Preparation method of adjustable bismuth-based multi-heterojunction photocatalytic material
By using molten salt medium and calcination treatment in the preparation of bismuth-based multi-heterojunction photocatalytic materials, a bismuth-based multi-heterojunction structure with rich active sites is formed, which solves the problem of low photocatalytic efficiency and material instability in the existing technology. problem, achieving efficient degradation of water pollutants and industrial application.
Patent Information
- Application Number
- CN202410828498.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-25
AI Technical Summary
Existing technology is difficult to effectively control heterostructures, resulting in low photocatalytic efficiency of bismuth silicate and bismuth oxychloride, unstable materials, and difficulty in expanding to industrial applications.
By calcining and treating materials such as Bi2O3, SiO2, K2CO3, and KCl under specific conditions, a controllable bismuth-based multi-heterojunction structure is formed. Molten salt is used to introduce displacement reactions and regulate the crystal phase ratio to generate a catalyst with rich active sites. .
It improves the activity and stability of the photocatalyst, reduces the reaction temperature and energy consumption, avoids agglomeration, achieves efficient degradation of organic pollutants in water, and is suitable for industrial production.
Smart Images

Figure CN118807790A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalysts, and in particular relates to a method for preparing a controllable bismuth-based multi-heterojunction photocatalytic material. Background Art
[0002] Bismuth silicate material is an extremely important photocatalytic composite material. It has excellent photogenerated carrier mobility and strong photogenerated hole anti-oxidation property. Bismuth oxychloride is a semiconductor material with a suitable band structure. Both have photocatalytic properties. In practical applications, the single sheet structure formed by bismuth silicate during the preparation process is too large and there will be serious layer-by-layer stacking. Bismuth oxychloride has problems such as large band gap width and insufficient stability, which greatly reduces their photocatalytic efficiency. Therefore, the composite structure formed with other materials is one of the means to improve the photocatalytic efficiency.
[0003] In the existing technology, it is still impossible to effectively control the heterogeneous structure, and the formed heterogeneous structure has problems such as instability and uncontrollable performance, which greatly limits the performance of photocatalysis to a certain extent. In addition, most of the existing technologies are still in the laboratory stage, and the prepared materials have many problems such as easy agglomeration, low yield, and long experimental cycle, which makes it impossible to expand to industrial applications. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of complex preparation and difficult process in the prior art, and to provide a method for preparing an adjustable bismuth-based multi-heterojunction photocatalytic material. The obtained catalyst material has many active sites, can improve the utilization rate of light, has high catalytic activity, and has good dispersibility. It can quickly degrade organic pollutants in water bodies. At the same time, the raw materials are easily available, the process is simple, and it can be prepared in a controllable manner, and it is expected to be put into industrial production.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a controllable bismuth-based multi-heterojunction photocatalytic material comprises the following steps:
[0007] Step 1: Get Bi 2 O 3 、SiO 2 and K 2 CO 3 , KCl are mixed and ground evenly; 2 O 3 With SiO 2 The amount of substance ratio is 1:1~9:1, K 2 CO 3 The molar ratio of KCl is 0.30:0.65~0.35:0.73, K2 CO 3 and KCl account for 35wt% to 45wt% of the total mixture;
[0008] Step 2, calcining the mixed and ground materials obtained in step 1 at 620° C. to 750° C. for 0.5 to 3 hours and then cooling;
[0009] Step 3, obtaining the controllable bismuth-based multi-heterojunction photocatalytic material by one of the following methods:
[0010] Method 1: Add water to the material obtained in step 2 and adjust the pH to 0.5-1.5, stir in a water bath, and centrifuge to dry.
[0011] Method 2: The material obtained in step 2 is washed alternately with water and alcohol for multiple times, and then dried; water is added and the pH is adjusted to 1-3, and salt is added, stirred in a water bath, and centrifuged to obtain the product.
[0012] In one embodiment, in step 1, the mixing is ball-milled for 3 hours to 8 hours.
[0013] In one embodiment, in step 1, K 2 CO 3 Combined with KCl to form a complex salt, expressed as K 2 CO 3 -KCl.
