Catalyst added with complexing agent and used for synthesizing dimethyl oxalate and preparing methyl glycolate through hydrogenation as well as preparation method and application of catalyst

By uniformly covering the surface of copper particles with a silver shell layer, the copper-silver core-shell structure catalyst solves the problems of low selectivity and poor stability of existing catalysts, achieves high selectivity and high stability catalytic effects, and reduces production costs and Extended catalyst life.

CN118807772AActive Publication Date: 2024-10-22TIANJIN UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410740701.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-10
Publication Date
2024-10-22
Estimated Expiration
2044-06-10

AI Technical Summary

Technical Problem

Among the existing catalysts for hydrogenating dimethyl oxalate to prepare methyl glycolate, the copper-based catalyst has low selectivity, the silver-based catalyst has high silver loading and poor stability, resulting in high production costs and reduced catalyst activity.

Method used

A bimetallic catalyst with a copper-silver core-shell structure is used to evenly cover the surface of copper particles with a silver shell layer and use silicon oxide as a carrier to prepare a catalyst with high catalytic activity and stability and reduce the silver loading.

Benefits of technology

The catalytic effect of high selectivity and high stability is achieved, the catalyst production cost is reduced, the yield of methyl glycolate is increased, and the service life of the catalyst is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807772A_ABST
    Figure CN118807772A_ABST
Patent Text Reader

Abstract

The invention discloses a complexing agent added catalyst for synthesizing dimethyl oxalate to prepare methyl glycolate through hydrogenation and a preparation method and application of the complexing agent added catalyst, the catalyst is a copper-silver bimetallic catalyst, active components are a copper species and a silver species, a carrier is silicon dioxide, and the carrier is a metal oxide. The structure of the copper-silver bimetallic catalyst is as follows: silver species uniformly cover the surface of copper species in the form of a shell layer to form a core-shell structure, the core-shell structure falls on a carrier silicon dioxide in the form of particles, and copper and silicon oxide form strong interaction. According to the preparation method, a catalyst precursor is synthesized through an ammonia distillation method, copper particles strongly interacting with silicon oxide are formed after reduction, then the copper-silver core-shell structure is synthesized through a replacement method, and in the preparation process, compactness, uniformity and compactness of a silver shell layer are guaranteed by adding different complexing agents and changing the pH value and the copper-silver mass ratio in the preparation process. The copper-silver bimetallic catalyst has the advantages of low silver loading capacity, high catalytic activity, high selectivity and high stability when being used for preparing methyl glycolate through dimethyl oxalate hydrogenation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a bimetallic catalyst, in particular to a catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating it to prepare methyl glycolate, and a preparation method and application thereof. The catalyst is used for hydrogenating dimethyl oxalate to prepare methyl glycolate (MG). Background Art

[0002] Methyl glycolate has a unique molecular structure: it has H, hydroxyl and ester functional groups at the same time, which makes it have the chemical properties of both alcohol and ester, and can undergo carbonylation reaction, hydrolysis reaction, oxidation reaction, etc. It is an important chemical raw material and is widely used in many fields such as chemical industry, medicine, pesticides, feed, fragrances and dyes.

[0003] my country's biodegradable material polyglycolic acid (PGA) industry has developed rapidly. Polyglycolic acid has strong environmental degradation and can be degraded into carbon dioxide and water in nature within 1-3 months. The demand is huge, so large-scale production of methyl glycolate, the raw material for synthesizing polyglycolic acid, is crucial. The traditional methyl glycolate production process has serious pollution and harsh reaction conditions, and it is impossible to produce methyl glycolate on a large scale. In recent years, the coal-based route to produce methyl glycolate by hydrogenation of dimethyl oxalate (DMO) has become one of the most promising coal chemical technologies in my country. It is expected that by regulating the distribution of hydrogenation reaction products, high-value-added biodegradable materials can be produced from coal. The process has high atomic utilization and is environmentally friendly, which is of great significance to promoting the high-end, diversified and low-carbon development of my country's coal chemical industry.

