Hydrofining catalyst and preparation method thereof

By optimizing the preparation process of transition metal phosphide catalysts in the co-precipitation method, using the specific preparation of multi-metal solutions and precipitants and the gelling reaction sequence, the problems of uneven distribution of active metals and small pore volume are solved, and the performance of the catalyst is improved. Hydrogenation activity and utilization rate, suitable for advanced treatment of heavy diesel.

CN118807797AActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310432259.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-22
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

During the preparation process of existing transition metal phosphide hydrogenation catalysts by the co-precipitation method, the active metals are unevenly distributed, and the pore volume and specific surface area are small, resulting in low utilization of the active metals of the catalyst and inability to effectively improve the hydrogenation activity.

Method used

The specific preparation of multi-metal solutions and precipitants and the sequence of gel-forming reactions are adopted. Through multiple pH aging and the use of phosphate compounds, the reaction conditions and temperature are controlled to form a phosphide catalyst with high transition metal content and improve the performance of the catalyst. Pore ​​size distribution and surface metal content.

Benefits of technology

The catalyst with high surface active site density and small phosphide particles is prepared, which significantly improves the hydrodesulfurization and denitrogenation reaction performance. It is suitable for ultra-deep hydrotreating of heavy diesel and reduces the cost of catalyst preparation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a hydrofining catalyst and a preparation method thereof. The hydrofining catalyst comprises transition metal phosphide and aluminum oxide, the transition metal phosphide is WP (Wolfram Phosphate) and Ni2P (Ni2P); wherein the ratio of the weight content of Ni2P in the surface phase to the weight content of Ni2P in the bulk phase is (2.5: 1)-(7.0: 1), and the ratio of the weight content of WP in the surface phase to the weight content of WP in the bulk phase is (2.5: 1)-(6.5: 1). The preparation method comprises the following steps: (1) carrying out first gelling reaction on a multi-metal solution and a precipitator to obtain first slurry; (2) adding the first slurry, a nickel-containing solution and a precipitant into a gel forming tank containing bottom water and a phosphate compound, and carrying out a second gel forming reaction to obtain second slurry; (3) performing multiple times of pH-value-variable aging on the second slurry, and adding one part of sodium metaaluminate solution in each aging process to obtain third slurry; and (4) filtering, drying and forming the third slurry to prepare the hydrofining catalyst. The catalyst disclosed by the invention is large in surface phase active site density and suitable for being applied to ultra-deep hydrodesulfurization and denitrification reactions of diesel fractions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogenation catalysts, and specifically relates to a phosphide hydrogenation refining catalyst with a high transition metal content and a preparation method thereof. Background Art

[0002] Phosphide catalyst is a new type of hydrogenation catalyst. In transition metal phosphides, metal atoms form the smallest structural unit of triangular prism structure. These triangular prism units form different lattice types in different combinations, and phosphorus atoms occupy the gaps inside the triangular prism. Phosphide is a triangular prism unit structure, which is similar to a sphere. Phosphide can expose more coordinated unsaturated surface atoms than sulfide, thus having a higher surface active site density. The factors affecting the activity of phosphides are mainly: 1. The content of active metal. The more active metals in phosphide, the more active centers can be provided. 2. The pore size and specific surface area of ​​phosphide catalyst affect its hydrogenation activity. Uneven dispersion of active metals will cause disordered distribution of different hydrogenation active metals. High content of metal in bulk catalyst is prone to excessive accumulation of metal particles, which reduces the generation of active phase. 3. The co-precipitation method has a high content of active metal, but the surface metal content is not high, resulting in the second highest metal utilization rate. The degree of phosphating of the precursor oxide prepared by this method affects the activity of its phosphide. 4. The grain size and dispersion of phosphide particles affect their activity.

[0003] CN101992109A discloses a transition metal phosphide hydrogenation refining catalyst and its preparation method. CN101168132A, CN1660695A, CN103962165A, and CN102744089A use different methods to make the active metal more dispersed on the carrier during the preparation process. However, the transition metal phosphide obtained by the above method has a large grain size, uneven distribution of active metals, relatively small active metal content, and no significant improvement in hydrogenation activity.

[0004] CN202010928225.9 provides a bulk nickel phosphide catalyst and a preparation method, first preparing a buffer system with a pH of 4-6, adding hypophosphite to the buffer system, then slowly adding nickel salt or a mixed solution of nickel salt and auxiliary metal M precursor, reacting at 85-95°C for 1-6h, filtering and washing, and drying at 90-120°C to obtain an amorphous precursor; the amorphous precursor is heat-treated in a hydrogen atmosphere, and then cooled to obtain a bulk nickel phosphide catalyst. The present invention successfully prepares a Ni-P-based catalyst with Ni3P as the active phase using a simple liquid phase reduction method, but the pore volume and specific surface area of ​​the catalyst are small.

[0005] CN111822015B discloses a method for preparing a hydrorefining catalyst. The method comprises: (1) preparing a mixed solution A and a mixed solution B containing transition metals respectively; (2) adding the mixed solution A and the sodium aluminate alkaline solution to a reaction tank in parallel to perform a gelling reaction to obtain slurry I, and aging; (3) adding the mixed solution B and the sodium aluminate alkaline solution to the aged slurry I in parallel to perform a gelling reaction to obtain slurry II, adding an organic phosphorus compound, and aging; (4) drying, shaping, and calcining the obtained material to obtain a phosphide catalyst precursor; (5) reducing the obtained material by hydrogen program temperature rise to obtain a hydrorefining catalyst; the catalyst phosphide prepared by the method has small particles, more active centers, and good dispersion, but its surface metal content is small, the degree of phosphating is low, and the hydrogenation activity needs to be further improved.

