Preparation method of needle-leaf-shaped high-low heterojunction photocatalyst
By combining Al-STO and ZnxCd1-xS through a solvothermal method, a needle-like high-low heterojunction nanocomposite is constructed, which solves the problems of easy recombination of photogenerated electrons and holes and insufficient active sites of a single Al-STO photocatalyst, significantly improving Improved photocatalytic efficiency and hydrogen production activity, suitable for solar energy and photocatalytic applications.
Patent Information
- Application Number
- CN202410885503.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-22
AI Technical Summary
The single-component strontium titanate (Al-STO) photocatalyst has the problem that photogenerated electrons and holes are easy to recombine and the reaction active sites are insufficient, which limits its photocatalytic efficiency.
Al-STO is composited with ZnxCd1-xS, which has a narrow band gap and high photocatalytic activity, through a solvothermal method to construct a needle-shaped Al-STO/ZnxCd1-xSⅠ type high-low heterojunction nanocomposite to increase photogenerated carriers. Composite and migration capabilities.
It significantly improves the visible light absorption capacity and redox activity of the photocatalyst, enhances the carrier separation efficiency and hydrogen production activity, and is suitable for solar energy and photocatalytic hydrogen production applications.
Smart Images

Figure CN118807782A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar energy and photocatalytic hydrogen production, and in particular to a method for preparing a needle-shaped high-low heterojunction photocatalyst. Background Art
[0002] Strontium titanate (hereinafter referred to as STO) is a perovskite oxide with the characteristics of an n-type semiconductor, a wide bandgap and excellent electronic properties. However, STO can only absorb ultraviolet light, which limits its photocatalytic water splitting quantum efficiency. According to previous studies, the doping valence state is lower than that of Ti 4+ Cations such as Mg 2+ , Ga 3+ and Al 3+ , which can avoid Ti 3+ The introduction of defects, and Ti 3+ Defects are recombination centers for photogenerated charges, and doping with external elements can also introduce intermediate states within the band gap of STO, thereby enhancing its visible light absorption. Currently, a variety of methods have been successfully used to prepare Al-STO nanomaterials, and there are a large number of research reports on the production or degradation of various pollutants by Al-STO materials. However, the photocatalytic effect of a single component is always restricted by factors such as the high degree of recombination of photogenerated carriers and the lack of active sites for redox reactions.
[0003] The addition of Zn not only reduces the toxicity of Cd, but also x Cd 1-x S solid solution has good photocatalytic performance and stability. x Cd 1-x S solid solution has some unique advantages compared with single metal sulfide photocatalysts, but Zn x Cd 1-x S solid solution still has the disadvantages of few reactive sites and high carrier recombination rate. The construction of heterojunction, especially type I high-low heterojunction, has a strong inhibitory effect on the recombination of photogenerated carriers in photocatalysts and can significantly improve their spatial separation and migration capabilities. Therefore, in order to solve the problems of easy recombination of photogenerated electrons and holes and insufficient active sites in the single photocatalytic material Al-STO, Zn with a narrow band gap and high photocatalytic activity is used. x Cd 1-x The composite of S and Al-STO to improve the carrier separation efficiency and redox activity is an effective strategy to improve the photocatalytic efficiency. x Cd 1-x The process of using SⅠ type high-low heterojunction nanocomposites for photocatalytic hydrogen production has not been reported. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a needle-shaped high-low heterojunction photocatalyst.
[0005] The invention provides a method for preparing a needle-shaped high-low heterojunction photocatalyst, wherein Al-STO and Zn are prepared by a solvent thermal method. x Cd 1-x S was compounded to obtain Al-STO / Zn with tight interface bonding, strong visible light response ability, good stability and type I high-low heterojunction characteristics. x Cd 1-x S nanocomposite photocatalyst, the preparation method thereof is as follows:
[0006] Step 1: Take a certain amount of Ti(C4H9O)4 and an appropriate amount of ethylene glycol and mix and stir until a clear solution is obtained;
[0007] Step 2: Take a certain amount of Sr(NO3)2 and Al(NO3)3·9H2O and dissolve them in an appropriate amount of deionized water, then add them dropwise to the solution obtained in step 1, then add a certain amount of NaOH solution, and continue stirring for 0.5-24h;
[0008] Step 3: The stirred solution is transferred into a hydrothermal reactor and kept at a certain temperature for 6-48 hours, then the product is washed with deionized water until neutral, and vacuum dried at a certain temperature for 6-36 hours to obtain Al-STO;
[0009] Step 4: Dissolve a certain amount of Zn(NO3)2 and CdSO4 in an appropriate amount of deionized water, add a certain amount of thiourea, and continue stirring for 0.5-24h;
[0010] Step 5: Transfer the stirred solution into a hydrothermal reactor and keep it at a certain temperature for 6-36 hours. Then wash the product with deionized water until it is neutral, and vacuum dry it at a certain temperature for 6-36 hours to obtain Zn x Cd 1-x S;
[0011] Step 6: Take a certain amount of Zn(NO3)2 and CdSO4 and dissolve them in an appropriate amount of deionized water, add a certain amount of Al-STO powder obtained in step 3, and then add a certain amount of thiourea, and continue stirring for 0.5-24h;
[0012] Step 7: The stirred solution is transferred into a hydrothermal reactor and kept at a certain temperature for 6-48 hours. The product is then washed with deionized water until neutral and vacuum dried at a certain temperature for 6-36 hours to obtain Al-STO / Zn x Cd 1-x S nanocomposite materials.
