Composite oxide catalyst for decomposing ammonia by plasma and preparation method of composite oxide catalyst

By using a composite oxide catalyst of cobalt oxide and cerium oxide in the plasma ammonia decomposition reaction, the problems of high energy consumption and carbon emissions in the traditional ammonia decomposition hydrogen production reaction are solved, and an efficient ammonia decomposition reaction at low temperature and normal pressure is achieved. , has broad application prospects.

CN118807776APending Publication Date: 2024-10-22HEFEI UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410790877.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The traditional ammonia decomposition hydrogen production reaction consumes high energy and emits a lot of carbon emissions. It is difficult to achieve efficient ammonia decomposition at low temperature and normal pressure with existing technology.

Method used

A composite oxide catalyst that uses plasma to decompose ammonia. The general formula of the catalyst is xM·yA·(1-x-y)ComCe1-mOn. It contains a composite oxide solid solution carrier of cobalt oxide and cerium oxide and a noble metal or transition metal as an active component. Catalysts with high activity and stability are prepared through specific preparation methods.

Benefits of technology

In a non-thermal plasma environment, the activity and stability of the ammonia decomposition hydrogen production reaction are significantly improved, energy loss is reduced, the process route is simplified, and an efficient ammonia decomposition reaction is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807776A_ABST
    Figure CN118807776A_ABST
Patent Text Reader

Abstract

The invention discloses a composite oxide catalyst for decomposing ammonia by plasma and a preparation method thereof, and belongs to the technical field of catalysts and preparation thereof, the composite oxide catalyst comprises an auxiliary agent, an active component and a carrier, the structural general formula of the composite oxide catalyst can be represented by xM. YA. (1-x-y) ComCe1-mOn, M is the active component, A is the active auxiliary agent, and m is a positive integer. And ComCe1-mOn is a composite oxide solid solution carrier of cobalt oxide and cerium oxide. According to the composite oxide catalyst for decomposing ammonia through plasma and the preparation method of the composite oxide catalyst, the prepared catalyst shows relatively high activity and stability in a reaction for producing hydrogen through ammonia decomposition in a non-thermal plasma environment, the energy loss in the traditional ammonia decomposition process is reduced, the process route is simplified, and the production cost is reduced. Wide application prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts and their preparation, in particular to a composite oxide catalyst for plasma decomposition of ammonia and a preparation method thereof. Background Art

[0002] The proportion of new energy in the entire energy system is increasing rapidly. As an efficient and clean green energy carrier, hydrogen has attracted much attention due to its advantages such as transportability, long-term storage and high energy density. Among them, hydrogen production by decomposition of ammonia is simple in process and does not produce CO. X These advantages have begun to attract widespread attention.

[0003] However, since the decomposition of ammonia to produce hydrogen (2NH3=N2+3H2) is an endothermic reaction, a high amount of heat is required to obtain sufficient products, resulting in a high energy consumption in the traditional ammonia decomposition reaction. In recent years, a variety of new technologies have been applied to the field of ammonia decomposition, including but not limited to electrochemistry, photochemistry and plasma technology. Among them, non-thermal plasma (NTP)-assisted ammonia decomposition can achieve the decomposition of ammonia to produce hydrogen at low temperature and normal pressure, greatly reducing the energy consumption in the reaction and reducing the carbon emissions generated in the process. Summary of the invention

[0004] The purpose of the present invention is to provide a composite oxide catalyst for plasma decomposition of ammonia and a preparation method thereof. The prepared composite oxide catalyst exhibits high activity and stability in the ammonia decomposition hydrogen production reaction in a non-thermal plasma environment, reduces the energy loss in the traditional ammonia decomposition process, simplifies its process route, and has broad application prospects.

[0005] To achieve the above object, the present invention provides a composite oxide catalyst for plasma decomposition of ammonia, wherein the catalyst has the general formula xM·yA·(1-xy)Co m Ce 1-m O n ,

[0006] Where M is the active component, A is the active auxiliary, Co m Ce 1-m O n It is a composite oxide solid solution carrier of cobalt oxide and cerium oxide, x and y are the mass percentages of M and A respectively, m is the weight proportion of cobalt in the composite oxide solid solution, n is the weight proportion of oxygen in the composite oxide solid solution, and 0.5%≤x≤40%, 0.05%≤y≤5%, 10%≤m≤65%, and the remaining weight is n.