[0006] At present, the number of active centers of phosphide catalysts prepared by coprecipitation can be greatly increased. Compared with supported phosphide catalysts, although the phosphide catalysts prepared by coprecipitation have high active metal content, their pore volume and specific surface area are small, the phosphide particles are of different sizes, and the active metal content in the catalyst surface phase is low, which affects the utilization rate of active metals. Therefore, how to increase the pore volume and specific surface area of ​​phosphide catalysts prepared by coprecipitation, increase the content of active metals in the catalyst surface phase, and improve the utilization rate of phosphides are the main problems faced by the preparation of phosphide catalysts by coprecipitation. Summary of the invention

[0007] In view of the deficiencies of the prior art, the present invention provides a hydrorefining catalyst and a preparation method thereof. The catalyst is a phosphide hydrorefining catalyst with a high transition metal content, a large surface active site density, more active centers, a small phosphide grain size, and high hydrodesulfurization and hydrodenitrogenation reaction performance, and is suitable for use in ultra-deep hydrodesulfurization and denitrogenation reactions of diesel fractions.

[0008] The hydrotreating catalyst of the present invention comprises a transition metal phosphide and alumina. Based on the weight of the catalyst, the total content of the transition metal phosphide is 35% to 82%, preferably 38% to 78%, and the content of alumina is 18% to 65%, preferably 22% to 62%. The transition metal phosphide is WP and Ni2P. The ratio of the weight content of Ni2P in the surface phase to the weight content of Ni2P in the bulk phase is 2.5:1 to 7.0:1, preferably 3.0:1 to 6.5:1, and the ratio of the weight content of WP in the surface phase to the weight content of WP in the bulk phase is 2.5:1 to 6.5:1, preferably 3.0:1 to 6.0:1.

[0009] The Ni / W molar ratio is 0.1:1-12:1, preferably 0.3:1-10:1.

[0010] The average particle diameter of the transition metal phosphide is 2-7 nm, preferably 3-6 nm.

[0011] The pore size distribution of the hydrotreating catalyst is as follows: the pore volume occupied by pores with a diameter of less than 6 nm accounts for 2% to 10% of the total pore volume, the pore volume occupied by pores with a diameter of 6 to 10 nm accounts for 45% to 67% of the total pore volume, the pore volume occupied by pores with a diameter of 10 to 15 nm accounts for 12% to 35% of the total pore volume, and the pore volume occupied by pores with a diameter of more than 15 nm accounts for 10% to 28% of the total pore volume.

[0012] The preparation method of the hydrotreating catalyst of the present invention comprises the following contents: (1) adding a multi-metal solution and a first precipitant in parallel into a colloidation tank containing bottom water to perform a first colloidation reaction to obtain a first slurry; the multi-metal solution is a solution containing W, Ni, and Al; the first precipitant is ammonia water and sodium phosphate solution; (2) adding the first slurry, the nickel-containing solution and the second precipitant in parallel into a gelling tank containing bottom water and a phosphate compound to carry out a second gelling reaction to obtain a second slurry; the second precipitant is ammonia water and a sodium phosphate solution; (3) the second slurry is subjected to multiple pH-changing aging processes, and a portion of sodium aluminate solution is added during each aging process to obtain a third slurry; (4) The third slurry is filtered, dried, formed, washed, dried, and calcined to obtain a phosphide catalyst precursor, which is then reduced with hydrogen to obtain a hydrotreating catalyst.

[0013] In the method of the present invention, in the first precipitant and the second precipitant in step (1) and step (2), the concentration of the aqueous ammonia is 5wt% to 10wt%, the concentration of the sodium phosphate solution is 8wt% to 20wt%, the molar ratio of the aqueous ammonia as NH3 to the sodium phosphate is 0.2:1 to 0.6:1, and the molar ratio of the aqueous ammonia to the sodium phosphate in steps (1) and (2) may be the same or different, preferably the same.

[0014] In the method of the present invention, in the multi-metal solution of step (1), the weight concentration of W calculated as WO3 is 5 to 140 g / L, preferably 10 to 130 g / L, the weight concentration of Ni calculated as NiO is 5 to 110 g / L, preferably 8 to 105 g / L, and the weight concentration of Al calculated as Al2O3 is 2 to 90 g / L, preferably 6 to 85 g / L; wherein, when preparing the solution containing W, Ni and Al, the tungsten source generally used is ammonium metatungstate, the nickel source generally used is one or more of nickel sulfate, nickel nitrate and nickel chloride; and the aluminum source is one or more of aluminum nitrate, aluminum sulfate, aluminum chloride and aluminum acetate.

[0015] In the method of the present invention, the conditions of the first gelling reaction in step (1) are as follows: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value of the co-current reaction is controlled at 5 to 6, and the reaction time is 0.1 to 1.0 hour.

[0016] In the method of the present invention, in the nickel-containing solution described in step (2), the weight concentration of Ni in terms of NiO is 10 to 130 g / L, preferably 15 to 115 g / L; when preparing the nickel-containing solution, the nickel source is generally one or more of nickel sulfate, nickel nitrate, and nickel chloride; In the method of the present invention, the phosphate compound described in step (2) is one or more of octadecyl ether phosphate (O-5P), alkylphenol ether phosphate (TXP-4, TXP-10), isomeric tridecanol ether phosphate (E-1310P), lauryl alcohol ether phosphate (MOA-3P, MOA-9P), castor oil phosphate, octadecyl phosphate, and lauryl phosphate, preferably one or more of alkylphenol ether phosphate (TXP-4, TXP-10), isomeric tridecanol ether phosphate (E-1310P), lauryl alcohol ether phosphate (MOA-3P, MOA-9P), octadecyl phosphate, and castor oil phosphate. The molar ratio of the added amount of the phosphate compound to the Ni in the nickel-containing solution is 0.8:1 to 6.0:1, preferably 1.5:1 to 5.5:1.

[0017] In the method of the present invention, the conditions of the second gelling reaction described in step (2) are as follows: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value is controlled at 8.0 to 10.5 at the end, and the reaction time is 0.5 to 2.5 hours; preferably, the reaction temperature of step (2) is the same as the reaction temperature of step (1).