[0014] In one embodiment, in step 2, the heating rate is set to 5°C / min during calcination, and the calcination temperature is maintained for 0.5h to 3h after reaching the calcination temperature.
[0015] In one embodiment, the method 1 is to weigh 0.5 g to 3 g of the material obtained in step 2, add 80 mL to 150 mL of water, then add acid to adjust the pH to 0.5 to 1.5, stir for 10 min to 30 min, centrifuge 3 to 5 times, and the water bath conditions are: stirring at 30° C. for 10 min to 30 min.
[0016] In one embodiment, the method 2 is as follows: weigh 0.1 g to 0.35 g of the material obtained in step 2, wash it with water and alcohol alternately for multiple times, and then dry it; then add 30 mL to 50 mL of water, stir it for 1 h to 2 h, add acid to adjust the pH to 1 to 3, add 5 mL to 60 mL of a salt solution with a concentration of 1 g / L to 3 g / L, stir it for 10 min to 40 min, and then centrifuge it 3 to 5 times.
[0017] In one embodiment, the salt added in method 2 is NaCl, NaBr, LiCl and ZnCl 2 One or more of .
[0018] In one embodiment, in method 2, the water bath conditions are: stirring at 30° C. for 30 min to 40 min.
[0019] The adjustable bismuth-based multi-heterojunction photocatalytic material obtained by the preparation method of the adjustable bismuth-based multi-heterojunction photocatalytic material of the present invention can be used as a catalyst for sewage treatment, which achieves the purpose of purifying water quality by decomposing organic matter and pollutants in the water body.
[0020] A lot of industrial wastewater may be generated during industrial production, including a lot of organic dyes. The photocatalyst prepared by the present invention is directly added into the industrial wastewater to decompose organic matter and pollutants in the water through surface adsorption and oxidation, thereby reducing their pollution to the environment.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. In the present invention, molten salt (such as K 2 CO 3 -KCl) is added to form Bi 12 -X(X=Bi 2 -BiOCl, BiOCl) type II heterojunction structure, on the one hand, the heterojunction can effectively separate the photogenerated carriers, on the other hand, oxygen vacancies are generated in the process of introducing X to form a heterojunction, forming adsorbed oxygen. At the same time, by adding molten salt to undergo a replacement reaction, the crystallization process can be controlled, the proportion of the generated crystal phase can be precisely controlled, and the chemical reaction process can be controlled, the catalyst surface can be activated, and more active functional groups can be generated, making it easier to generate oxygen vacancies and adsorb oxygen.
[0023] 2. The molten salt introduced in the present invention can form bismuth oxyhalide with the generated bismuth base in the reaction, and in this process, the formation of the heterojunction is adjusted, the position of the valence band and conduction band of the catalyst is affected, the band gap width of the catalyst can be regulated, and the position of the catalyst band gap can be changed. The band gap width of the prepared bismuth silicate is significantly narrowed. After the introduction of bismuth oxychloride, the energy band gap of the catalyst is changed according to demand, the recombination rate of the photogenerated carriers of the catalyst is reduced, and defect energy levels are generated by the introduction of defects during the reaction process, which is easy for the transition and separation of photogenerated carriers.
[0024] 3. The method used in the present invention is simple. By adding molten salt, the reaction temperature can be effectively reduced, the particle size of the material can be reduced, the reaction can be easily controlled, and Bi can be effectively regulated. 2 、Bi 12 The crystal phase ratio can better react with the halogen in the molten salt, thereby improving the performance of the prepared material. The operation process is simple, which reduces the energy consumption problem in the reaction process and can be used in actual production.
[0025] 4. In the present invention, a multi-heterogeneous catalytic material is generated by the introduction of molten salt, the reaction temperature is low, the operation process is simple, the preparation cycle is moderate and the material cost is not high. The prepared catalytic material can improve its performance while ensuring the output, and is not easy to agglomerate, providing a new idea for realizing the transition from laboratory to industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the nanosheets stacked to form a flower shape after modification.