[0013] Preferably, the mass of Ti(C4H9O)4 used in step 1 is 1-10 g, and the volume of ethylene glycol is 5-60 mL.
[0014] Preferably, the mass of Sr(NO3)2 used in step 2 is 0.5-10g, the mass of Al(NO3)3·9H2O is 1-30g, the volume of deionized water is 5-60mL, the concentration of NaOH solution is 1-10M, and the volume is 1-30mL.
[0015] Preferably, the temperature of the hydrothermal kettle in step 3 is 80-350°C; and the vacuum drying temperature is 40-100°C.
[0016] 5. The method for preparing a needle-shaped high-low heterojunction photocatalyst according to claim 1 is characterized in that the mass of Zn(NO3)2 used in step 4 is 0.1-10g, the mass of CdSO4 is 0.1-10g, the volume of deionized water is 5-200mL, and the mass of thiourea is 0.1-10g.
[0017] Preferably, in step 5, the temperature of the hydrothermal kettle is 80-300°C; and the vacuum drying temperature is 40-100°C.
[0018] Preferably, the mass of Zn(NO3)2 used in step six is 0.1-10g, the mass of CdSO4 is 0.1-10g, the volume of deionized water is 5-200mL, the mass of Al-STO powder is 0.1-5g, and the mass of thiourea is 0.1-10g.
[0019] Preferably, the temperature of the hydrothermal kettle in step seven is 80-350°C; and the vacuum drying temperature is 40-100°C.
[0020] Compared with the related art, the preparation method of the needle-shaped high-low heterojunction photocatalyst provided by the present invention has the following beneficial effects:
[0021] The present invention provides a method for preparing a needle-shaped high-low heterojunction photocatalyst:
[0022] Al-STO and Zn were synthesized by solvothermal method x Cd 1-x S was compounded to construct a needle-shaped Al-STO / Zn x Cd 1-x SⅠ type high-low heterojunction nanocomposite material significantly improves the Al-STO and Zn x Cd 1-x S has the ability to absorb light and successfully improved the separation and migration of photogenerated electrons and holes. The resulting needle-shaped Al-STO / Zn x Cd 1-xSⅠ-type high-low heterojunction nanocomposites have the advantages of strong visible light response, tight interface bonding, stable structure, high reduction potential and hydrogen production activity, and are expected to be applied in solar energy and photocatalytic hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is an XRD diagram of a sample prepared in an embodiment of a method for preparing a needle-shaped high-low heterojunction photocatalyst of the present invention;
[0024] Figure 2 The Al-STO / Zn prepared in the method for preparing a needle-shaped high-low heterojunction photocatalyst of the present invention x Cd 1-x TEM images of S composite materials at different magnifications;
[0025] Figure 3 This is a photocatalytic hydrogen production rate diagram of the sample obtained from an embodiment of the preparation method of a needle-shaped high-low heterojunction photocatalyst of the present invention. Figures (ab) show the change of hydrogen production rate with the value of x in ZnxCd1-xS when the molar ratio of Al-STO / ZnxCd1-xS is fixed at 20%; Figure (cd) shows the change of hydrogen production rate with the molar ratio of Al-STO / ZnxCd1-xS when x=0.6 in ZnxCd1-xS. DETAILED DESCRIPTION
[0026] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0027] Embodiment 1:
[0028] The present invention provides a method for preparing a needle-shaped high-low heterojunction photocatalyst, comprising the steps of:
[0029] (1) 1.05 g Sr(NO3)2 and 3.75 g Al(NO3)3·9H2O were taken as raw materials, dissolved in 10 mL deionized water, and added dropwise to a mixed solution of 1.7 g Ti(C4H9O)4 and 10 mL ethylene glycol, and then 5 mL 10 M NaOH solution was added. After continuous stirring for 12 h, the mixture was transferred into a hydrothermal reactor and kept at 180 °C for 30 h. The obtained product was washed with water until neutral and then vacuum dried at 50 °C for 18 h to obtain Al-STO;
[0030] (2) 0.38 g Zn(NO3)2 and 0.43 g CdSO4 were used as raw materials, dissolved in 20 mL deionized water, and then 0.38 g thiourea was added. After continuous stirring for 12 h, the mixture was transferred into a hydrothermal reactor and kept at 140 °C for 18 h. The obtained product was washed with water until neutral and then dried in vacuum at 50 °C for 18 h to obtain ZnxCd1-xS (where x = 0.4);
[0031] (3) 0.38 g Zn(NO3)2 and 0.43 g CdSO4 were used as raw materials and dissolved in 20 mL deionized water. 0.21 g Al-STO was added and 0.38 g thiourea was added. After continuous stirring for 12 h, the mixture was transferred into a hydrothermal reactor and kept at 180 °C for 30 h. The product was washed with water until neutral and then dried in vacuum at 50 °C for 18 h to obtain a needle-shaped SZ0.4-20Ⅰ type high-low heterojunction nanocomposite material (where 0.4 is the value of x in ZnxCd1-xS; 20 is the molar ratio of Al-STO / ZnxCd1-xS).