[0004] At present, the commonly used catalysts for preparing methyl glycolate by hydrogenation of dimethyl oxalate are copper-based catalysts and silver-based catalysts. Compared with copper-based catalysts, silver-based catalysts have weaker hydrogenation ability and weaker adsorption effect on methyl glycolate. Therefore, they can catalyze the highly selective hydrogenation of dimethyl oxalate to methyl glycolate, inhibit its deep hydrogenation, and show a higher methyl glycolate yield of more than 85%. However, silver-based catalysts still have the following problems: 1. In order to ensure that the silver species exists in the form of metallic silver and shows good catalytic activity, the catalyst silver loading is generally high, often greater than 10wt.%, expensive and costly; 2. The Tamman temperature of silver is low, and the reaction temperature easily leads to the agglomeration and sintering of silver particles, resulting in poor catalyst stability. If a carrier with strong interaction with the silver species is selected, the silver loses electrons, causing its activity to drop significantly, and the acid-base sites on the surface of the carrier easily promote side reactions, reducing selectivity. Summary of the invention

[0005] The invention aims to solve the problems of low selectivity of copper-based catalysts, high silver loading and poor stability of silver-based catalysts in the technology of hydrogenating dimethyl oxalate to prepare methyl glycolate. Copper nanoparticles that strongly interact with carrier silicon oxide are used as catalyst precursors, and a complexing agent is added during the preparation process to replace the metal on the surface of the copper particles with a single layer of uniform silver species, thereby reducing the silver loading and promoting the stability of the catalyst without reducing the metallic properties and activity of silver.

[0006] The present invention successfully prepares a copper-silver bimetallic catalyst with a copper-silver core-shell structure by using a replacement method and a complexing agent. When used for the reaction of preparing methyl glycolate by hydrogenation of dimethyl oxalate, the catalyst has the characteristics of simple preparation, high catalytic activity, high selectivity and high stability.

[0007] The technical solution adopted by the present invention is:

[0008] A catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating to prepare methyl glycolate comprises a carrier and an active component, wherein the active component is a copper species and a silver species, the carrier is silicon dioxide, and the structure of the copper-silver bimetallic catalyst is: the silver species is uniformly covered on the surface of the copper species in the form of a shell layer to form a core-shell structure, and the core-shell structure is located on the carrier silicon dioxide in the form of particles, wherein copper and silicon oxide form a strong interaction. First, a copper-containing catalyst precursor is prepared, and then the copper-containing catalyst precursor, a silver salt and a complexing agent are mixed and treated to obtain a finished catalyst product.

[0009] The core-shell structure here means that the silver particles are evenly dispersed on the surface of the copper particles like a shell, ensuring that there is a shell layer composed of silver particles coating the outside of the copper particles. At the same time, the silver shell is also uniform and dense, and can ensure the uniform dispersion of the Cu@Ag particles.

[0010] The silver species accounts for 1-10wt.% of the total mass of the copper-silver bimetallic catalyst, and the copper species accounts for 1-10wt.% of the total mass of the copper-silver bimetallic catalyst. The reason why the mass of the copper-silver bimetallic catalyst needs to be limited to the above range is that: 1. High silver content will make the distribution of the silver shell layer on the surface of the particles uneven, resulting in uneven particle size, which will lead to decreased activity; 2. Increased silver content may also cause part of the silver to not participate in the formation of the core-shell structure, and form silver flocs that grow freely outside the particles, causing some particles to agglomerate. 3. High copper content will cause the particles to be too large and the activity to decrease; 4. Increased copper content may also make the outer layer of copper unable to be completely covered by silver, and the exposed copper is easy to catalyze the deep hydrogenation of methyl glycolate to produce ethylene glycol, resulting in decreased selectivity.

[0011] The copper-silver bimetallic catalyst has a specific surface area of ​​50-300 m 2 / g, average pore volume is 0.4-1.7cm 3 / g, the average pore size is 5-30nm. The particle size of the copper-silver bimetal is 1.0-10nm, and the thickness of the silver shell is 0.2-2nm; the particle size of the copper-silver bimetal is 1.0-8nm, and the thickness of the silver shell is 0.2-1nm.

[0012] Another object of the present invention is to provide a method for preparing a catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating it to prepare methyl glycolate, comprising the following steps:

[0013] (1) Dissolve copper nitrate in deionized water and add a certain volume of ammonia water;

[0014] (2) mixing the two solutions obtained in step (1), mechanically stirring the mixture, and dripping a certain amount of silica sol at a certain rate;

[0015] (3) aging the solution obtained in step (2), then heating to evaporate ammonia, and filtering and washing the obtained mixed solution;

[0016] (4) drying the product obtained in step (3) in an oven, calcining at high temperature to obtain a catalyst precursor, and performing a reduction treatment on the catalyst precursor;

[0017] (5) mixing the catalyst precursor obtained in step (4) with silver nitrate, ethanol and a complexing agent, adjusting the pH value, and subjecting the solution to ultrasonic treatment and mechanical stirring during the process;

[0018] (6) The solution obtained in step (5) is centrifuged to extract the Cu@Ag particles therein, which are then washed with ethanol and deionized water, and dried to obtain a finished catalyst product.

