH3-SCR reactions. x With its abundant unstable oxygen and multiple variable valence states (especially high Mn 3+ / Mn 4+ The research on MnO2 has become the main research direction of denitrification catalyst materials. However, single Mn-based catalysts still have some shortcomings that need to be solved, such as poor sulfur resistance and low N2 selectivity. Further research found that these problems can be solved by adding other metals to Mn-based catalysts. Among many metals, Co has attracted widespread attention due to its unique redox ability. The introduction of Co makes MnO2 xA large number of high-valent metal ions and chemically adsorbed oxygen species are generated on the surface, enriching the number of acid sites and significantly improving the redox ability and electron transfer efficiency of Co-Mn oxides. The synergistic effect between Co and Mn can reduce the NH3-SCR reaction temperature and improve the sulfur resistance of the catalyst. In addition, CeO2, as a rare earth metal oxide with strong oxygen storage and release capacity, is also widely used in NH3-SCR catalysts. Studies have shown that in the presence of MnO x The introduction of Ce into the catalyst can form a special Mn-O-Ce structure, and the rich variable valence cycles on its surface can greatly reduce the reaction temperature and increase the number of acid sites. However, such catalysts in the prior art still have certain deficiencies in terms of the number of reaction sites, sulfur resistance, and the complexity of the preparation method, and still need to be improved. Therefore, how to make the catalyst have low-temperature NH3-SCR activity while maintaining sulfur resistance has become a research focus that needs to be solved urgently. Summary of the invention

[0004] The object of the present invention is to provide a Ce-modified Co-Mn material and a preparation method and application thereof. The present invention adopts PVP as a complexing agent, and disperses cobalt salt, manganese salt, cerium salt and complexing agent in a dispersant, and the formed product structure is a cauliflower-like surface structure with a high specific surface area, which significantly improves the contact efficiency between the active component and the polluted gas. The Ce-modified Co-Mn material (Ce / CoMn catalyst) prepared by the present invention realizes the efficient removal of NO, and solves the problems of high cost, easy to generate secondary pollution, low removal rate, short life and poor sulfur resistance of traditional catalysts.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention is to provide a method for preparing a Ce / CoMn catalyst, comprising the following steps:

[0007] Mixing a cobalt salt, a manganese salt, a cerium salt, a dispersant and a complexing agent to obtain a mixture, and heating the mixture to obtain the Ce / CoMn catalyst;

[0008] The complexing agent is polyvinyl pyrrolidone (PVP).

[0009] Preferably, the cobalt salt is cobalt nitrate, the manganese salt is manganese nitrate, the cerium salt is cerium nitrate, and the dispersant is ethylene glycol.

[0010] Preferably, the molar ratio of the cerium salt to the manganese salt is 0-0.1, and is not 0; the molar ratio of the cobalt salt to the manganese salt is 1:2; the dispersant accounts for 91-91.03wt% in the mixture, and the complexing agent accounts for 0.73-0.74wt% in the mixture.

[0011] Preferably, the heating comprises the following steps: heating at 180°C for 12 hours, heating to 600°C at a heating rate of 5°C / min, and maintaining for 4 hours.

[0012] The high temperature heating treatment of the present invention can remove organic components in the material and fully oxidize the material.

[0013] Preferably, after the heating operation, a crushing step is further included; the crushing step is crushing until it passes through a 40-60 mesh sieve.

[0014] The second technical solution of the present invention is to provide a Ce / CoMn catalyst obtained according to the above preparation method.

[0015] Preferably, the molar ratio of Ce element to Mn element in the Ce / CoMn catalyst is 0.05.

[0016] Through research, it is found that, under the preparation method of the present invention, the introduction of 5% Ce can cause the Co-Mn spinel structure to collapse, thereby maintaining a higher degree of dispersion of each metal, so that the synergistic effect between Co-Mn-Ce can be fully exerted, and the contact efficiency between active components and pollutants can be effectively promoted, thereby further improving the catalytic performance of the catalyst, reducing the reaction temperature window, and improving sulfur resistance, which has broad application prospects.

[0017] The third technical solution of the present invention is to provide an application of the above-mentioned Ce / CoMn catalyst in the field of nitrogen oxide removal.

[0018] The beneficial technical effects of the present invention are as follows:

[0019] The present invention selects two transition metals as prerequisite materials, uses rare earth metals as modified materials, and adopts a hydrothermal method to prepare a rare earth-transition metal oxide catalyst, which not only achieves efficient removal of NO, but also reduces production costs.