[0027] Figure 2 This is a photocatalytic degradation diagram of Rhodamine B prepared by the one-step and two-step methods respectively. DETAILED DESCRIPTION
[0028] The following is a detailed description of the implementation of the present invention in conjunction with the accompanying drawings and examples. The technical solution of the present invention is not limited to the specific implementations listed below, but also includes any combination of the specific methods.
[0029] A method for preparing a controllable bismuth-based multi-heterojunction photocatalytic material comprises the following steps:
[0030] Step 1: Bi the raw materials 2 O 3 and SiO 2 Weigh according to the molar ratio of 1:1 to 9:1, and select K 2 CO 3 , KCl are used as the salt used in the present invention, and 35wt% to 45wt% are weighed and mixed, and the powder material A is obtained by grinding evenly by ball milling for 3h to 5h.
[0031] In this step, Bi 2 O 3 and SiO 2 Weigh the corresponding mass and add 35wt% to 45wt% K 2 CO 3 Simple mixing and ball milling with KCl can evenly mix the molten salt and raw materials before firing.
[0032] Step 2: Weigh 3g to 5g of the above-mentioned uniformly ground powder material A, calcine it in a muffle furnace at 620℃ to 750℃, with a heating rate of 5℃ / min to 15℃ / min, and finally keep it warm for 0.5h to 3h. Take out the sample after the reaction is completed and cool it to obtain powder material B.
[0033] This step realizes the modification of the catalyst, so that the molten salt added in step one reacts with the raw material mixture, which changes the position of the catalyst valence band and conduction band, which is beneficial to the subsequent modification to adjust the band gap width of the powder.
[0034] Step 3: Use one of the following methods to prepare the final product.
[0035] Method 1: Weigh 0.5 g to 3 g of powder material B, add 80 mL to 100 mL of water, adjust the pH to the range of 0.5 to 1.5, and stir in a water bath. After 10 min to 30 min, a solution is obtained. The solution is centrifuged 3 to 5 times in a centrifuge, and the obtained precipitate is washed and dried to obtain the desired product C.
[0036] In this step, the modified powder is added, the pH value is adjusted by a one-step method, and the microstructure is regulated in a water bath at 30° C. to form a type II heterojunction structure. On the one hand, in the present invention, the addition of the molten salt in step 2 can accurately regulate the proportion of the generated crystalline phase, and on the other hand, it can be formed by a one-step method, reducing the reaction steps and making the preparation process simpler.
[0037] Method 2: Wash the powder material B alternately in the order of water-alcohol for 3 to 5 times, and dry the obtained sample to obtain the product. Take 0.1g to 0.35g, add 30mL to 50mL of water, and stir for 1h to 2h; add nitric acid to adjust the pH to 1 to 3 and stir for 10min to 40min; finally, add 5mL to 60mL of NaCl, NaBr, LiCl, ZnCl with a concentration of 1g / L to 3g / L respectively. 2 The salt solution is stirred in a water bath for 10 to 40 minutes, and the stirred sample is centrifuged 3 to 5 times to obtain the desired sample D.
[0038] In this step, the molten salt in step 2 is washed away, and then new molten salt is added to adjust the microstructure of the catalyst, so that the catalyst generates a type II heterojunction structure. This method can make the prepared catalyst produce more defects in the process, and the photogenerated carrier transition and separation are easier. In addition, the addition of molten salt can achieve precise control of the crystal phase ratio, generate more oxygen vacancies and adsorbed oxygen, and the prepared product is more conducive to the transformation of industrialization.
[0039] Of the two methods of the present invention, method one is more concise, while product D obtained by method two has a faster efficiency in degrading water pollutants, a more obvious effect, and is more conducive to industrial transformation.
[0040] Based on the above technical solutions and principles, several specific embodiments of the present invention are as follows.
[0041] Example 1
[0042] (1) The raw material Bi 2 O 3 and SiO 2 Weigh according to the molar ratio of 1:1, with 35wt% K 2 CO3 -KCl is used as the salt used in the present invention, and a uniform powder material A is obtained by mixing and ball milling for 3 hours; wherein K 2 CO 3 The molar ratio of KCl is 0.30:0.65.