[0019] The complexing agent is selected from any one of phenylalanine, tyrosine, L-histidine (L-His), gelatin, polyvinylpyrrolidone (PVP), glycine, dl-malic acid, citric acid or tannic acid;

[0020] The stirring time in step (2) is 30 minutes; the aging time in step (3) is 4 hours, and the ammonia evaporation temperature is 80° C.; the drying conditions in step (4) are: the drying temperature is 80-130° C., and the drying time is 12-24 hours; the reduction treatment conditions are 300° C., and hydrogen reduction is 4 hours; the ambient temperature of the catalyst precursor, silver nitrate, ethanol and complexing agent in step (5) is room temperature, i.e., 20-30° C.; the drying conditions in step (6) are: the drying temperature is 80-130° C., and the drying time is 12-24 hours.

[0021] The amount of silver nitrate added in step (5) ensures that the copper-silver mass ratio is any one of 1:1, 2:1 and 1:2; the pH value of the solution is adjusted by adding an alkaline substance dropwise in step (5), and the pH value of the solution after adjustment is in the range of 8-12, preferably weakly alkaline.

[0022] Another object of the present invention is to provide an application of a catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating it to produce methyl glycolate, wherein the catalyst is used to catalyze the selective hydrogenation of dimethyl oxalate to produce methyl glycolate;

[0023] Specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst for reaction; the reaction pressure is 0.5-3.5 MPa; the reaction temperature is 180-240° C.; the mass space velocity of dimethyl oxalate is 0.1-4.0 h -1 ; The hydrogen ester molar ratio is 60-150.

[0024] The preferred scheme is: using the catalyst prepared by the preparation method of the core-shell copper-silver bimetallic catalyst synthesized by adding a complexing agent, and using the catalyst to catalyze the selective hydrogenation of dimethyl oxalate to produce methyl glycolate;

[0025] Specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst for reaction; the reaction pressure is 0.5-3.5 MPa; the reaction temperature is 180-240° C.; the mass space velocity of dimethyl oxalate is 0.1-4.0 h -1 ; The hydrogen ester molar ratio is 60-150.

[0026] The present invention has the following beneficial effects:

[0027] 1. The present invention successfully prepares a bimetallic catalyst with a copper-silver core-shell structure. The core-shell structure here means that silver particles are evenly dispersed on the surface of copper particles like a shell layer, ensuring that there is a shell layer composed of silver particles coating the outside of the copper particles. At the same time, the silver shell layer is also uniform and dense, and can ensure the uniform dispersion of Cu@Ag particles.

[0028] 2. The copper-silver bimetallic catalyst of the present invention has high stability when used in the heterogeneous hydrogenation reaction of dimethyl oxalate. The reason is that: layered copper silicate is used as a precursor, and copper nanometal particles with strong interaction with silicon oxide are formed after reduction, and the Ag species are located on the surface of the copper species. The interaction between copper and silicon oxide provides a basis for anchoring the silver species, which can prevent the sintering of silver particles and ensure that there is no problem of silver particle growth during long-term use, thereby improving its stability and greatly reducing the cost of catalyst replacement in industry.

[0029] 3. The copper-silicon bimetallic catalyst of the present invention has the characteristics of low silver loading and high catalytic activity when used for the heterogeneous hydrogenation reaction of dimethyl oxalate. Compared with the silver loading of more than 10wt.% in the prior art, the silver species loading in the present invention is only 4-6wt.%, and the MG yield can reach more than 90%. The catalyst silver loading in the present invention is low, the utilization efficiency of silver is greatly improved, and the catalyst production cost is greatly saved.

[0030] 4. Different complexing agents are added during the preparation of the copper-silver bimetallic catalyst of the present invention, and the copper-silver mass ratio is changed. The addition of the complexing agent changes the uniformity of the silver shell of the core-shell structure; the change in the mass ratio changes the size of the copper particles of the core-shell structure and the thickness of the silver shell. The present invention uses this method to control the size of the silver shell of Cu@Ag, thereby obtaining a core-shell copper-silver bimetallic catalyst with a copper-silver bimetallic particle size of 1.0-10nm and a silver shell size of 0.2-2nm, thereby changing the catalyst performance.

[0031] 5. The present invention changes the particle size of the copper-silver bimetallic particles and the formation of the core-shell structure by adjusting the pH value during the synthesis process.

[0032] 6. When the copper-silver bimetallic catalyst obtained by the present invention is used for the heterogeneous hydrogenation reaction of dimethyl oxalate, the raw materials for catalyst preparation are easily available, the reaction conditions are mild, the process is simple and controllable, the structure is stable, the operability is strong, and it has good industrial application prospects and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is the molecular formula of the complexing agent in the embodiment of the present invention;

[0034] Figure 2 This is a high-resolution TEM image of the Cu@Ag structure of the copper-silver bimetallic catalyst of the present invention;

[0035] Figure 3 This is a stability test of the catalysts in the comparative examples and embodiments of the present invention. DETAILED DESCRIPTION

[0036] The present invention is further described below by way of examples, which are not limited to the examples. Experimental methods without specific conditions specified in the examples are generally carried out under conventional conditions and conditions described in the manual, or under conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used are all commercially available unless otherwise specified.