[0032] Embodiment 2:
[0033] The present invention provides a method for preparing a needle-shaped high-low heterojunction photocatalyst, comprising the steps of:
[0034] (1) Take 2.1g Sr(NO3)2 and 7.5g Al(NO3)3·9H2O as raw materials, dissolve them together in 20mL deionized water, add them dropwise to a mixed solution of 3.4g Ti(C4H9O)4 and 20mL ethylene glycol, then add 10mL 5M NaOH solution, continue stirring for 24h, move into a hydrothermal autoclave, keep warm at 200℃ for 24h, wash the obtained product with water until neutral, and then vacuum dry it at 60℃ for 12h to obtain Al-STO;
[0035] (2) 0.57 g Zn(NO3)2 and 0.29 g CdSO4 were used as raw materials, dissolved in 20 mL deionized water, and 0.38 g thiourea was added. After continuous stirring for 24 h, the mixture was transferred into a hydrothermal reactor and kept at 180 °C for 12 h. The obtained product was washed with water until neutral and then dried in vacuum at 60 °C for 12 h to obtain ZnxCd1-xS (where x = 0.6);
[0036] (3) 0.57 g Zn(NO3)2 and 0.29 g CdSO4 were used as raw materials and dissolved in 20 mL deionized water. 0.21 g Al-STO was added and 0.38 g thiourea was added. After continuous stirring for 24 h, the mixture was transferred into a hydrothermal reactor and kept at 200 °C for 24 h. The product was washed with water until neutral and then dried in vacuum at 60 °C for 12 h to obtain a needle-shaped SZ0.6-20Ⅰ type high-low heterojunction nanocomposite material (where 0.6 is the value of x in ZnxCd1-xS; 20 is the molar ratio of Al-STO / ZnxCd1-xS).
[0037] Embodiment 3:
[0038] The present invention provides a method for preparing a needle-shaped high-low heterojunction photocatalyst, comprising the steps of:
[0039] (1) 3.15 g Sr(NO3)2 and 11.25 g Al(NO3)3·9H2O were taken as raw materials, dissolved in 30 mL deionized water, and added dropwise to a mixed solution of 5.1 g Ti(C4H9O)4 and 30 mL ethylene glycol, and then 10 mL 10 M NaOH solution was added. After continuous stirring for 18 h, the mixture was transferred into a hydrothermal reactor and kept at 240 °C for 18 h. The obtained product was washed with water until neutral and then vacuum dried at 80 °C for 8 h to obtain Al-STO;
[0040] (2) 0.57 g Zn(NO3)2 and 0.29 g CdSO4 were used as raw materials, dissolved in 20 mL deionized water, and then 0.38 g thiourea was added. After continuous stirring for 18 h, the mixture was transferred into a hydrothermal reactor and kept at 220 °C for 10 h. The obtained product was washed with water until neutral and then dried in vacuum at 80 °C for 8 h to obtain ZnxCd1-xS (where x = 0.6);
[0041] (3) 0.57 g Zn(NO3)2 and 0.29 g CdSO4 were used as raw materials and dissolved in 20 mL deionized water. 0.315 g Al-STO was added and 0.38 g thiourea was added. After continuous stirring for 18 h, the mixture was transferred into a hydrothermal kettle and kept at 240 °C for 18 h. The product was washed with water until neutral and then dried in vacuum at 80 °C for 8 h to obtain a needle-shaped SZ0.6-30Ⅰ type high-low heterojunction nanocomposite material (where 0.6 is the value of x in ZnxCd1-xS; 30 is the molar ratio of Al-STO / ZnxCd1-xS).