[0043] (2) Weigh 3 g of the uniformly ground powder material A and calcine it in a muffle furnace at 620°C with a heating rate of 5°C / min, and keep it warm for 0.5 h. After the reaction is completed, take out the sample and cool it to obtain powder material B;
[0044] (3) Weigh 0.5 g of powder material B, add 80 mL of water, adjust the pH to 0.5, stir in a water bath for 10 min to obtain a solution, centrifuge the solution three times, wash and dry, and obtain the desired product C;
[0045] (4) After the powder material B was washed alternately three times in the order of water-alcohol, the obtained sample was dried, 0.2 g was added to 30 mL of water and stirred for 1 h, nitric acid was added to adjust the pH, and when the pH value was adjusted to about 1, stirring was continued for 60 min. Finally, 5 mL of NaCl salt solution with a concentration of 1.8 g / L was added and stirred in a water bath for 10 min. The stirred sample was centrifuged three times to obtain the desired sample D.
[0046] Example 2
[0047] (1) The raw material Bi 2 O 3 and SiO 2 Weigh according to the molar ratio of 3:1, with 40wt% K 2 CO 3、 KCl is used as the salt in the present invention, and a uniform powder material A is obtained by mixing and ball milling for 3 hours; wherein K 2 CO 3 The molar ratio of KCl is 0.33:0.66.
[0048] (2) Weigh 3.5 g of the uniformly ground powder material A and calcine it in a muffle furnace at 690°C with a heating rate of 10°C / min, and keep it warm for 0.8 h. After the reaction is completed, take out the sample and cool it to obtain powder material B;
[0049] (3) Weigh 1 g of powder material B, add 100 mL of water, adjust the pH to 1, stir in a water bath for 30 min to obtain a solution, centrifuge the solution for 4 min, then wash and dry to obtain the desired product C;
[0050] (4) After the powder material B was washed alternately three times in the order of water-alcohol, the obtained sample was dried, 0.30 g was added to 35 mL of water and stirred for 1.5 h, nitric acid was added to adjust the pH, and when the pH value was adjusted to about 1.5, stirring was continued for 40 min. Finally, 10 mL of NaBr salt solution with a concentration of 1.6 g / L was added and stirred in a water bath for 30 min. The stirred sample was centrifuged three times to obtain the desired sample D.
[0051] The SEM image of the product D obtained in this example is as follows Figure 1 As shown, it can be seen that the powder particles are stacked together in a thin flake structure with a thickness of about 0.05μm. The surface of the nanosheet is relatively smooth and the sheets overlap with each other. The inorganic material presents a heterojunction morphology structure grown on the nanosheet, exposing a large number of sites on the surface and forming a three-dimensional structure that is intertwined in space.
[0052] Figure 2 The photocatalytic degradation curves of the catalyst products C and D obtained in this example are put into a solution containing the organic dye Rhodamine B and then degraded. In the experiment, 10 mg / L of Rhodamine B was taken, and the photocatalyst was put into the solution, and the photocatalytic reaction was carried out for 90 minutes, including 60 minutes of dark reaction and 30 minutes of light reaction. It can be seen from the photocatalytic degradation graph that under the condition of 30 minutes of illumination, the degradation rate is close to 100%. This is due to the fact that the heterojunction shunts electron holes, inhibits recombination, and increases the surface area and defect formation, providing more active sites for the prepared catalyst, so that more organic pollutants can react at the active sites, thereby effectively improving the photocatalytic effect.
[0053] Example 3
[0054] (1) The raw material Bi 2 O 3 and SiO 2 Weigh according to the molar ratio of 6:1, with 42wt% K 2 CO 3 -KCl is used as the salt used in the present invention, and a uniform powder material A is obtained by mixing and ball milling for 3 hours; wherein K 2 CO 3 The molar ratio of KCl is 0.35:0.73.