[0007] Preferably, the active component M includes one or more metals and / or metal oxides selected from the group consisting of Rh, Ru, Pt, Pd, Ba, Al, Mn, Fe, Ni, Cu, Zn, and Mo.

[0008] Preferably, the Co m Ce 1-m O n The carrier comprises a composite oxide solid solution of cobalt oxide and cerium oxide, and its precursors are Co(NO3)2·6H2O and Ce(NO3)2·6H2O.

[0009] Preferably, the active auxiliary agent A includes one or more metals and / or metal oxides selected from La and Y, and the precursor of the active auxiliary agent is one selected from La(NO3)3 and Y(NO3)3.

[0010] The present invention provides a method for preparing a composite oxide catalyst for plasma decomposition of ammonia, comprising the following steps:

[0011] Step 1, preparing a cobalt-cerium aqueous solution by adding a cobalt precursor and a cerium precursor into deionized water, dissolving and mixing, and stirring;

[0012] Step 2: adding ammonia water to the cobalt-cerium aqueous solution to generate a precipitate, and filtering, washing, vacuum drying, crushing and heating in air the precipitate in sequence to prepare a cobalt-cerium composite oxide solid solution A;

[0013] Step 3: adding the precursor of the active component and the precursor of the auxiliary agent into deionized water to dissolve them, and adding the composite oxide solid solution A into the solution and stirring them, thereby preparing a solution B;

[0014] Step 4: adding ammonia water to solution B to generate a precipitate, and filtering and washing the precipitate to obtain solid C;

[0015] Step 5: Dry the solid C in a vacuum drying oven, crush it, and then reduce it in a H2 atmosphere to obtain a catalyst.

[0016] Preferably, the vacuum drying temperature in step 2 is 100-150° C., and the drying time is 5-14 hours.

[0017] Preferably, in step 2, the heating temperature in air is 400-800° C., and the heating time is 1-6 hours.

[0018] Preferably, in step 5, the vacuum drying temperature is 100-150° C., the drying time is 5-12 h, and the reduction temperature is 400-800° C. under H2 atmosphere, and the time is 1-8 h.

[0019] A catalyst that decomposes ammonia into nitrogen and hydrogen by effectively coupling with NTP comprises a noble metal represented by Ru or a transition metal represented by Fe or Ni as a catalyst active component, a rare earth metal represented by La as a catalyst promoter component, and a composite oxide solid solution containing cobalt oxide and cerium oxide as a catalyst carrier, so that compared with a conventional ammonia decomposition catalyst, the catalyst has a higher ammonia conversion rate at low temperature and normal pressure.

[0020] Therefore, the present invention adopts the above-mentioned composite oxide catalyst for plasma decomposition of ammonia and its preparation method. The prepared composite oxide catalyst shows high activity and stability in the ammonia decomposition and hydrogen production reaction in a non-thermal plasma environment, reduces the energy loss in the traditional ammonia decomposition process, simplifies its process route, and has broad application prospects.

[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a composite oxide catalyst for plasma decomposition of ammonia and an embodiment of a preparation method thereof. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0024] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0025] Example

[0026] The present invention provides a composite oxide catalyst for plasma decomposition of ammonia, the general formula of the catalyst is xM·yA·(1-xy)Co m Ce 1-m O n ,

[0027] Where M is the active component, A is the active auxiliary, Co m Ce 1-m O n It is a composite oxide solid solution carrier of cobalt oxide and cerium oxide, x and y are the mass percentages of M and A respectively, m is the weight proportion of cobalt in the composite oxide solid solution, n is the weight proportion of oxygen in the composite oxide solid solution, and 0.5%≤x≤40%, 0.05%≤y≤5%, 10%≤m≤65%, and the remaining weight is n.

[0028] The active component M includes one or more metals and / or metal oxides selected from Rh, Ru, Pt, Pd, Ba, Al, Mn, Fe, Ni, Cu, Zn, and Mo, and the precursor of the active component is one selected from Ru(NO3)3, Fe(NO3)3, Al(NO3)3, Ba(NO3)2, Ni(NO3)2, and Cu(NO3)2. These metals have good plasma activity and can enhance the adsorption capacity of the catalyst for NH3, thereby promoting the decomposition reaction of NH3.