[0037] The methods for online reduction of the catalyst and evaluation of the catalytic effect in this embodiment and comparative example are as follows:

[0038] In the present invention, the hydrogenation reaction of dimethyl oxalate is carried out in a fixed bed reactor. 0.5 g of catalyst is loaded, reduced at 300° C. in a hydrogen atmosphere of 2.5 MPa, with a gas flow rate of 80 mL / min, maintained for 4 hours, cooled to the reaction temperature, the dimethyl oxalate solution is gasified and mixed with hydrogen and then enters the reaction system, the hydrogen-ester ratio is 80, and the hydrogenation reaction is carried out at 2.5 MPa, 210° C. or 225° C. The product after the reaction is analyzed by gas chromatography, and the conversion rate of dimethyl oxalate and the selectivity and yield of methyl glycolate are calculated. Since the hydrogenation reaction of dimethyl oxalate is a series reaction and methyl glycolate is an intermediate hydrogenation product, the difference in selectivity for the intermediate product can only be reflected when the conversion rate is not 100%. Therefore, the reaction space velocity was adjusted so that the reaction conversion rate was 98.5%. In the process of stability evaluation, in order to make full use of all active sites to participate in the reaction and prevent the situation where the catalyst is deactivated while the conversion rate is still 100%, it is necessary to carry out stability evaluation under the condition that the conversion rate is not 100%. In order to characterize the thermal stability of the catalyst, the atmosphere is switched during the reaction, and the catalyst is heat treated at 350°C with nitrogen for 20 hours, and then the catalyst performance is tested by feeding again.

[0039] The specific experimental conditions of the comparative examples and catalysts of each embodiment are shown in Table 1 below, and the activity data are shown in Table 2.

[0040] Comparative Example 1

[0041] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, without complexing agent added, co-impregnation method, copper-silver mass ratio 1:1) This comparative example is the preparation of copper-silver bimetallic catalyst comparative sample 1 synthesized at 25°C without adding complexing agent, as follows:

[0042] Dissolve a certain amount of silver nitrate (AgNO3) and copper nitrate (Cu(NO3)2·3H2O) in 150 mL of deionized water, stir at room temperature, and avoid light. Then slowly add the corresponding amount of dried fumed silica and stir vigorously for 20 hours in the dark. Rotary evaporate the mixture at 40°C to remove excess water. Dry the obtained solid in a 110°C oven for 15 hours and calcine it at 400°C in a muffle furnace for 4 hours. Reduce the obtained catalyst at 300°C in H2 for 4 hours before use. The catalyst in this comparative example was reduced at 1.0 h in accordance with the above-mentioned online reduction conditions and catalyst evaluation method. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 11.0%, and during the period from 270 h to 500 h, the yield decreased from 38.7% to 11.6%.

[0043] Comparative Example 2

[0044] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, without complexing agent, replacement method, copper-silver mass ratio 1:1)

[0045] This comparative example is the preparation of the copper-silver bimetallic catalyst comparative sample 2 synthesized at 25°C without adding a complexing agent, as follows:

[0046] Preparation of catalyst precursor by ammonia evaporation method:

[0047] Weigh a certain amount of Cu(NO3)2·H2O and dissolve it in 150mL of deionized water, and mix it with a certain volume of ammonia water (25wt.%) to form a copper ammonia solution. After stirring for 30 minutes, a certain amount of silica sol is dripped into the copper ammonia solution at a certain rate and aged for 4 hours, then the solution is heated to 80°C to start ammonia evaporation, and the ammonia evaporation is completed when the pH of the solution drops to 6-7. The mixed solution is filtered and washed with deionized water. The obtained sample is placed in a 110°C oven to dry for 12 hours, calcined in a muffle furnace at 400°C for 4 hours, and then reduced in a H2 atmosphere at 300°C for 4 hours to obtain a catalyst precursor with a Cu loading of 10wt.%.

[0048] Preparation of copper-silver bimetallic catalyst:

[0049] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for 4h, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution. A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, and a certain volume of AgNO3 solution (mass ratio Cu: Ag = 1: 1) was added, and attention was paid to avoid light. After stirring and mixing for 90min, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12h to obtain the catalyst.

[0050] The catalyst of this comparative example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 9.1%, and during the period from 270 h to 500 h, the yield decreased from 44.5% to 23.9%.