[0018] In the method of the present invention, the multiple pH value changing aging process described in step (3) is as follows: in the first step, a portion of sodium aluminate solution is dripped into the second reaction slurry to control the pH value to 11.5-13.5, and the aging is performed for 0.05-0.5 hours; in the second step, the pH value is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; in the third step, the pH value is adjusted to 4.5-6.3, and the aging time is 0.05-0.5 hours; the three-step pH value changing process is repeated multiple times, preferably 2-8 times; the aging temperature is 60-98°C, preferably 65-92°C. In the aging process, except for the sodium aluminate solution used in the first step of pH value adjustment, the acid and alkali used for adjusting the pH value can be inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements, the inorganic acid can be hydrochloric acid and acetic acid, and the inorganic alkali can be one or more of sodium carbonate, sodium bicarbonate, ammonia water, and sodium hydroxide. The concentration and dosage of the acid and alkali solutions can be adjusted according to the actual preparation needs.

[0019] In the method of the present invention, the sodium aluminate solution in step (3) has a weight concentration of Al in terms of Al2O3 of 5 to 70 g / L, preferably 8 to 60 g / L. The sodium aluminate solution is divided equally by volume, the number of portions being the number of multiple agings.

[0020] In the method of the present invention, the Ni added via the Ni-containing solution accounts for 55% to 85%, preferably 60% to 82%, of the total Ni in the obtained hydrorefining catalyst calculated as NiO.

[0021] In the method of the present invention, the Al added via the sodium aluminate solution accounts for 5% to 55%, preferably 6% to 50%, of the total Al in the obtained hydrorefining catalyst calculated as Al2O3.

[0022] In the method of the present invention, the drying, molding and washing described in step (4) can be carried out by conventional methods in the art. The drying conditions are as follows: drying at 40-150°C for 1-48 hours, preferably drying at 50-120°C for 4-36 hours. During the molding process, conventional molding aids, such as one or more of peptizers, extrusion aids, etc., can be added as needed. The peptizer is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the extrusion aid refers to a substance that is conducive to extrusion molding, such as one or more of sesbania powder, carbon black, graphite powder, citric acid, etc., and the amount of the extrusion aid accounts for 1wt% to 10wt% of the total material dry basis. Washing is generally performed with deionized water or a solution containing decomposable salts (such as ammonium acetate, ammonium chloride, ammonium nitrate, etc.) until neutral.

[0023] In the method of the present invention, the roasting conditions in step (4) are as follows: the roasting temperature is 350-700° C., and the roasting time is 1-24 hours.

[0024] In the method of the present invention, the hydrogen reduction in step (4) adopts programmed temperature reduction, and the specific process includes: the precursor is in a hydrogen atmosphere, the hydrogen purity is greater than 99v%, the hydrogen flow rate is 150~700mL / min, preferably 250~600mL / min; in the first stage, the temperature is increased from room temperature to 300~550℃ at a rate of 3~10℃ / min, and the temperature is kept constant for 1~5 hours; in the second stage, the temperature is increased to 600~750℃ at a rate of 0.5~5℃ / min, and the temperature is kept constant for 2~8 hours; the temperature increase rate in the second stage is at least 1℃ / min lower than the temperature increase rate in the first stage, preferably at least 2℃ / min lower. In order to prevent the phosphide from vigorous oxidation reaction when it contacts with air, before the prepared catalyst sample contacts with air, it is first passivated with O2 / N2 passivation gas with an oxygen volume concentration of 0.5%~3% for 1~5 hours.

[0025] The hydrotreating catalyst of the present invention can be in the form of flakes, spheres, cylindrical bars and special-shaped bars (three-leaf clover, four-leaf clover) as required, preferably cylindrical bars and special-shaped bars (three-leaf clover, four-leaf clover). The diameter of the catalyst can be a thin bar of 0.8-2.0 mm or a thick bar of >2.5 mm.

[0026] The hydrorefining catalyst of the present invention is used in ultra-deep hydrodesulfurization, denitrogenation reaction and hydrodearomatization of heavy diesel fractions, wherein the aromatic content in the heavy diesel fraction is 50wt% to 85wt% and the cetane number is less than 24.

[0027] The catalyst surface phase in the bulk catalyst of the present invention has a relatively high hydrogenation active site, a high utilization rate of active metals, and improves the hydrogenation activity of heavy oil treatment, reduces the catalyst preparation cost, and is particularly beneficial to the aromatic saturation of heavy oil, effectively reduces the content of polycyclic aromatic hydrocarbons, and improves the cetane number. Compared with the prior art, the specific advantages are as follows: 1. The present invention adopts phosphate and sodium phosphate as phosphorus sources, wherein sodium phosphate and ammonia water are used as precipitants in a specific ratio, and phosphorus is evenly distributed in the generated reactants. Phosphate is added in the second gelling reaction process to make phosphorus evenly distributed on the catalyst surface, while improving the strong interaction between W, Ni, P and the carrier, so that the transition active metal is fully phosphated to prevent the phosphide from aggregating on the catalyst surface.

[0028] 2. The present invention first precipitates the W, Ni, and Al solutions, and then drops the Ni-containing solution into the resulting slurry at a specific pH value. The specific addition sequence, the corresponding pH value control, and the active metal precipitation sequence significantly increase the active metal content in the surface phase.

[0029] 3. The present invention dissolves amorphous oxides in oxide particles through multiple pH value aging processes, and the size of oxide particles is re-modified by adding sodium aluminate solution. After the pH value swings n times, the growth of oxide particles is controlled to make the oxide particles more uniform and small, exposing more active metals in the surface phase, which can increase the macropores in the bulk catalyst and make it easier for macromolecular reactants to pass through the pores. At the same time, the aluminum introduced by the sodium aluminate solution increases the surface hydroxyl groups, further enhancing the adhesion of the oxide, which is beneficial to the formation of the bulk catalyst. DETAILED DESCRIPTION

[0030] In the present invention, the specific surface area, pore volume and pore distribution are measured by low temperature liquid nitrogen adsorption method, the mechanical strength is measured by lateral pressure method, and the diameter of transition metal phosphide particles is measured by TEM technology. In the present invention, wt% is mass fraction and v% is volume fraction.