[0029] Co m Ce 1-m O n The carrier includes a composite oxide solid solution of cobalt oxide and cerium oxide, and its precursors are Co(NO3)2·6H2O and Ce(NO3)2·6H2O. The cobalt metal can exist in the form of metal Co or Co3O4 while keeping its weight unchanged, that is, it can serve as a stable carrier material and promote the NH3 decomposition reaction. The cerium metal mainly exists in the form of CeO2, which can serve as a stable carrier material with a rich pore structure for the plasma-catalyzed NH3 decomposition reaction, and can also improve the dispersion of active components to further promote the NH3 decomposition reaction.

[0030] The active additive A includes one or more metals and / or metal oxides of La and Y. The precursor of the active additive is one of La(NO3)3 and Y(NO3)3. The active additive can enhance the dispersion of the active components on the carrier, thereby optimizing the overall performance of the catalyst and achieving the goal of high ammonia decomposition conversion rate under mild conditions.

[0031] like Figure 1 As shown, the present invention provides a method for preparing a composite oxide catalyst for plasma decomposition of ammonia, comprising the following steps:

[0032] Step 1, preparing a cobalt-cerium aqueous solution by adding a cobalt precursor and a cerium precursor into deionized water, dissolving and mixing, and stirring;

[0033] Step 2: A cobalt-cerium composite oxide solid solution A is prepared by dripping ammonia water into the cobalt-cerium aqueous solution to generate a precipitate, and filtering, washing, vacuum drying, crushing and heating the precipitate in the air. The vacuum drying temperature is 100-150° C., and the drying time is 5-14 hours. The heating temperature in the air is 400-800° C., and the heating time is 1-6 hours.

[0034] Step 3: adding the precursor of the active component and the precursor of the auxiliary agent into deionized water to dissolve them, and adding the composite oxide solid solution A into the solution and stirring them, thereby preparing a solution B;

[0035] Step 4: adding ammonia water to solution B to generate a precipitate, and filtering and washing the precipitate to obtain solid C;

[0036] Step 5: Dry the solid C in a vacuum drying oven, crush it, and then reduce it in a H2 atmosphere to obtain a catalyst. The vacuum drying temperature is 100-150°C, the drying time is 5-12h, and the reduction temperature in the H2 atmosphere is 400-800°C, and the time is 1-8h.

[0037] Embodiment 1

[0038] A method for preparing a composite oxide catalyst for plasma decomposition of ammonia comprises the following steps:

[0039] Ammonia water is added to a solution of cobalt salt and cerium salt mixed in proportion to obtain a composite oxide solid solution A, and then the oxide solid solution A is co-precipitated with active component salt M and active auxiliary salt A in deionized water to form solid C, which is dried and reduced to the target catalyst.

[0040] In this embodiment, the cobalt salt, cerium salt and active auxiliary salt A are all nitrates, namely, cobalt nitrate hexahydrate, cerium nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively, and the active component salt M is a chloride salt, namely, ruthenium chloride trihydrate. 3.24g of cobalt nitrate hexahydrate and 2.48g of cerium nitrate hexahydrate are added to 50mL of deionized water to dissolve and mix, and stirred to prepare a cobalt-cerium aqueous solution, and 0.6mol of ammonia water is dripped into the aqueous solution until the pH value of the solution reaches 9, at which time a precipitate has been generated. After filtering and washing the precipitate under a pressure of 0.05MPa until the pH value of the washing water is 7, it is placed in a vacuum drying oven, dried at a temperature of 100°C for 12h, and then crushed. And calcined at a temperature of 550°C for 2h in a H2 atmosphere to obtain a composite oxide solid solution A, whose molecular formula can be expressed as: Co 0.18 Ce 0.18 O 0.64 , at this time, it was weighed and found that its weight was 5.06g.

[0041] In order to load 5 wt% of the active component Ru and 0.5 wt% of the active auxiliary La, 0.66 g of ruthenium chloride trihydrate, 0.068 g of lanthanum nitrate hexahydrate and Co 0.18 Ce 0.18 O 0.64Add to 50mL deionized water to dissolve and mix to obtain solution B, and drop 0.6mol ammonia water into solution B until the pH value of the solution reaches 9, at which time a precipitate has been generated. The precipitate is filtered and washed at a pressure of 0.05MPa until the pH value of the washing water is 7 to obtain solid C, which is then placed in a vacuum drying oven, dried at a temperature of 110°C for 14h, crushed, and calcined at a temperature of 550°C for 3h in a H2 atmosphere to obtain the target composite metal oxide catalyst: 5wt%Ru / 0.5wt%La / Co 0.18 Ce 0.18 O 0.64 .