[0051] Example 1

[0052] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, adding complexing agent phenylalanine, displacement method, copper-silver mass ratio 1:1)

[0053] This comparative example is a preparation of copper-silver bimetallic catalyst sample 1 synthesized at 25°C and added with a complexing agent phenylalanine, as follows:

[0054] Preparation of catalyst precursor by ammonia evaporation method:

[0055] Weigh 7.6g of Cu(NO3)2·H2O and dissolve it in 150mL of deionized water, and mix it with 25.9mL of ammonia water (ammonia water concentration is 25wt.%) to form a copper ammonia solution. After stirring for 30min, 50mL of silica sol is dripped into the copper ammonia solution at a certain rate (slowly dripped, such as: 1 drop per second, etc.) and aged for 4h, then the solution is heated to 80℃ to start ammonia evaporation, and the ammonia evaporation is completed when the pH of the solution drops to 6-7. The mixed solution is filtered and washed with deionized water (using a Buchner funnel). The obtained sample is placed in a 110℃ oven to dry for 12h, calcined at 400℃ in a muffle furnace for 4h, and then reduced at 300℃ in a H2 atmosphere for 4h to obtain a catalyst precursor with a Cu loading of 10wt.%.

[0056] Preparation of copper-silver bimetallic catalyst:

[0057] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for 4 hours for reduction. 0.4 g of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0058] Add a certain volume of ethanol to a three-necked flask, connect the flask to a Schlenk line and flush it with nitrogen at room temperature to remove the air in the system. Then add 4g of the reduced catalyst precursor, 10g / L of phenylalanine (sufficient amount of complexing agent), and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu:Ag=1:1), avoid light, stir and mix for 90 minutes, filter and wash the mixed solution with deionized water, and finally dry the obtained sample in an oven at 110℃ for 12 hours (vacuum drying) to obtain the catalyst.

[0059] The catalyst of this comparative example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 5.5%, and during the period from 270 h to 500 h, the yield decreased from 91.7% to 88.7%.

[0060] Example 2

[0061] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, adding complexing agent tyrosine, displacement method, copper-silver mass ratio 1:1)

[0062] This example is the preparation of copper-silver bimetallic catalyst sample 2, which is different from the preparation of copper-silver bimetallic catalyst sample 1 in Example 1 in that tyrosine is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0063] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0064] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, 10 g / L of tyrosine was added, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain a catalyst.

[0065] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0066] Example 3

[0067] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, added with complexing agent L-histidine, displacement method, copper-silver mass ratio 1:1)

[0068] This example is the preparation of copper-silver bimetallic catalyst sample 3, which is different from the preparation of copper-silver bimetallic catalyst sample 2 in Example 2 in that L-histidine is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0069] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0070] Add a certain volume of ethanol to a three-necked flask, connect the flask to a Schlenk line and flush it with nitrogen at room temperature to remove the air in the system. Then add a certain amount of reduced catalyst precursor, 10 g / L L-histidine, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1), pay attention to avoid light, stir and mix for 90 minutes, filter and wash the mixed solution with deionized water, and finally place the obtained sample in a 110°C oven to dry for 12 hours to obtain the catalyst.

[0071] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0072] Example 4

[0073] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, added complexing agent gelatin, replacement method, copper-silver mass ratio 1:1)

[0074] This example is the preparation of copper-silver bimetallic catalyst sample 4, which is different from the preparation of copper-silver bimetallic catalyst sample 3 in Example 3 in that gelatin is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0075] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0076] Add a certain volume of ethanol to a three-necked flask, connect the flask to a Schlenk line and flush it with nitrogen at room temperature to remove the air in the system. Then add a certain amount of reduced catalyst precursor, 10 g / L gelatin, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1), avoid light, stir and mix for 90 minutes, filter and wash the mixed solution with deionized water, and finally dry the obtained sample in an oven at 110°C for 12 hours to obtain the catalyst.

[0077] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0078] Example 5

[0079] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, added complexing agent PVP, replacement method, copper-silver mass ratio 1:1)

[0080] This example is the preparation of copper-silver bimetallic catalyst sample 5, which is different from the preparation of copper-silver bimetallic catalyst sample 4 in Example 4 in that PVP is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0081] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0082] Add a certain volume of ethanol to a three-necked flask, connect the flask to a Schlenk line and flush it with nitrogen at room temperature to remove the air in the system. Then add a certain amount of reduced catalyst precursor, 10 g / L PVP, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1), avoid light, stir and mix for 90 minutes, filter and wash the mixed solution with deionized water, and finally dry the obtained sample in an oven at 110°C for 12 hours to obtain the catalyst.