[0031] The phosphide content of the catalyst surface phase is determined by X-ray photoelectron spectroscopy (XPS), and the phosphide content of the catalyst bulk phase is determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES). First, the surface phase and bulk active metal content of the transition metal oxide of the catalyst precursor of the present invention are determined, and then converted into the transition metal phosphide content of the catalyst surface phase and bulk phase. Example 1

[0032] Ammonium metatungstate, nickel chloride and aluminum chloride solution are added to a dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in terms of WO3 is 40 g / L, the weight concentration of Ni in terms of NiO is 28 g / L, and the weight concentration of Al in terms of Al2O3 is 56 g / L. Nickel chloride is added to a dissolution tank 2 filled with deionized water to prepare a solution containing Ni, wherein the Ni in the Ni-containing solution accounts for 65% of the total Ni in terms of NiO in the obtained hydrorefining catalyst. The Al in the sodium aluminate solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and the solution is divided into 4 equal parts by volume, deionized water is added to the reaction tank 1, and ammonia water, sodium phosphate solution and a solution containing W, Ni and Al are added to the reaction tank in parallel to perform a gelling reaction, the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.4:1, the gelling temperature is maintained at 60°C, the pH value is controlled at 5.2 during the parallel gelling reaction, and the gelling time is controlled at 0.7 hours to generate a precipitate slurry I containing W, Al, Ni and P. Deionized water and castor oil phosphate are added to the reaction tank 2, and the molar ratio of castor oil phosphate to the total number of Ni atoms in the Ni-containing solution is 2.6. The slurry I containing W, Al, Ni, and P, the solution containing Ni, and the ammonia water and sodium phosphate solution are added to the reaction tank 2 in parallel (the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.4:1), the reaction temperature remains unchanged, the reaction time is 1.0 hour, the reaction pH value is controlled at 8.9, and a precipitate slurry containing nickel, tungsten, aluminum, and phosphorus is generated. The resulting slurry is aged at an aging temperature of 76°C. During aging, an equal portion of sodium aluminate solution is first added to control the pH value to 13.3. After aging for 0.2 hours, the aging pH value is controlled at 9.7. After aging for 0.2 hours, the pH value is then controlled to 5.5, and the aging time is 0.15 hours. The above operation process is repeated 4 times to end aging. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. Then the washed wet strips are dried at 80°C for 10.0 hours. The dried material was calcined at 530°C for 5 hours to obtain the phosphide catalyst precursor A. Precursor A was heated from room temperature to 410°C in a pure hydrogen atmosphere at a hydrogen flow rate of 290 mL / min and a heating rate of 6°C / min. After being kept at this temperature for 3.6 hours, it was heated to 710°C at a heating rate of 2.5°C / min and kept at this temperature for 4 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2% for 2 hours before being exposed to air to obtain a hydrorefining catalyst A. The catalyst composition and main physicochemical properties are shown in Table 1. Example 2

[0033] Ammonium metatungstate, nickel chloride and aluminum chloride solution are added to a dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in terms of WO3 is 46 g / L, the weight concentration of Ni in terms of NiO is 25.9 g / L, and the weight concentration of Al in terms of Al2O3 is 54.6 g / L. Nickel chloride is added to a dissolution tank 2 filled with deionized water to prepare a solution containing Ni, wherein the Ni in the Ni-containing solution accounts for 63% of the total Ni in terms of NiO in the obtained hydrorefining catalyst. The Al in the sodium aluminate solution accounts for 35% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and the solution is divided into 5 equal parts by volume. Deionized water is added to the reaction tank 1, and ammonia water, sodium phosphate solution and a solution containing W, Ni and Al are added to the reaction tank in parallel to perform a gelling reaction. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.35:1, the gelling temperature is maintained at 65°C, the pH value is controlled at 5.5 during the parallel gelling reaction, and the gelling time is controlled at 0.8 hours to generate a precipitate slurry I containing W, Al, Ni and P. Deionized water and lauryl ether phosphate are added to the reaction tank 2, and the molar ratio of lauryl ether phosphate to the total number of Ni atoms in the Ni-containing solution is 2.3. The slurry I containing W, Al, Ni, and P, the solution containing Ni, and the ammonia water and sodium phosphate solution are added to the reaction tank 2 in parallel (the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.35:1), the reaction temperature is unchanged, the reaction time is 1.2 hours, the reaction pH value is controlled at 9.3, and a precipitate slurry containing nickel, tungsten, aluminum, and phosphorus is generated. The resulting slurry is aged at an aging temperature of 80°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 13.0. After aging for 0.15 hours, the aging pH value is controlled to 9.4. After aging for 0.2 hours, the pH value is then controlled to 5.1, and the aging time is 0.15 hours. Repeat the above operation process 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 90°C for 9 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. Then the washed wet strips are dried at 80°C for 9.0 hours. The dried material was calcined at 540°C for 4 hours to obtain the phosphide catalyst precursor B. Precursor B was heated from room temperature to 415°C in a pure hydrogen atmosphere at a hydrogen flow rate of 320 mL / min and a heating rate of 5°C / min. After being kept at this temperature for 3.4 hours, it was heated to 680°C at a heating rate of 3.0°C / min and kept at this temperature for 6 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2.2% for 3 hours before being exposed to air to obtain the hydrofining catalyst B. The catalyst composition and main physicochemical properties are shown in Table 1. Example 3