[0020] The present invention adopts PVP as a complexing agent, and disperses cobalt salt, manganese salt, cerium salt and the complexing agent in the dispersant, so that the formed product structure is a cauliflower-like surface structure with a high specific surface area, which significantly improves the contact efficiency between the active component and the polluted gas.

[0021] The Ce / CoMn catalyst prepared by the present invention realizes the efficient removal of NO, solves the problems of high cost, easy to generate secondary pollution, low removal rate, short life and poor sulfur resistance of traditional catalysts, and can realize the removal of nitrogen oxides in the exhaust gas of diesel vehicles in underground mines, effectively improving the working environment in the mines and the safety of people's lives and property.

[0022] The present invention uses high-space-velocity NO to detect the NO conversion rate and nitrogen selectivity of the catalyst. The results show that the prepared catalyst can achieve nearly 100% NO removal efficiency and high nitrogen selectivity at a relatively low temperature. Sulfur dioxide is introduced into the tail gas to detect the sulfur resistance of the catalyst. The results show that the prepared catalyst effectively overcomes the problem of poor sulfur resistance and can still achieve 85% NO conversion rate after 4 hours of use. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The following is a flow chart for the preparation of the products of Examples 1-3.

[0025] Figure 2 The SEM morphology images of the products of Example 2 and Comparative Example 2. Among them, (a) and (b) are SEM morphology images of Example 2 at different magnifications, and (c) is the SEM morphology image of the product of Comparative Example 2.

[0026] Figure 3 It is the XRD diagram of the products of Examples 1-3 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0027] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0028] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0030] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0031] Figure 1 The following is a flow chart for the preparation of the products of Examples 1-3.

[0032] Unless otherwise specified, "overnight" in the present invention is calculated as 12 hours.

[0033] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.

[0034] Example 1

[0035] Preparation of Ce / CoMn catalyst:

[0036] 3 mL of deionized water and 100 mL of ethylene glycol were mixed to obtain solution A, 2.9 g of cobalt nitrate hexahydrate (0.01 mol) was dissolved in 30 mL of deionized water, and stirred evenly under magnetic stirring to obtain solution B. Then, solution A was slowly poured into solution B under magnetic stirring and stirred evenly, 7.16 g of manganese nitrate aqueous solution (containing 0.02 mol of manganese nitrate) and 0.0433 g of cerium nitrate hexahydrate (0.0001 mol) were added to the above mixed solution, and 0.9 g of PVP was added and fully dissolved after stirring and mixing evenly, and then the mixed solution was added to a polytetrafluoroethylene-lined autoclave, reacted at 180° C. for 12 h, washed alternately with deionized water and anhydrous ethanol after cooling, and dried at 60° C. overnight to obtain Ce / CoMn precursor. The prepared Ce / CoMn precursor was heated to 600° C. at a heating rate of 5° C. / min in a muffle furnace and calcined for 4 h, and then crushed to pass through a 40-mesh sieve to obtain a Ce / CoMn catalyst (denoted as 1CMO).

[0037] Example 2

[0038] Preparation of Ce / CoMn catalyst:

[0039] 3 mL of deionized water and 100 mL of ethylene glycol were mixed to obtain solution A, 2.9 g of cobalt nitrate hexahydrate was dissolved in 30 mL of deionized water, and stirred evenly under magnetic stirring to obtain solution B. Then, solution A was slowly poured into solution B under magnetic stirring and stirred evenly, 7.16 g of manganese nitrate aqueous solution (containing 0.02 mol of manganese nitrate) and 0.217 g of cerium nitrate hexahydrate were added to the above mixed solution, and 0.9 g of PVP was added and fully dissolved after stirring and mixing evenly, and then the mixed solution was added to a polytetrafluoroethylene-lined autoclave, reacted at 180 ° C for 12 h, and washed alternately with deionized water and anhydrous ethanol after cooling, and dried at 60 ° C overnight to obtain Ce / CoMn precursor. The prepared Ce / CoMn precursor was heated to 600 ° C in a muffle furnace at a heating rate of 5 ° C / min and calcined for 4 h, crushed to 40 mesh, and obtained Ce / CoMn catalyst (referred to as 5CMO).