[0055] (2) Weigh 4 g of the uniformly ground powder material A and calcine it in a muffle furnace at 720°C with a heating rate of 10°C / min, and keep it warm for 1 hour. After the reaction is completed, take out the sample and cool it to obtain powder material B;
[0056] (3) Weigh 3 g of powdered material B, add 100 mL of water, adjust the pH to 1.5, stir in a water bath for 30 min to obtain a solution, centrifuge the solution 5 times, wash and dry to obtain the desired product C;
[0057] (4) After the powder material B was washed alternately with water-alcohol for 5 times, the obtained sample was dried, 0.35 g was added to 50 mL of water and stirred for 1 h, nitric acid was added to adjust the pH, and stirring was continued for 30 min after the pH value was adjusted to about 1. Finally, 45 mL of LiCl salt solution with a concentration of 2 g / L was added and stirred in a water bath for 40 min. The stirred sample was centrifuged 3 times to obtain the desired sample D.
[0058] The operation method of the present invention is simple in steps, and the powder material prepared has uniform particle size and is not easy to agglomerate. The heterojunction structure with excellent activity is used to increase the overall catalytic sites, increase the active sites in the reaction process, and help regulate the activity of the catalytic sites to show higher photocatalytic performance. In addition, the photocatalyst is generally applicable and recyclable to antibiotics, and has the ability to degrade rhodamine B, tetracycline (TC), and ciprofloxacin (CIP), which greatly broadens its application scope and application prospects.
[0059] In more embodiments of the present invention, the above parameters are combined in different types. For example, in step 1), 2 O 3 With SiO 2 The mixing ratios were 1:1, 3:1, 4:1, 6:1, and 9:1, respectively. 2 CO 3 -KCl was used as the salt in the present invention to carry out experiments, with the proportions of 35wt%, 40wt%, and 45wt%, respectively. The ball milling time was selected to be 3h, 3.5h, 4h, 4.5h, and 5h, respectively. The results showed that powder A could be prepared.
[0060] Similarly, in step 2), 3.0 g, 3.3 g, 3.5 g, 3.7 g, 3.9 g, 4.3 g, 4.6 g and 5.0 g of powder A were weighed respectively and calcined at 620°C, 634°C, 730°C and 745°C in a muffle furnace. The heating rates were 5°C / min, 10°C / min and 15°C / min, and the holding times were 0.5 h, 0.8 h, 1 h, 2 h and 3 h respectively. Powder B was prepared after cooling the initial sample.
[0061] Similarly, in step 3), the powder B prepared in the above experiment can be weighed in an amount of 0.5 g, 1 g, 1.5 g, 2 g, and 3 g. After the reaction, the pH is adjusted to 0.1, 0.5, 1, and 1.5 by adding different amounts of water of 80 mL, 85 mL, 90 mL, 95 mL, and 100 mL, and then stirred in a water bath. The stirring time is 10 min, 15 min, 20 min, and 30 min, and then cooled to room temperature, centrifuged 3 times, 4 times, and 5 times and washed, and then dried in a drying oven. The results show that powder product C can be prepared.
[0062] For example, in step 4), the obtained fraction product B is washed alternately with water and alcohol for 3, 4, and 5 times, and the obtained sample is dried to obtain the product. 0.1 g, 0.15 g, 0.25 g, and 0.35 g of the sample are added with 30 mL, 40 mL, and 50 mL of water, respectively, and stirred for 1 h, 1.3 h, 1.4 h, and 1.5 h; nitric acid is added to adjust the pH, and after adjusting the pH to 1, 2, and 3, different concentrations of salt are added, stirred, and then centrifuged, and the washed sample is dried to obtain product D.
[0063] In summary, the present invention introduces a low melting point molten salt K 2 CO 3 -KCl, bismuth silicate is calcined in a molten salt medium and then reacted with acid to form Bi 12 -X(X=Bi 2 -BiOCl, BiOCl)(Bi 12 =Bi 12 SiO 20 、Bi 2 =Bi 2 SiO 5 ) multi-heterogeneous catalytic materials. By regulating Bi 2 、Bi 12 The crystal phase ratio can effectively regulate the band gap position and inhibit the recombination of electrons and holes. At the same time, the morphology of the catalyst changes from particle agglomerates to flower-like shapes stacked with nanosheets, which is conducive to the catalytic reaction. The multi-heterogeneous photocatalyst obtained by the method of the present invention has a simple preparation process, low required temperature, low material cost, and more active sites. It can be used multiple times in the degradation process and has good performance, and is expected to achieve industrial production.