[0034] Ammonium metatungstate, nickel chloride and aluminum chloride solution are added to a dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in terms of WO3 is 30 g / L, the weight concentration of Ni in terms of NiO is 26.4 g / L, and the weight concentration of Al in terms of Al2O3 is 60.7 g / L. Nickel chloride is added to a dissolution tank 2 filled with deionized water to prepare a solution containing Ni, wherein the Ni in the Ni-containing solution accounts for 70% of the total Ni in terms of NiO in the obtained hydrorefining catalyst. The Al in the sodium aluminate solution accounts for 26% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and the solution is divided into 6 equal parts by volume, deionized water is added to the reaction tank 1, and ammonia water, sodium phosphate solution and a solution containing W, Ni and Al are added to the reaction tank in parallel to perform a gelling reaction, the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.42:1, the gelling temperature is maintained at 55°C, the pH value is controlled at 5.7 during the parallel gelling reaction, and the gelling time is controlled at 0.7 hours to generate a precipitate slurry I containing W, Al, Ni and P. Deionized water and isomeric tridecanol ether phosphate are added to the reaction tank 2, and the molar ratio of isomeric tridecanol ether phosphate to the total number of Ni atoms in the Ni-containing solution is 3.2. The slurry I containing W, Al, Ni, and P, the solution containing Ni, and the ammonia water and sodium phosphate solution are added to the reaction tank 2 in parallel (the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.42:1), the reaction temperature is unchanged, the reaction time is 1.3 hours, the reaction pH value is controlled at 8.7, and a precipitate slurry containing nickel, tungsten, aluminum, and phosphorus is generated. The resulting slurry is aged at an aging temperature of 83°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 12.7. After aging for 0.2 hours, the aging pH value is controlled to 9.9. After aging for 0.15 hours, the pH value is then controlled to 4.6, and the aging time is 0.2 hours. The above operation process is repeated 6 times to end aging. The aged slurry is filtered, the filter cake is dried at 120°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. Then the washed wet strips are dried at 90°C for 10.0 hours. The dried material was calcined at 510°C for 6 hours to obtain the phosphide catalyst precursor C. Precursor C was heated from room temperature to 440°C in a pure hydrogen atmosphere at a hydrogen flow rate of 350 mL / min and a heating rate of 7°C / min. After being kept at this temperature for 2.9 hours, it was heated to 660°C at a heating rate of 4.0°C / min and kept at this temperature for 6 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2.3% for 3.2 hours before being exposed to air to obtain the hydrofining catalyst C. The catalyst composition and main physicochemical properties are shown in Table 1. Example 4

[0035] Ammonium metatungstate, nickel chloride and aluminum chloride solution are added to a dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in terms of WO3 is 24 g / L, the weight concentration of Ni in terms of NiO is 23 g / L, and the weight concentration of Al in terms of Al2O3 is 52 g / L. Nickel chloride is added to a dissolution tank 2 filled with deionized water to prepare a solution containing Ni, wherein the Ni in the Ni-containing solution accounts for 75% of the total Ni in the obtained hydrorefining catalyst in terms of NiO. The Al in the sodium aluminate solution accounts for 38% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and the solution is divided into 5 equal parts by volume. Deionized water is added to the reaction tank 1, and ammonia water, sodium phosphate solution and a solution containing W, Ni and Al are added to the reaction tank in parallel to perform a gelling reaction. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.5:1, the gelling temperature is maintained at 68°C, the pH value is controlled at 5.5 during the parallel gelling reaction, and the gelling time is controlled at 0.6 hours to generate a precipitate slurry I containing W, Al, Ni and P. Deionized water and castor oil phosphate are added to the reaction tank 2, and the molar ratio of castor oil phosphate to the total number of Ni atoms in the Ni-containing solution is 2.2. The slurry I containing W, Al, Ni, and P, the solution containing Ni, and the ammonia water and sodium phosphate solution are added to the reaction tank 2 in parallel (the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.5:1), the reaction temperature remains unchanged, the reaction time is 1.1 hours, the reaction pH value is controlled at 9.5, and a precipitate slurry containing nickel, tungsten, aluminum, and phosphorus is generated. The resulting slurry is aged at an aging temperature of 87°C. During aging, an equal portion of sodium aluminate solution is first added, and the pH value is controlled to 12.9. After aging for 0.15 hours, the aging pH value is controlled to 9.1. After aging for 0.2 hours, the pH value is then controlled to 5.0, and the aging time is 0.15 hours. The above operation process is repeated 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. Then the washed wet strips are dried at 90°C for 11.0 hours. The dried material was calcined at 530°C for 5 hours to obtain the phosphide catalyst precursor D. Precursor D was heated from room temperature to 450°C in a pure hydrogen atmosphere at a hydrogen flow rate of 400 mL / min and a heating rate of 7°C / min. After being kept at this temperature for 4.0 hours, it was heated to 680°C at a heating rate of 3.5°C / min and kept at this temperature for 5 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 1.8% for 3.5 hours before being exposed to air to obtain the hydrofining catalyst D. The catalyst composition and main physicochemical properties are shown in Table 1.