[0040] Example 3

[0041] Preparation of Ce / CoMn catalyst:

[0042] 3 mL of deionized water and 100 mL of ethylene glycol were mixed to obtain solution A, 2.9 g of cobalt nitrate hexahydrate was dissolved in 30 mL of deionized water, and stirred evenly under magnetic stirring to obtain solution B. Then, solution A was slowly poured into solution B under magnetic stirring and stirred evenly, 7.16 g of manganese nitrate aqueous solution (containing 0.02 mol of manganese nitrate) and 0.433 g of cerium nitrate hexahydrate were added to the above mixed solution, and 0.9 g of PVP was added and fully dissolved after stirring and mixing evenly, and then the mixed solution was added to a polytetrafluoroethylene-lined autoclave, reacted at 180 ° C for 12 h, and washed alternately with deionized water and anhydrous ethanol after cooling, and dried at 60 ° C overnight to obtain Ce / CoMn precursor. The prepared Ce / CoMn precursor was heated to 600 ° C at a heating rate of 5 ° C / min in a muffle furnace and calcined for 4 h, crushed to 40 mesh, and obtained Ce / CoMn catalyst (recorded as 10CMO).

[0043] Comparative Example 1

[0044] Preparation of Ce-free CoMn catalyst:

[0045] 3 mL of deionized water and 100 mL of ethylene glycol were mixed to obtain solution A, 2.9 g of cobalt nitrate hexahydrate was dissolved in 30 mL of deionized water, and stirred evenly under magnetic stirring to obtain solution B. Then, solution A was slowly poured into solution B under magnetic stirring and stirred evenly, 7.16 g of manganese nitrate aqueous solution (containing 0.02 mol of manganese nitrate) was added to the mixed solution, and 0.9 g of PVP was added and fully dissolved after stirring and mixing evenly, and then the mixed solution was added to a polytetrafluoroethylene-lined autoclave, reacted at 180 ° C for 12 h, and washed alternately with deionized water and anhydrous ethanol after cooling, and dried at 60 ° C overnight to obtain Ce / CoMn precursor. The prepared Ce / CoMn precursor was heated to 600 ° C in a muffle furnace at a heating rate of 5 ° C / min and calcined for 4 h, crushed to 40 mesh, and a CoMn catalyst (denoted as CMO) was obtained.

[0046] Comparative Example 2

[0047] Preparation of Ce / CoMn catalyst:

[0048] 3 mL of deionized water and 100 mL of ethylene glycol were mixed to obtain solution A, 2.9 g of cobalt nitrate hexahydrate was dissolved in 30 mL of deionized water, and stirred evenly under magnetic stirring to obtain solution B. Then, solution A was slowly poured into solution B under magnetic stirring and stirred evenly, 7.16 g of manganese nitrate aqueous solution (containing 0.02 mol of manganese nitrate) and 0.217 g of cerium nitrate hexahydrate were added to the above mixed solution, and 1.98 g of glucose was added and fully dissolved after stirring and mixing evenly, and then the mixed solution was added to a polytetrafluoroethylene-lined autoclave, reacted at 180 ° C for 12 h, and washed alternately with deionized water and anhydrous ethanol after cooling, and dried at 60 ° C overnight to obtain Ce / CoMn precursor. The prepared Ce / CoMn precursor was heated to 600 ° C in a muffle furnace at a heating rate of 5 ° C / min and calcined for 4 h, crushed to 40 mesh, and obtained Ce / CoMn catalyst (recorded as 5CMO-g).

[0049] Figure 2 The SEM morphology images of the products of Example 2 and Comparative Example 2. Among them, (a) and (b) are SEM morphology images of Example 2 at different magnifications, and (c) is the SEM morphology image of the product of Comparative Example 2.

[0050] Figure 3 The XRD diagrams of the products of Examples 1-3 and Comparative Examples 1-2 are shown in FIG. Figure 3It can be seen that when the introduction amount of Ce reaches 5%, the spinel phase begins to disappear, and the fluorite structure diffraction peak of CeO2 is observed, indicating that the excessive introduction of Ce content will cause the Co-Mn spinel structure to collapse and be accompanied by the formation of CeO2. At this time, Ce, Mn and Co are highly dispersed. Due to the increase in the dispersion of metal ions, strong interactions are generated between the ions, and the ions of different valence states are transformed into each other. The content and exposure ratio of active components increase, which greatly improves the migration rate of lattice oxygen, thereby greatly increasing the catalytic performance.