[0083] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0084] Example 6

[0085] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, added complexing agent glycine, displacement method, copper-silver mass ratio 1:1)

[0086] This example is the preparation of copper-silver bimetallic catalyst sample 6, which is different from the preparation of copper-silver bimetallic catalyst sample 5 in Example 5 in that glycine is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0087] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0088] Add a certain volume of ethanol to a three-necked flask, connect the flask to a Schlenk line and flush it with nitrogen at room temperature to remove the air in the system. Then add a certain amount of reduced catalyst precursor, 10 g / L glycine, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1), avoid light, stir and mix for 90 minutes, filter and wash the mixed solution with deionized water, and finally dry the obtained sample in an oven at 110°C for 12 hours to obtain the catalyst.

[0089] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0090] Example 7

[0091] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, added with complexing agent dl-malic acid, displacement method, copper-silver mass ratio 1:1)

[0092] This example is the preparation of copper-silver bimetallic catalyst sample 7, which is different from the preparation of copper-silver bimetallic catalyst sample 6 in Example 6 in that dl-malic acid is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0093] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0094] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, 10 g / L of dl-malic acid was added, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain a catalyst.

[0095] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0096] Example 8

[0097] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, adding complexing agent citric acid, displacement method, copper-silver mass ratio 1:1)

[0098] This example is the preparation of copper-silver bimetallic catalyst sample 8, which is different from the preparation of copper-silver bimetallic catalyst sample 7 in Example 7 in that citric acid is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example, and potassium carbonate is added to adjust the solution pH to 8. The preparation process is as follows:

[0099] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0100] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, 10 g / L of citric acid was added, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain a catalyst.

[0101] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0102] Example 9

[0103] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, adding complexing agent tannic acid, displacement method, copper-silver mass ratio 1:1)

[0104] This example is the preparation of copper-silver bimetallic catalyst sample 9, which is different from the preparation of copper-silver bimetallic catalyst sample 8 in Example 8 in that tannic acid is added as a complexing agent during the preparation of the copper-silver bimetallic catalyst prepared in this example. The preparation process is as follows:

[0105] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours, and a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.

[0106] Add a certain volume of ethanol to a three-necked flask, connect the flask to a Schlenk line and flush with nitrogen at room temperature to remove the air in the system. Then add a certain amount of reduced catalyst precursor, 10 g / L tannic acid, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1: 1), avoid light, stir and mix for 90 minutes, filter and wash the mixed solution with deionized water, and finally dry the obtained sample in an oven at 110°C for 12 hours to obtain the catalyst.

[0107] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0108] Examples 10-13

[0109] The copper-silver bimetallic catalyst (synthesized at 25°C, with the addition of chelating agent tannic acid, replacement method, copper-silver mass ratio of 1:1) was prepared. The effects of different pH on the copper-silver bimetallic catalyst and its effect on the catalytic activity were investigated.

[0110] Compared with Example 9, the only difference is that the solution pH is 9, 10, 11, and 12 respectively.

[0111] Catalysts of Examples 10-13 were subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0112] Embodiment 14, 15

[0113] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, adding complexing agent glycine, displacement method)

[0114] The effects of different copper-silver mass ratios on copper-silver bimetallic catalysts and their effects on catalyst activity were investigated.

[0115] Compared with Example 6, the only difference is that the ratio of Cu:Ag is 2:1 and 1:2 respectively.

[0116] The catalysts of Examples 14 and 15 were subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 1.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0117] Example 16

[0118] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, adding complexing agent phenylalanine, displacement method, copper-silver mass ratio 1:1)

[0119] The effects of high temperature and high space velocity on the selectivity of copper-silver bimetallic catalysts were investigated.

[0120] Compared with Example 1, the reaction conditions were changed to 225°C, 2.0 h -1 .

[0121] Example 16 The catalyst was subjected to the above-mentioned online reduction conditions and catalyst evaluation method at 225°C for 2.0 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values ​​are shown in Table 2.

[0122] From Comparative Examples 1 and 2, it can be seen that the catalyst in Comparative Example 1 was synthesized by the co-impregnation method at room temperature, and the yield was only 49.7%. In Comparative Example 2, the activity of the catalyst prepared by the replacement method was increased, and the MG yield was increased to 53.6. Therefore, the replacement method was used in the preparation of the copper-silver bimetallic catalyst, which can make the copper species and the silver species better anchored through strong interactions, enhance the catalyst activity, improve the directional selectivity of methyl glycolate, enhance the stability of the catalyst, and reduce the catalyst replacement cost in industrial applications.