[0036] Comparative Example 1 According to the preparation method of Example 3 disclosed in CN111822015A, reference agent G, the specific process is as follows: According to the component content ratio of catalyst C in Table 1, nickel nitrate and ammonium metatungstate were added to dissolving tank 1 to prepare mixed solution A, in which the weight concentration of Ni in NiO was 23.4 g / L, and the weight concentration of W in WO3 was 20 g / L. Nickel nitrate was added to dissolving tank 2 to prepare mixed solution B, in which the weight concentration of Ni in NiO was 28 g / L. Tetrapropylammonium bromide and deionized water were added to the reaction tank, the total molar ratio of tetrapropylammonium bromide to tungsten and nickel in mixed solution A was 1.5:1, and sodium metaaluminate solution with a weight concentration of 30 g / L in Al2O3 and mixed solution A were added to the reaction tank in parallel, the gelling temperature was maintained at 53°C, the pH value was controlled at 7.5 during the parallel gelling reaction, and the gelling time was controlled at 1.3 hours to generate precipitate slurry I. The obtained precipitate slurry I was aged under stirring, the stirring speed was 215 rpm, the aging temperature was 72°C, the aging pH value was controlled at 7.1, and the aging time was 0.4 hours. After the aging was completed, solution B, phenylethylamine, and a sodium aluminate solution with a weight concentration of 24 g / L in terms of Al2O3 were added to the slurry I in parallel, the molar ratio of phenylethylamine to nickel in the mixed solution B was 1.3:1, the gelling temperature was maintained at 52°C, the pH value was controlled at 8.7 during the parallel gelling reaction, and the gelling time was controlled at 2.7 hours to obtain precipitate slurry II, hexamethylenediaminetetramethylenephosphonic acid was added to the precipitate slurry II, the molar ratio of hexamethylenediaminetetramethylenephosphonic acid to the transition metal in the finally prepared hydrorefining catalyst was 4.0:1, the stirring speed was 380 rpm, the aging temperature was 75°C, the pH value was controlled at 9.1, the aging time was 4.6 hours, and the obtained material was dried at 160°C for 10 hours, rolled, and extruded into strips. After forming, the catalyst was calcined at 490°C for 6 hours to obtain a phosphide catalyst precursor C. Precursor C was heated from room temperature to 510°C in a hydrogen atmosphere at a hydrogen flow rate of 450 mL / min and a heating rate of 5.8°C / min. After being kept at this temperature for 5 hours, the temperature was increased to 710°C at a heating rate of 3.2°C / min and kept at this temperature for 6 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated for 4 hours with an oxygen volume concentration of 1.1% O2 / N2 passivation gas before contacting the air to obtain a hydrorefining catalyst E, wherein the weight of nickel and tungsten introduced by the mixed solution A accounted for 55% of the weight of nickel and tungsten in the hydrorefining catalyst E, and the weight of Al in the precipitate I accounted for 62% of the weight of Al in the hydrorefining catalyst E. The catalyst composition and main physicochemical properties are shown in Table 1.

[0037] Comparative Example 2 The reference agent F was prepared in the same manner as in Example 1. Aluminum was not added during aging, but was added during the first gelling reaction. The aging pH value was fixed. The specific preparation process was as follows: Ammonium metatungstate, nickel chloride and aluminum chloride solution are added to the dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. The weight concentration of W in the solution containing W, Ni and Al is 40g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 28g / L, and the weight concentration of Al in terms of Al2O3 is 80g / L. Nickel chloride is added to the dissolution tank 2 filled with deionized water to prepare a solution containing Ni. The Ni in the Ni-containing solution accounts for 65% of the total Ni in the obtained hydrorefining catalyst in terms of NiO. Deionized water is added to the reaction tank 1, and ammonia water, sodium phosphate solution and the solution containing W, Ni and Al are added to the reaction tank in parallel to carry out gelation reaction. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.4:1. The gelation temperature is maintained at 60°C. The pH value is controlled at 5.2 during the parallel gelation reaction, and the gelation time is controlled at 0.7 hours to generate a precipitate slurry I containing W, Al, Ni and P. Deionized water and castor oil phosphate are added to the reaction tank 2, and the molar ratio of castor oil phosphate to the total number of Ni atoms in the Ni-containing solution is 2.6. The slurry I containing W, Al, Ni, and P, the Ni-containing solution, and the ammonia water and sodium phosphate solution are added to the reaction tank 2 in parallel (the molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.4:1), the reaction temperature remains unchanged, the reaction time is 1.0 hour, and the reaction pH value is controlled at 8.9 to generate a precipitate slurry containing nickel, tungsten, aluminum, and phosphorus. The resulting slurry is aged at 76°C, the aging pH value is controlled to 8.5, and the aging time is 2.5 hours before the aging is terminated. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. Then the washed wet strips are dried at 80°C for 10.0 hours. The dried material is roasted at 530°C for 5 hours to obtain the phosphide catalyst precursor F. Precursor F was heated from room temperature to 410°C in a pure hydrogen atmosphere at a hydrogen flow rate of 290 mL / min and a heating rate of 6°C / min. After being kept at this temperature for 3.6 hours, it was heated to 710°C at a heating rate of 2.5°C / min and kept at this temperature for 4 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2% for 2 hours before being exposed to air to obtain a hydrorefining catalyst F. The catalyst composition and main physicochemical properties are shown in Table 1.

[0038] Comparative Example 3 The same method as in Example 1 was used to prepare reference agent G., except that aqueous ammonia was used as a precipitant.

[0039] Comparative Example 4 The same method as in Example 1 was used to prepare reference agent H using sodium phosphate solution as a precipitant.

[0040] Comparative Example 5 The same as Example 1, the molar ratio of ammonia water (NH3) to sodium phosphate is 0.75:1, and reference agent I is prepared. Example 5

[0041] This example is an activity evaluation experiment of the catalyst of the present invention, and is compared with the catalyst of the comparative example. The catalysts A, B, C, D of the present invention and the catalysts E, F, G, H, I of the comparative examples are respectively used to conduct comparative evaluation experiments on a 200mL small hydrogenation device. The experimental process is as follows: 60mL of the hydrorefining catalyst is evenly mixed with 340mL of quartz sand and then loaded into a small fixed bed reactor. Hydrogen is introduced into the catalyst before the reaction at 10℃min - 1 The temperature was raised to 660°C at a rate of 1.50 °C and maintained for 40 minutes to remove the surface passivation layer and obtain a fresh hydrotreating catalyst. Catalyst activity evaluation process conditions: hydrogen partial pressure of 6.4 MPa, reaction temperature of 358°C, liquid hourly volume space velocity of 1.8 h -1 The volume ratio of hydrogen to oil is 500:1. The evaluation results are shown in Table 4. The types of nitrides in the hydrorefined oil were detected by gas chromatography-atomic emission spectrometry detector (GC-AED). The results are shown in Table 5.