[0051] Effect verification

[0052] (1) The NO conversion rate of the above catalyst was tested: the test was carried out using a fixed bed reactor, the catalyst addition amount was 0.2 g, the gas introduced was 500 ppm NO, 500 ppm NH3 and 8 vol% oxygen, the test temperature range was 50-300°C, and the exhaust gas concentration under different temperature conditions was detected using a flue gas analyzer under stable exhaust gas; before the test began, the catalyst was purged with N2 at 100°C for 30 minutes to remove water molecules and impurities on the surface. The test results are shown in Table 1.

[0053] The calculation formula of NO conversion rate is:

[0054]

[0055] In the formula, [NO] out Represents the concentration of outlet NO; [NO] in Represents the inlet NO concentration.

[0056] Table 1 NO conversion rate (%)

[0057]

[0058]

[0059] As can be seen from Table 1, although pure CMO shows acceptable catalytic activity, its low-temperature NH3-SCR activity (50-200°C) is low. After the introduction of Ce, all catalysts in each embodiment achieved a NO conversion rate of more than 87% at 100°C, and a NO conversion rate of nearly 100% at 150-200°C. Among them, 5CMO showed the best NO conversion rate in all temperature zones, and showed a NO conversion rate of nearly 100% at 150-250°C. When the reaction temperature exceeds 250°C, the conversion rate of NO begins to decline and the catalytic activity is relatively reduced, which can be attributed to the oxidation of NH3 caused by high temperature. It can be concluded that the introduction of an appropriate amount of Ce can greatly improve the catalytic activity of the catalyst. By comparing the NO conversion rates of 5CMO and 5CMO-g, it is found that PVP as a chelating agent can better improve the catalytic efficiency of the catalyst, which may be related to the catalyst morphology and metal dispersibility.

[0060] (2) The nitrogen selectivity of the above catalyst was tested: the test was carried out using a fixed bed reactor, the catalyst addition amount was 0.2 g, the gas introduced was 500 ppm NO, 500 ppm NH3 and 8 vol% oxygen, and the test temperature range was 50-300°C; before the test began, the catalyst was purged with N2 at a relatively low temperature for 30 minutes. The test results are shown in Table 2.

[0061] The nitrogen selectivity calculation formula is:

[0062]

[0063] In the formula, [N2O] out Represents the outlet N2O concentration; [NO x ] in Representative entrance NO x Concentration; [NH3] in represents the concentration of inlet NH3; [NO x ] out Representative export NO x Concentration of [NH3] out Represents the outlet NH3 concentration.

[0064] Table 2 N2 selectivity (%)

[0065]

[0066]

[0067] As shown in Table 2, all catalysts showed outstanding N2 selectivity at low temperature, which was greater than 74% at 150°C. However, the selectivity gradually decreased with increasing temperature, because NH3 decomposed into N2O at high temperature, which reduced the N2 selectivity. Among all catalysts, 5CMO also showed the best N2 selectivity.

[0068] (3) The catalytic performance of 5CMO and 5CMO-g at different air velocities was tested to study the effect of tail gas flow rate on the catalytic NO conversion rate. The test was carried out in a fixed bed reactor with a catalyst addition of 0.2 g, 500 ppm NO, 500 ppm NH3 and 8 vol% oxygen as the gas, the test temperature was 50-300 °C, and the air velocities were set to 40000 h-1 and 40000 h-2 respectively. -1 、60000h -1 and 100000h -1 Before the test, the catalyst was purged with N2 at a relatively low temperature for 30 min. The test results are shown in Table 3.

[0069] Table 3 NO conversion rate at different space velocities

[0070] airspeed <![CDATA[40000h -1 ]]> <![CDATA[60000h -1 ]]> <![CDATA[100000h -1 ]]> Temperature at maximum conversion 150~200℃ 160~190℃ 175~200℃ 5CMONO conversion rate ~100% ~99% ~98% 5CMO-gNO conversion rate ~99% ~98% ~96%

[0071] The results show that the airspeed is 40000h -1 When the NO conversion rate of 5CMO reaches nearly 100% at 150-200℃, the space velocity is increased to 60000h -1 The NO conversion rate of 5CMO reached 99% at 160-190℃. When the space velocity was increased to 100000h -1 When the NO conversion rate of 5CMO was 175-200℃, it reached a conversion rate of nearly 98%. However, the NO conversion rate of 5CMO-g at different space velocities was lower than that of 5CMO and was more affected by the space velocity. Therefore, it was found through experiments that 5CMO has a better catalytic effect in harsh environments. Although the space velocity has an effect on the NO conversion rate of the catalyst, the effect is small, indicating that the 5CMO catalyst can maintain a high catalytic efficiency in a more complex environment.