[0042] Embodiment 4:
[0043] The photocatalytic performance test was carried out, and the photocatalytic overall water decomposition reaction was carried out on a photocatalytic hydrogen production system equipped with a gas circulation system. In detail, 50 mg of the sample was added to 100 ml of a mixed solution of 0.35 M Na2S and 0.25 M Na2SO3, ultrasonically dispersed for 30 minutes, and then transferred to a top radiation photoreactor. A 280 W xenon lamp was used as the light source. Before the measurement, the gas circulation system was evacuated to remove the air. During the test, the temperature of the cooling water circulation system was maintained at 5 ° C. The amount of hydrogen produced was detected by equipping a thermal conductivity detector and a gas chromatograph. The experiment was carried out for 3 hours, and the amount of hydrogen was measured every 0.5 hours.
[0044] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a needle-shaped high-low heterojunction photocatalyst, characterized in that: The steps include: Step 1: Take a certain amount of Ti(C4H9O)4 and an appropriate amount of ethylene glycol and mix and stir until a clear solution is obtained; Step 2: Take a certain amount of Sr(NO3)2 and Al(NO3)3·9H2O and dissolve them in an appropriate amount of deionized water, then add them dropwise to the solution obtained in step 1, then add a certain amount of NaOH solution, and continue stirring for 0.5-24h; Step 3: The stirred solution is transferred into a hydrothermal reactor and kept at a certain temperature for 6-48 hours, then the product is washed with deionized water until neutral, and vacuum dried at a certain temperature for 6-36 hours to obtain Al-STO; Step 4: Dissolve a certain amount of Zn(NO3)2 and CdSO4 in an appropriate amount of deionized water, add a certain amount of thiourea, and continue stirring for 0.5-24h; Step 5: Transfer the stirred solution into a hydrothermal reactor and keep it at a certain temperature for 6-36 hours. Then wash the product with deionized water until it is neutral, and vacuum dry it at a certain temperature for 6-36 hours to obtain Zn x Cd 1-x S; Step 6: Take a certain amount of Zn(NO3)2 and CdSO4 and dissolve them in an appropriate amount of deionized water, add a certain amount of Al-STO powder obtained in step 3, and then add a certain amount of thiourea, and continue stirring for 0.5-24h; Step 7: The stirred solution is transferred into a hydrothermal reactor and kept at a certain temperature for 6-48 hours. The product is then washed with deionized water until neutral and vacuum dried at a certain temperature for 6-36 hours to obtain Al-STO / Zn x Cd 1-x S nanocomposite materials.
2. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: The mass of Ti(C4H9O)4 used in step 1 is 1-10 g, and the volume of ethylene glycol is 5-60 mL.
3. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: The mass of Sr(NO3)2 used in step 2 is 0.5-10g, the mass of Al(NO3)3·9H2O is 1-30g, the volume of deionized water is 5-60mL, the concentration of NaOH solution is 1-10M, and the volume is 1-30mL.
4. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: In the step 3, the temperature of the hydrothermal kettle is 80-350°C; the vacuum drying temperature is 40-100°C.
5. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: The mass of Zn(NO3)2 used in step 4 is 0.1-10g, the mass of CdSO4 is 0.1-10g, the volume of deionized water is 5-200mL, and the mass of thiourea is 0.1-10g.
6. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: In the step 5, the temperature of the hydrothermal kettle is 80-300°C; the vacuum drying temperature is 40-100°C.
7. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: The mass of Zn(NO3)2 used in step 6 is 0.1-10g, the mass of CdSO4 is 0.1-10g, the volume of deionized water is 5-200mL, the mass of Al-STO powder is 0.1-5g, and the mass of thiourea is 0.1-10g.
8. The method for preparing the needle-shaped high-low heterojunction photocatalyst according to claim 1, characterized in that: In step seven, the temperature of the hydrothermal kettle is 80-350°C; the vacuum drying temperature is 40-100°C.
Citation Information
Patent Citations
ZnxCdl-xS / TiO2 nanometer photocatalytic material and preparation thereof
CN106391056A
Hollow ZnCdS loaded V-SrTiO3 microsphere heterojunction photocatalytic material and preparation method thereof
CN111437833A
M0 / SrTi1-xMYO3-delta as well as preparation method and application thereof
CN114632505A
Synthesis method of zinc-cadmium-sulfur nano-materials with different morphologies and photocatalytic hydrogen production application of zinc-cadmium-sulfur nano-materials
CN115193448A
Aluminum-doped strontium titanate loaded nickel sulfide photocatalytic composite material and preparation method thereof
CN117718059A
Cited By
Preparation method of CuPt-CSTO nano composite material
CN119140119A