[0042] From the physicochemical properties and evaluation results of the phosphide catalyst, it can be seen that the catalyst of the present invention has excellent hydrogenation activity, the phosphide particles in the catalyst are small, the phosphide content in the catalyst surface phase is high, and the catalyst is evenly dispersed. It not only has excellent hydrodesulfurization activity and hydrodenitrogenation activity, but also has excellent hydrogenation saturation performance, effectively reducing the aromatic content of heavy distillate oil, and the reduction of polycyclic aromatic hydrocarbons is more obvious. Compared with the reference agent E, the mass content of active metal oxides decreases by 11m%. The catalyst of the present invention is used for processing heavy distillate oil, especially for processing inferior diesel fractions with high aromatic content and great processing difficulty. It has excellent hydrogenation saturation, hydrodesulfurization and hydrodenitrogenation performance, effectively reduces the content of polycyclic aromatic hydrocarbons, and improves the cetane number of diesel.

[0043] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples Catalyst No. A B C D E F G H I <![CDATA[Ni2P,wt%]]> 40 35 44 46 53 40 40 40 40 WP, wt% 20 23 15 12 18 20 20 20 20 <![CDATA[Al2O3,wt%]]> margin margin margin margin margin margin margin margin margin <![CDATA[Specific surface area, m 2 / g]]> 307 301 312 317 273 258 156 299 178 Pore ​​volume, mL / g 0.431 0.420 0.439 0.445 0.383 0.354 0.221 0.419 0.289 Pore ​​distribution, % <6nm 5.32 5.63 5.03 4.89 35.67 47.13 70.36 6.45 57.31 6nm~10nm 55.61 55.42 57.11 57.02 16.85 32.45 16.45 40.12 20.23 10nm~15nm 20.87 20.74 18.67 18.46 37.68 11.25 8.35 32.46 10.15 >15nm 18.20 18.21 19.19 19.63 9.80 9.17 5.84 20.97 12.31 Average particle diameter of transition metal phosphide, nm 4.3 4.2 4.5 4.4 5.3 8.1 7.8 22.1 11.9 Table 2 Ratio of the weight content of active metal oxides on the catalyst surface to the weight content of active metal oxides in the bulk phase Catalyst No. A B C D E F G H I <![CDATA[Surface I Ni2P / Bulk I Ni2P > 5.64 5.45 5.78 5.89 1.22 2.04 1.64 2.14 1.85 <![CDATA[Surface I WP / Bulk I WP > 4.78 4.63 4.88 4.96 1.13 1.35 1.22 1.42 1.31 Table 3 Main properties of crude oil project Analyze the results <![CDATA[Density (20 °C), g / cm 3 > 0.9393 Distillation range, ℃ 162-384 S, µg / g 14980 N, µg / g 898 Aromatics, wt% 72.6 PAHs, wt% 46.8 Cetane number <24 Table 4 Catalyst activity evaluation results Catalyst No. A B C D E F <![CDATA[Generated oil density (20 °C), g / cm 3 > 0.8674 0.8678 0.8672 0.8670 0.8682 0.8768 Distillation range, ℃ 168-368 167-369 167-367 166-366 172-371 180-376 S, µg / g 7.5 8.2 7.0 6.9 9.8 74.3 N, µg / g 4.8 4.2 4.4 4.1 8.5 45.4 Aromatics, wt% 34.7 35.1 34.4 34.0 38.8 46.5 PAHs, wt% 5.0 5.4 4.8 4.6 7.5 16.1 Cetane number 39.1 38.9 39.5 39.8 38.4 30.5 Table 4 Catalyst No. G H I <![CDATA[Generated oil density (20 °C), g / cm 3 > 0.8813 0.8784 0.8801 Distillation range, ℃ 184-379 182-377 185-378 S, µg / g 130.2 98.4 110.7 N, µg / g 77.6 60.8 68.6 Aromatics, wt% 56.3 51.6 53.8 PAHs, wt% 23.4 19.4 21.8 Cetane number, 26.1 29.3 27.8 Table 5 Content of different nitrogen compounds in hydrorefined oil Catalyst No. A B C D E F G H I Nitrogen content in hydrorefined oil, µg / g 4.8 4.2 4.4 4.1 8.5 45.4 77.6 60.8 68.6 1- MCB, µg / g 2.6 2.4 2.5 2.3 4.5 21.8 38.9 31.2 34.3 1,8-BMCB, µg / g 1.2 1.1 1.1 1.1 2.5 15.4 23.3 18.4 21.1 1,4,8-TMCB, µg / g 1.0 0.7 0.8 0.7 1.5 8.2 15.4 11.2 13.2

Claims

1. A hydrotreating catalyst, characterized in that: The catalyst comprises transition metal phosphides and alumina, wherein the total content of transition metal phosphides is 35% to 82%, preferably 38% to 78%, and the content of alumina is 18% to 65%, preferably 22% to 62%, based on the weight of the catalyst; the transition metal phosphides are WP and Ni2P; wherein the ratio of the weight content of Ni2P in the surface phase to the weight content of Ni2P in the bulk phase is 2.5:1 to 7.0:1, preferably 3.0:1 to 6.5:1, and the ratio of the weight content of WP in the surface phase to the weight content of WP in the bulk phase is 2.5:1 to 6.5:1, preferably 3.0:1 to 6.0:

1.

2. The catalyst according to claim 1, characterized in that: The Ni / W molar ratio is 0.1:1-12:1, preferably 0.3:1-10:

1.

3. The catalyst according to claim 1, characterized in that: The average particle diameter of the transition metal phosphide is 2-7 nm, preferably 3-6 nm.

4. The catalyst according to claim 1, characterized in that: The pore size distribution of the hydrotreating catalyst is as follows: the pore volume occupied by pores with a diameter of less than 6 nm accounts for 2% to 10% of the total pore volume, the pore volume occupied by pores with a diameter of 6 to 10 nm accounts for 45% to 67% of the total pore volume, the pore volume occupied by pores with a diameter of 10 to 15 nm accounts for 12% to 35% of the total pore volume, and the pore volume occupied by pores with a diameter of more than 15 nm accounts for 10% to 28% of the total pore volume.