[0042] Embodiment 2

[0043] In this embodiment, the cobalt salt, cerium salt and active auxiliary salt A are all nitrates, namely, cobalt nitrate hexahydrate, cerium nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively, and the active component salt M is a chloride salt, namely, ruthenium chloride trihydrate. 5.72g of cobalt nitrate hexahydrate and 2.19g of cerium nitrate hexahydrate are added to 60mL of deionized water to dissolve and mix, and stirred to prepare a cobalt-cerium aqueous solution, and 0.6mol of ammonia water is dripped into the aqueous solution until the pH value of the solution reaches 9, at which time a precipitate has been generated. After filtering and washing the precipitate under a pressure of 0.05MPa until the pH value of the washing water is 7, it is placed in a vacuum drying oven, dried at a temperature of 100°C for 12h, and then crushed. And calcined at a temperature of 550°C for 2.5h in a H2 atmosphere to obtain a composite oxide solid solution A, whose molecular formula can be expressed as: Co 0.23 Ce 0.12 O 0.65 , at this time, it was weighed and found to weigh 6.96g.

[0044] In order to load 5 wt% of the active component Ru and 0.5 wt% of the active auxiliary La, 0.90 g of ruthenium chloride trihydrate, 0.093 g of lanthanum nitrate hexahydrate and Co 0.23 Ce 0.12 O 0.65 Add to 60mL deionized water to dissolve and mix to obtain solution B, and drop 0.6mol ammonia water into solution B until the pH value of the solution reaches 9, at which time a precipitate has been generated. The precipitate is filtered and washed at a pressure of 0.05MPa until the pH value of the washing water is 7 to obtain solid C, which is then placed in a vacuum drying oven, dried at a temperature of 110°C for 14h, crushed, and calcined at a temperature of 550°C for 3h in a H2 atmosphere to obtain the target composite metal oxide catalyst: 5wt%Ru / 0.5wt%La / Co 0.23 Ce 0.12 O 0.65 .

[0045] Embodiment 3

[0046] In this embodiment, the cobalt salt, cerium salt and active auxiliary salt A are all nitrates, namely, cobalt nitrate hexahydrate, cerium nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively, and the active component salt M is a chloride salt, namely, ruthenium chloride trihydrate. 2.43g of cobalt nitrate hexahydrate and 3.72g of cerium nitrate hexahydrate are added to 50mL of deionized water to dissolve and mix, and stirred to prepare a cobalt-cerium aqueous solution, and 0.6mol of ammonia water is dripped into the aqueous solution until the pH value of the solution reaches 9, at which time a precipitate has been generated. After filtering and washing the precipitate under a pressure of 0.05MPa until the pH value of the washing water is 7, it is placed in a vacuum drying oven, dried at a temperature of 100°C for 12h, and then crushed. And calcined at a temperature of 550°C for 2h in a H2 atmosphere to obtain a composite oxide solid solution A, whose molecular formula can be expressed as: Co 0.13 Ce 0.26 O 0.61 , at this time, it was weighed and found that its weight was 5.45g.

[0047] In order to load 5 wt% of the active component Ru and 0.5 wt% of the active auxiliary La, 0.71 g of ruthenium chloride trihydrate, 0.073 g of lanthanum nitrate hexahydrate and Co 0.13 Ce 0.26 O 0.61 Add to 60mL deionized water to dissolve and mix to obtain solution B, and drop 0.6mol ammonia water into solution B until the pH value of the solution reaches 9, at which time a precipitate has been generated. The precipitate is filtered and washed at a pressure of 0.05MPa until the pH value of the washing water is 7 to obtain solid C, which is then placed in a vacuum drying oven, dried at a temperature of 110°C for 12h, crushed, and calcined at a temperature of 550°C for 3h in a H2 atmosphere to obtain the target composite metal oxide catalyst: 5wt%Ru / 0.5wt%La / Co 0.13 Ce 0.26 O 0.61 .