[0072] (3) The sulfur resistance of 5CMO and 5CMO-g was tested to study the sustainable use ability of the catalyst. The test was carried out using a fixed bed reactor, with a catalyst addition of 0.2 g, 500 ppm of NO, 500 ppm of NH3 and 8 vol% of oxygen introduced, and 50 ppm of SO2 was introduced to simulate a harsh environment to study the effect of the presence of SO2 in the exhaust gas on the catalytic NO conversion rate; the test temperature was 50-300 ° C, and the air velocity was set to 40000 h -1Before the test, the catalyst was purged with N2 at a relatively low temperature for 30 min. The test results are shown in Table 4.

[0073] Table 4 Sulfur resistance test of materials at 160°C

[0074] 5CMO 5CMO-g <![CDATA[Conversion rate before introducing SO2]]> ~100% ~98% Balanced conversion rate ~85% ~80% <![CDATA[Conversion rate after stopping and resuming SO2 supply]]> ~96% ~93%

[0075] After testing, the effect of SO2 on the NO conversion rate of the catalyst was obtained. The results show that when there is no SO2 in the exhaust gas, the NO conversion rate of 5CMO is -1 , it reaches nearly 100% at 160℃. When SO2 is introduced into the tail gas, the conversion rate of NO begins to decrease gradually over time. After about 4 hours of reaction in the atmosphere of SO2, the conversion rate of NO reaches an equilibrium state of about 85%. After 12 hours of reaction, the introduction of SO2 is cancelled, and the conversion rate of NO gradually recovers, but the performance still decreases, and gradually reaches the highest conversion rate of about 96% after 2 hours. In this case, the performance of 5CMO is better than that of 5CMO-g. The conversion rate of NO of 5CMO-g reaches an equilibrium state of about 80% after about 4 hours of reaction in the atmosphere of SO2. After 12 hours of reaction, the introduction of NO is cancelled and the conversion rate recovers to 93%. This shows that the 5CMO catalyst prepared with PVP as a complexing agent has better SO2 tolerance, and the catalytic performance of the catalyst gradually recovers when there is no SO2 in the tail gas, and the catalyst will not be deactivated to a large extent due to long-term contact with SO2. The 5CMO catalyst prepared with PVP as a complexing agent can better improve the dispersion of metal ions while accelerating the formation of CeO2, which balances the surface acid sites while reducing the adsorption capacity of the catalyst active components for SO2. At this time, SO2 is more inclined to adsorb on CeO2, thereby further avoiding the sulfidation of the active components, thereby improving the sulfur resistance of the catalyst.

[0076] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a Ce / CoMn catalyst, characterized in that: The following steps are involved: Mixing a cobalt salt, a manganese salt, a cerium salt, a dispersant and a complexing agent to obtain a mixture, and heating the mixture to obtain the Ce / CoMn catalyst; The complexing agent is polyvinyl pyrrolidone.

2. The preparation method according to claim 1, characterized in that: The cobalt salt is cobalt nitrate, the manganese salt is manganese nitrate, the cerium salt is cerium nitrate, and the dispersant is ethylene glycol.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the cerium salt to the manganese salt is 0-0.1, and is not 0; the molar ratio of the cobalt salt to the manganese salt is 1:2; the dispersant accounts for 91-91.03wt% of the mixture, and the complexing agent accounts for 0.73-0.74wt% of the mixture.

4. The preparation method according to claim 1, characterized in that: The heating comprises the following steps: heating at 180° C. for 12 hours, heating to 600° C. at a heating rate of 5° C. / min, and maintaining the temperature for 4 hours.

5. The preparation method according to claim 1, characterized in that: After the heating operation, a crushing step is further included; the crushing step is crushing until the product passes through a 40-60 mesh sieve.

6. A Ce / CoMn catalyst obtained according to the preparation method according to any one of claims 1 to 5.

7. The Ce / CoMn catalyst according to claim 6, characterized in that The molar ratio of Ce element to Mn element in the Ce / CoMn catalyst is 0.

05.

8. Use of the Ce / CoMn catalyst according to claim 6 or 7 in the field of nitrogen oxide removal.

Citation Information

Patent Citations

  • Low-temperature denitration catalyst with mesocrystal structure and preparation method of low-temperature denitration catalyst with mesocrystal structure

    CN106311221A

  • Transition metal doped cerium-based complex oxide polyhedron catalyst and preparation method

    CN107754779A

  • Modified low-temperature SCO denitrification catalyst and preparation method thereof

    CN108262049A