5. A method for preparing the hydrotreating catalyst according to any one of claims 1 to 4, characterized in that The method comprises the following contents: (1) adding a multi-metal solution and a first precipitant to a gelling tank containing bottom water in parallel to carry out a first gelling reaction, thereby obtaining a first slurry; the multi-metal solution is a solution containing W, Ni and Al; the first precipitant is ammonia water and a sodium phosphate solution; (2) adding the first slurry, a nickel-containing solution and a second precipitant to a gelling tank containing bottom water and a phosphate ester compound in parallel to carry out a second gelling reaction, thereby obtaining a second slurry; the second precipitant is ammonia water and a sodium phosphate solution; (3) the second slurry is subjected to multiple pH-changing aging, and a portion of sodium aluminate solution is added during each aging process to obtain a third slurry; (4) the third slurry is filtered, dried, formed, washed, dried and calcined to obtain a phosphide catalyst precursor, and then reduced with hydrogen to obtain a hydrogenation refining catalyst.

6. The method according to claim 5, characterized in that: In the first precipitant and the second precipitant described in step (1) and step (2), the concentration of the aqueous ammonia is 5wt% to 10wt%, the concentration of the sodium phosphate solution is 8wt% to 20wt%, the molar ratio of the aqueous ammonia as NH3 to the sodium phosphate is 0.2:1 to 0.6:1, and the molar ratio of the aqueous ammonia to the sodium phosphate in steps (1) and (2) is the same or different.

7. The method according to claim 5, characterized in that: In the multi-metal solution described in step (1), the weight concentration of W calculated as WO3 is 5 to 140 g / L, preferably 10 to 130 g / L, the weight concentration of Ni calculated as NiO is 5 to 110 g / L, preferably 8 to 105 g / L, and the weight concentration of Al calculated as Al2O3 is 2 to 90 g / L, preferably 6 to 85 g / L.

8. The method according to claim 5, characterized in that: The conditions of the first gelling reaction in step (1) are as follows: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value of the co-current reaction is controlled at 5 to 6, and the reaction time is 0.1 to 1.0 hour.

9. The method according to claim 5, characterized in that: In the nickel-containing solution described in step (2), the weight concentration of Ni in terms of NiO is 10 to 130 g / L, preferably 15 to 115 g / L.

10. The method according to claim 5, characterized in that: The phosphate compound described in step (2) is one or more of octadecyl ether phosphate, alkylphenol ether phosphate, isomeric tridecyl alcohol ether phosphate, lauryl alcohol ether phosphate, castor oil phosphate, octadecyl phosphate, and lauryl phosphate.

11. The method according to claim 5, characterized in that: The molar ratio of the added amount of the phosphate compound to the Ni in the nickel-containing solution is 0.8:1 to 6.0:1, preferably 1.5:1 to 5.5:

1.

12. The method according to claim 5, characterized in that: The conditions of the second gelling reaction in step (2) are as follows: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value is controlled at 8.0 to 10.5 at the end, and the reaction time is 0.5 to 2.5 hours.

13. The method according to claim 5, characterized in that: The multiple pH value changing aging process described in step (3) is as follows: in the first step, a portion of sodium aluminate solution is added dropwise to the second reaction slurry to control the pH value to 11.5-13.5, and the aging is performed for 0.05-0.5 hours; in the second step, the pH value is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; in the third step, the pH value is adjusted to 4.5-6.3, and the aging time is 0.05-0.5 hours; the three-step pH value changing process is repeated multiple times, preferably 2-8 times; the aging temperature is 60-98°C, preferably 65-92°C.

14. The method according to claim 13, characterized in that: During the aging process, except for the use of sodium aluminate solution in the first step of pH adjustment, the other acids and alkalis used to adjust the pH value are inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements.

15. The method according to claim 5, characterized in that: The sodium aluminate solution described in step (3) has a weight concentration of Al in terms of Al2O3 of 5 to 70 g / L. The sodium aluminate solution is divided into equal parts by volume, and the number of parts is the number of times of multiple aging.

16. The method according to claim 5, characterized in that: The Ni added via the Ni-containing solution accounts for 55% to 85% of the total Ni in the resulting hydrotreating catalyst calculated as NiO.

17. The method according to claim 5, characterized in that: The Al added via the sodium aluminate solution accounts for 5% to 55% of the total Al in the resulting hydrorefining catalyst calculated as Al2O3.

18. The method according to claim 5, characterized in that: The roasting conditions in step (4) are as follows: the roasting temperature is 350-700° C., and the roasting time is 1-24 hours.

19. The method according to claim 5, characterized in that: The hydrogen reduction in step (4) adopts programmed temperature reduction, and the specific process includes: the precursor is in a hydrogen atmosphere, the hydrogen purity is greater than 99v%, and the hydrogen flow rate is 150~700mL / min; in the first stage, the temperature is increased from room temperature to 300~550℃ at a rate of 3~10℃ / min, and the temperature is kept constant for 1~5 hours; in the second stage, the temperature is increased to 600~750℃ at a rate of 0.5~5℃ / min, and the temperature is kept constant for 2~8 hours; the heating rate in the second stage is at least 1℃ / min lower than the heating rate in the first stage.

20. Use of the hydrotreating catalyst according to any one of claims 1 to 4 in ultra-deep hydrodesulfurization, denitrogenation and hydrodearomatization of heavy diesel fractions, wherein the aromatic content in the heavy diesel fraction is 50wt% to 85wt% and the cetane number is less than 24.

Citation Information

Patent Citations

  • Hydrocracking catalyst and preparation method thereof

    CN106179463A

  • Preparation method of hydrofining catalyst

    CN110038580A

  • Preparation method of hydrofining catalyst

    CN111822015A

  • Na-Y Molecular Sieve, H-Y Molecular Sieve, and Preparation Methods Thereof, Hydrocracking Catalyst, and Hydrocracking Method

    US20160151771A1

  • Methodsmethod for preparing nickel-cobalt-aluminum precursor material andor positive electrode material with gradient distribution of aluminum element