[0048] Embodiment 4

[0049] In this embodiment, the cobalt salt, cerium salt and active auxiliary salt A are all nitrates, namely, cobalt nitrate hexahydrate, cerium nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively, and the active component salt M is a chloride salt, namely, ruthenium chloride trihydrate. 2.43g of cobalt nitrate hexahydrate and 3.72g of cerium nitrate hexahydrate are added to 50mL of deionized water to dissolve and mix, and stirred to prepare a cobalt-cerium aqueous solution, and 0.6mol of ammonia water is dripped into the aqueous solution until the pH value of the solution reaches 9, at which time a precipitate has been generated. After filtering and washing the precipitate under a pressure of 0.05MPa until the pH value of the washing water is 7, it is placed in a vacuum drying oven, dried at a temperature of 100°C for 12h, and then crushed. And calcined at a temperature of 550°C for 2h in a H2 atmosphere to obtain a composite oxide solid solution A, whose molecular formula can be expressed as: Co 0.13 Ce 0.26 O 0.61 , at this time, it was weighed and found that its weight was 5.45g.

[0050] In order to load 15 wt% of the active component Ru and 0.5 wt% of the active auxiliary La, 2.27 g of ruthenium chloride trihydrate, 0.073 g of lanthanum nitrate hexahydrate and Co 0.13 Ce 0.26 O 0.61 Add to 60mL deionized water to dissolve and mix to obtain solution B, and drop 0.6mol ammonia water into solution B until the pH value of the solution reaches 9, at which time a precipitate has been generated. The precipitate is filtered and washed at a pressure of 0.05MPa until the pH value of the washing water is 7 to obtain solid C, which is then placed in a vacuum drying oven, dried at a temperature of 110°C for 12h, crushed, and calcined at a temperature of 550°C for 3h in a H2 atmosphere to obtain the target composite metal oxide catalyst: 15wt%Ru / 0.5wt%La / Co 0.13 Ce 0.26 O 0.61 .

[0051] Embodiment 5

[0052] In this embodiment, the cobalt salt, cerium salt and active auxiliary salt A are all nitrates, namely, cobalt nitrate hexahydrate, cerium nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively, and the active component salt M is a chloride salt, namely, ruthenium chloride trihydrate. 2.43g of cobalt nitrate hexahydrate and 3.72g of cerium nitrate hexahydrate are added to 50mL of deionized water to dissolve and mix, and stirred to prepare a cobalt-cerium aqueous solution, and 0.6mol of ammonia water is dripped into the aqueous solution until the pH value of the solution reaches 9, at which time a precipitate has been generated. After filtering and washing the precipitate under a pressure of 0.05MPa until the pH value of the washing water is 7, it is placed in a vacuum drying oven, dried at a temperature of 100°C for 12h, and then crushed. And calcined at a temperature of 550°C for 2h in a H2 atmosphere to obtain a composite oxide solid solution A, whose molecular formula can be expressed as: Co0.13 Ce 0.26 O 0.61 , at this time, it was weighed and found that its weight was 5.45g.

[0053] In order to load 25 wt% of the active component Ru and 0.5 wt% of the active auxiliary La, 3.53 g of ruthenium chloride trihydrate, 0.073 g of lanthanum nitrate hexahydrate and Co 0.13 Ce 0.26 O 0.61 Add to 60mL deionized water to dissolve and mix to obtain solution B, and drop 0.6mol ammonia water into solution B until the pH value of the solution reaches 9, at which time a precipitate has been generated. The precipitate is filtered and washed at a pressure of 0.05MPa until the pH value of the washing water is 7 to obtain solid C, which is then placed in a vacuum drying oven, dried at a temperature of 110°C for 12h, crushed, and calcined at a temperature of 550°C for 3h in a H2 atmosphere to obtain the target composite metal oxide catalyst: 25wt%Ru / 0.5wt%La / Co 0.13 Ce 0.26 O 0.61 .

[0054] In order to test the effect of the prepared composite oxide catalyst, the ammonia decomposition reaction was tested in a plasma environment, with the main reference being the ammonia conversion rate. 2g of catalyst was taken into a quartz tube with an outer diameter of 9mm, an inner diameter of 6mm, and a length of 400mm, fixed with quartz wool, a tungsten needle as the inner electrode connected to the high voltage pole of the power supply, and a copper mesh as the outer electrode connected to the low voltage pole of the power supply. In this experiment, the discharge power was 10-30W, the frequency was 9.5kHz, and the flow rate was 50mLmin -1 Ammonia gas with a concentration of 75% was introduced at a flow rate of , and the reaction results of Examples 1 to 5 under normal temperature and pressure conditions are shown in Table 1:

[0055] Table 1 Conversion rate of plasma catalytic ammonia decomposition experiment

[0056]

[0057] From the above data, it can be seen that the prepared composite oxide catalyst for plasma-catalyzed ammonia decomposition achieves a high conversion rate of plasma-catalyzed ammonia decomposition at normal temperature and pressure, and can be applied to other plasma-catalyzed reactions, with broad prospects.