[0064] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, substitutions, combinations, simplifications, etc. made based on the principles or spirit of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a controllable bismuth-based multi-heterojunction photocatalytic material, characterized in that: The steps include: Step 1, taking Bi2O3, SiO2 and K2CO3, KCl and mixing and grinding them uniformly; wherein the molar ratio of Bi2O3 to SiO2 is 1:1-9:1, the molar ratio of K2CO3 to KCl is 0.30:0.65-0.35:0.73, and K2CO3 and KCl account for 35wt%-45wt% of the total amount of the mixture; Step 2, calcining the mixed and ground materials obtained in step 1 at 620° C. to 750° C. for 0.5 to 3 hours and then cooling; Step 3, obtaining the controllable bismuth-based multi-heterojunction photocatalytic material by one of the following methods: Method 1: Add water to the material obtained in step 2 and adjust the pH to 0.5-1.5, stir in a water bath, and centrifuge to dry. Method 2: The material obtained in step 2 is washed alternately with water and alcohol for multiple times, and then dried; water is added and the pH is adjusted to 1-3, and salt is added, stirred in a water bath, and centrifuged to obtain the product.
2. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1, characterized in that: The step 1 is to mix and ball mill for 3 hours to 8 hours.
3. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1, characterized in that: In the step 1, K2CO3 is combined with KCl to form a composite salt.
4. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1, characterized in that: In the step 2, the heating rate is set to 5°C / min during calcination, and the calcination temperature is maintained for 0.5h to 3h after reaching the calcination temperature.
5. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1, characterized in that: The method 1 comprises the following steps: weighing 0.5 g to 3 g of the material obtained in step 2, adding 80 mL to 150 mL of water, then adding acid to adjust the pH to 0.5 to 1.5, stirring for 10 min to 30 min, centrifuging 3 to 5 times, and the water bath condition is: stirring at 30° C. for 10 min to 30 min.
6. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1, characterized in that: The second method comprises the following steps: weighing 0.1 g to 0.35 g of the material obtained in step 2, washing it with water and alcohol alternately for multiple times, and then drying it; then adding 30 mL to 50 mL of water, stirring it for 1 h to 2 h, adding acid to adjust the pH to 1 to 3, adding 5 mL to 60 mL of a salt solution with a concentration of 1 g / L to 3 g / L, stirring it for 10 min to 40 min, and then centrifuging it for 3 to 5 times.
7. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1 or 6, characterized in that: The salt added in the second method is one or more of NaCl, NaBr, LiCl and ZnCl2.
8. The method for preparing the controllable bismuth-based multi-heterojunction photocatalytic material according to claim 1 or 6, characterized in that: In the second method, the water bath condition is: stirring at 30° C. for 30 min to 40 min.
9. The use of the adjustable bismuth-based multi-heterojunction photocatalytic material obtained by the preparation method of the adjustable bismuth-based multi-heterojunction photocatalytic material according to any one of claims 1 to 8 as a catalyst for sewage treatment, which achieves the purpose of purifying water quality by decomposing organic matter and pollutants in the water.
10. The use according to claim 9, characterized in that The controllable bismuth-based multi-heterojunction photocatalytic material is directly added into industrial wastewater.
Citation Information
Patent Citations
Method for preparing Bi2SiO5 powder by molten salt growth method
CN101979320A
A method for preparing bismuth silicate powder using the molten salt method
CN102275943A
Method for preparing flaky bismuth silicate powder
CN102351203A
Electrochemical preparation method of BiOBr / Bi12SiO20 composite film photocatalyst and application of BiOBr / Bi12SiO20 composite film photocatalyst
CN110624575A
Nanosheet layer stacked controllable flower-like BSOCB photocatalyst and preparation method thereof
CN117085744A