[0123] From Comparative Example 2 and Example 1, it can be seen that the catalyst in Comparative Example 2 was synthesized at room temperature and no complexing agent was used, so the catalyst activity was low, but the selectivity was only 62.1% and the yield was only 53.6%. In Example 1, the addition of the complexing agent increased the catalyst activity, the selectivity was increased to 98.7%, the MG yield was increased to more than 90%, and the space-time yield was increased from 5.1 g·g cat -1 ·h -1 Increased to 9.3 g·g cat -1 ·h -1 . . Therefore, the introduction of a complexing agent in the preparation process of the copper-silver bimetallic catalyst enhances the catalyst activity, improves the directional selectivity of methyl glycolate, enhances the stability of the catalyst, and reduces the cost of catalyst replacement in industrial applications.

[0124] It can be seen from Examples 1-9 that different complexing agents were added during the preparation process. Under the action of different complexing agents, the catalyst selectivity and MG yield changed, so different complexing agents have different effects on the synthesis of copper-silver bimetallic catalysts.

[0125] It can be seen from Comparative Examples 2 and 3 that the synthesis temperature was changed during the preparation process of Comparative Examples 2 and 3, and the MG yield and space-time yield of the catalysts prepared therefrom under the reaction conditions were also different, indicating that the synthesis temperature has an effect on the preparation of the copper-silver bimetallic catalyst.

[0126] It can be seen from Examples 9-13 that the pH of the copper-silver bimetallic catalysts in Examples 9-13 changed during the preparation process, and the MG yield and space-time yield of the prepared catalysts under the reaction conditions were also different, indicating that pH has an effect on the preparation of the copper-silver bimetallic catalysts.

[0127] It can be seen from Example 6 and Examples 14 and 15 that the copper-silver mass ratio of the copper-silver bimetallic catalysts in Examples 4 and Examples 14 and 15 changed during the preparation process, and the MG yield and time-space yield of the prepared catalysts under the reaction conditions were also different, indicating that the copper-silver mass ratio has an effect on the preparation of the copper-silver bimetallic catalyst.

[0128] Table 1 Preparation conditions and particle size of each catalyst

[0129]

[0130] Table 2 Activity data of various catalysts for heterogeneous hydrogenation of dimethyl oxalate

[0131]

[0132] By Examples 1-9 in Table 1-2 and Figure 1 It can be seen that phenylalanine has the best effect as a complexing agent. This is because phenylalanine itself contains amino and hydroxyl groups that can form bonds with Ag and anchor Ag species. In addition, the amino and hydroxyl structures of phenylalanine itself are located in the side chain, avoiding the ring structure of the complexing agent itself and avoiding the aggregation of some molecules. Therefore, phenylalanine has a better effect as a complexing agent.

[0133] It can be seen from Examples 9-13 in Table 1-2 that pH=11 has the best effect during the preparation process. This is because weak alkalinity can promote the reduction of silver ions, and when the pH is about 11, more functional groups such as hydroxyl or carbonyl can form bonds with Ag and interact with each other, while when the alkalinity is higher, it is easy to cause some negative silver ions to precipitate, so pH=11 has the best effect.

[0134] By Example 6 and Examples 14, 15 in Table 1-2 and Figure 2 It can be seen that during the preparation process, Cu:Ag=1:1 has the best effect. This is because when the Ag content is low, all the metal Cu species cannot be coated by Ag, resulting in a low catalytic selectivity of the catalyst. When the Ag content is high, the Ag species agglomerate during the replacement process, the Ag nanoparticles grow, and Cu cannot be coated by Ag. Therefore, Cu:Ag=1:1 has the best effect.

[0135] By comparing Example 1 with Example 16, the catalyst has higher selectivity for MG and better space-time yield at high space velocity and high reaction temperature. This is because the high space velocity and high reaction temperature can make the DMO hydrogenation process of the catalyst stay at the stage of generating MG, thereby inhibiting the deep hydrogenation process.

[0136] By comparing the comparative examples 1 and 2 with the examples 1 to 9 in Table 1-2 and Figure 3 It can be seen that the introduction of a complexing agent during the catalyst synthesis process can enhance the catalyst activity and stability.

[0137] The catalyst prepared by adding a complexing agent in the present invention has the characteristics of mild conditions, simple preparation process, easy-to-obtain raw materials, low cost, excellent catalytic performance, etc. When actually applied to industry, it can be used alone for the production of methyl glycolate with high economic value and high demand, and can still maintain a methyl glycolate yield of more than 90% at a relatively high space velocity. In addition, the stability of the catalyst is greatly improved, the life of the catalyst is greatly increased, the loss caused by industrial catalyst replacement is reduced, and its industrialization cost is reduced.