[0058] Therefore, the present invention adopts the above-mentioned composite oxide catalyst for plasma decomposition of ammonia and its preparation method. The prepared composite oxide catalyst shows high activity and stability in the ammonia decomposition and hydrogen production reaction in a non-thermal plasma environment, reduces the energy loss in the traditional ammonia decomposition process, simplifies its process route, and has broad application prospects.

[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A composite oxide catalyst for plasma decomposition of ammonia, characterized in that: The catalyst has the general formula xM·yA·(1-xy)Co m Ce 1-m O n , Where M is the active component, A is the active auxiliary, Co m Ce 1-m O n It is a composite oxide solid solution carrier of cobalt oxide and cerium oxide, x and y are the mass percentages of M and A respectively, m is the weight proportion of cobalt in the composite oxide solid solution, n is the weight proportion of oxygen in the composite oxide solid solution, and 0.5%≤x≤40%, 0.05%≤y≤5%, 10%≤m≤65%, and the remaining weight is n.

2. The composite oxide catalyst for plasma decomposition of ammonia according to claim 1, characterized in that: The active component M includes one or more metals and / or metal oxides selected from the group consisting of Rh, Ru, Pt, Pd, Ba, Al, Mn, Fe, Ni, Cu, Zn, and Mo.

3. The composite oxide catalyst for plasma decomposition of ammonia according to claim 1, characterized in that: The Co m Ce 1-m O n The carrier includes a composite oxide solid solution of cobalt oxide and cerium oxide, the precursor of which is Co(NO3) 2· 6H2O and Ce(NO3) 2· 6H2O.

4. The composite oxide catalyst for plasma decomposition of ammonia according to claim 1, characterized in that: The active auxiliary agent A includes one or more metals and / or metal oxides selected from La and Y, and the precursor of the active auxiliary agent is one of La(NO3)3 and Y(NO3)3.

5. A method for preparing a composite oxide catalyst for plasma decomposition of ammonia according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1, preparing a cobalt-cerium aqueous solution by adding a cobalt precursor and a cerium precursor into deionized water, dissolving and mixing, and stirring; Step 2: adding ammonia water to the cobalt-cerium aqueous solution to generate a precipitate, and filtering, washing, vacuum drying, crushing and heating in air the precipitate in sequence to prepare a cobalt-cerium composite oxide solid solution A; Step 3: adding the precursor of the active component and the precursor of the auxiliary agent into deionized water to dissolve them, and adding the composite oxide solid solution A into the solution and stirring them, thereby preparing a solution B; Step 4: adding ammonia water to solution B to generate a precipitate, and filtering and washing the precipitate to obtain solid C; Step 5: Dry the solid C in a vacuum drying oven, crush it, and then reduce it in a H2 atmosphere to obtain a catalyst.

6. The method for preparing a composite oxide catalyst for plasma decomposition of ammonia according to claim 5, characterized in that: The vacuum drying temperature in step 2 is 100-150° C., and the drying time is 5-14 hours.

7. The method for preparing a composite oxide catalyst for plasma decomposition of ammonia according to claim 5, characterized in that: In the step 2, the heating temperature in the air is 400-800° C., and the heating time is 1-6 hours.

8. The method for preparing a composite oxide catalyst for plasma decomposition of ammonia according to claim 5, characterized in that: In the step 5, the vacuum drying temperature is 100-150° C., the drying time is 5-12 h, and the reduction temperature is 400-800° C. under H2 atmosphere, and the time is 1-8 h.

Citation Information

Patent Citations

  • Copper-based cerium-cobalt-lanthanum composite oxide catalyst and preparation method thereof

    CN103230803A

  • Preparation method of composite molecular sieve catalyst for diesel-car tail gas

    CN105478158A

  • Nanogold catalyst for ester generation by one-step oxidative esterification of aldehyde and alcohol and its preparation method and application

    CN107899575A

  • Mn-La-Ce catalyst for selective catalytic reduction of NO and application of Mn-La-Ce catalyst

    CN108435238A

  • Ammonia decomposition catalyst and preparation method and application thereof

    CN110270340A