Claims

1. A catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating it to prepare methyl glycolate, the catalyst being a copper-silver bimetallic catalyst, Features: The catalyst comprises a carrier and an active component, wherein the active component is a copper species and a silver species, and the carrier is silicon dioxide; the silver species accounts for 1-10 wt.% of the total mass of the catalyst, and the copper species accounts for 1-10 wt.% of the total mass of the catalyst; Firstly, a copper-containing catalyst precursor is prepared, and then the copper-containing catalyst precursor, a silver salt and a complexing agent are mixed and treated to obtain a finished catalyst product.

2. A catalyst with a complexing agent added for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 1, Features: The specific surface area of ​​the catalyst is 50-300m 2 / g, average pore volume is 0.4-1.7cm 3 / g, and the average pore size is 5-30nm.

3. A catalyst with added complexing agent for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 2, Features: The structure of the catalyst is that the silver species covers the surface of the copper species in the form of a shell layer to form a core-shell structure. The preferred solution is: The core-shell structure is deposited on the carrier silica in the form of particles, wherein copper forms a strong interaction with silica.

4. A catalyst with added complexing agent for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 3, Features: The particle size of the copper-silver bimetal is 1.0-10 nm, and the thickness of the silver shell layer is 0.2-2 nm. The preferred solution is: The particle size of the copper-silver bimetal is 1.0-8 nm, and the thickness of the silver shell is 0.2-1 nm.

5. A method for preparing a catalyst with a complexing agent added for preparing methyl glycolate by hydrogenation of dimethyl oxalate as claimed in claim 1, 2, 3 or 4, Features: It includes the following steps: Dissolve copper salt in water, add ammonia water, stir evenly and then drop silica sol; After aging treatment, the temperature is raised to evaporate ammonia, and after completion, it is filtered and washed; The washed product is dried and then calcined to obtain a catalyst precursor, which is then subjected to reduction treatment; The catalyst precursor, silver salt, ethanol and complexing agent are mixed, the pH value is adjusted, the copper and silver particles are extracted after centrifugation, and the finished catalyst is obtained after washing and drying.

6. A method for preparing a catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating it to prepare methyl glycolate according to claim 5, Features: The aging treatment time is 4 hours, and the temperature of the ammonia evaporation is 80 degrees Celsius.

7. A method for preparing a catalyst with a complexing agent added for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 5, Features: The drying conditions of the washed product are: temperature of 80-130 degrees Celsius, and drying time of 12-24 hours.

8. A method for preparing a catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating it to prepare methyl glycolate according to claim 5, Features: The temperature after the catalyst precursor, silver salt, ethanol and complexing agent are mixed is room temperature.

9. A method for preparing a catalyst with a complexing agent added for preparing methyl glycolate by hydrogenation of dimethyl oxalate according to claim 5, 6, 7 or 8, Features: The copper salt is copper nitrate. The optimized solution is: The complexing agent is any one of phenylalanine, tyrosine, L-histidine, gelatin, polyvinyl pyrrolidone, glycine, dl-malic acid, citric acid or tannic acid. The preferred solution is: The mass ratio of copper to silver is any one of 1:1, 2:1 or 1:

2. The preferred solution is: Adjust pH to slightly alkaline.

10. Use of a catalyst with a complexing agent added for preparing methyl glycolate by hydrogenation of dimethyl oxalate as claimed in claim 1, 2, 3 or 4, Features: The catalyst is used for catalyzing the selective hydrogenation of dimethyl oxalate to produce methyl glycolate; Specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst to react; The reaction pressure is 0.5-3.5MPa; the reaction temperature is 180-240℃; the mass space velocity of dimethyl oxalate is 0.1-4.0h -1 ; The hydrogen ester molar ratio is 60-150. The preferred solution is: An application of a catalyst obtained by the method for preparing a catalyst with a complexing agent added for synthesizing dimethyl oxalate and hydrogenating methyl glycolate as claimed in claim 9, Features: The catalyst is used for catalyzing the selective hydrogenation of dimethyl oxalate to produce methyl glycolate; Specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst to react; The reaction pressure is 0.5-3.5MPa; the reaction temperature is 180-240℃; the mass space velocity of dimethyl oxalate is 0.1-4.0h -1 ; The hydrogen ester molar ratio is 60-150.

Citation Information

Patent Citations

  • Catalyzer for oxalic ester hydrogenation synthesizing of glycolate and method of preparing the same

    CN101138730A

  • Catalyst for use in synthesis process of methyl glycolate as well as preparation method and application of catalyst

    CN108499564A

  • Multi-metal core-shell structure nano material based on multiple complexing agents and preparation method of multi-metal core-shell structure nano material

    CN114789248A

  • Preparation method and application of dimethyl oxalate selective hydrogenation catalyst

    CN115007172A

  • Silver-based catalyst and preparation method and application thereof

    CN116603525A