Preparation method of phosphide hydrofining catalyst

By using a pH stepwise incremental gel-forming reaction and multiple pH adjustments in a co-precipitation method, combined with phosphate compounds and sodium metaaluminate solution, phosphide with high surface phosphide content and small particle size is prepared The catalyst solves the problems of low catalyst pore volume and active metal utilization in the existing technology, and achieves efficient hydrogenation activity and low-cost preparation.

CN118807798AActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310433890.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-22
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

During the preparation process of existing phosphide catalysts by co-precipitation method, the pore volume and specific surface area are small, and the utilization rate of active metal is low, which affects the hydrogenation activity of the catalyst.

Method used

Use W-Ni-Al solution to carry out pH value step-wise incremental gel-forming reaction, add phosphate ester compounds and sodium metaaluminate solution, and form a high surface phosphide content and small particles through multiple pH value adjustments and aging treatments. diameter phosphide catalyst.

Benefits of technology

It improves the hydrogenation activity and metal utilization rate of the catalyst, increases the pore volume and specific surface area, is suitable for hydrodesulfurization and denitrification reactions of heavy diesel, and reduces the cost of catalyst preparation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a phosphide hydrofining catalyst, which comprises the following steps: (1) adding a W-Ni-Al solution into a reaction tank, dropwise adding a mixed precipitant into the reaction tank to carry out pH value increasing gelling reaction, adding a nickel-containing solution in each time of increasing, adding a phosphate compound when the last but one time of increasing is started, and reacting for 2-3 hours; after the gel forming reaction is finished, slurry is obtained; wherein the mixed precipitator is a mixture of ammonia water and a sodium phosphate solution; (2) performing at least two times of pH value decreasing aging on the slurry, and obtaining an aging product after the aging is finished; and (3) preparing the aged product into the phosphide hydrofining catalyst. The catalyst prepared by the method disclosed by the invention is high in surface phase phosphide content, and is suitable for being applied to ultra-deep hydrodesulfurization and denitrification reactions of diesel fractions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a phosphide hydrogenation refining catalyst and a preparation method thereof. Background Art

[0002] At present, crude oil is becoming heavier and inferior, and with the continuous development of the world economy and increasingly stringent environmental regulations, a large amount of light clean fuel needs to be produced. The development and use of ultra-low sulfur or even sulfur-free gasoline and diesel is the trend of clean fuel development worldwide. The development of more active catalysts is an urgent need for oil refining companies. Phosphide catalysts have become a research hotspot as a new type of hydrogenation catalyst. In transition metal phosphides, metal atoms form the smallest structural unit of a triangular prism structure. These triangular prism units form different lattice types in different combinations, and phosphorus atoms occupy the gaps inside the triangular prism. Phosphides are triangular prism units, which are approximately spherical. Phosphides can expose more coordinated unsaturated surface atoms than sulfides, thus having a higher surface active site density.

[0003] CN202110241298.5 A method for preparing a phosphide hydrogenation catalyst, specifically comprising the steps of: (1) preparation of a precursor: mixing a soluble metal salt solution and a dimethyl imidazole solution, and then aging, centrifuging and drying to obtain a precursor; (2) preparation of a catalyst: heating the precursor and sodium hypophosphite to obtain a phosphide hydrogenation catalyst. The present invention adopts a MOF material with well-developed pores as a precursor, and the hydrodesulfurization catalyst prepared by phosphating has a small pore volume and specific surface area, and the hydrogenation activity of heavy raw materials is not significantly improved.

[0004] CN111822015B discloses a method for preparing a hydrorefining catalyst. The method comprises: (1) preparing a mixed solution A and a mixed solution B containing transition metals respectively; (2) adding the mixed solution A and the sodium aluminate alkaline solution to a reaction tank in parallel to carry out a gelling reaction to obtain slurry I, and aging; (3) adding the mixed solution B and the sodium aluminate alkaline solution to the aged slurry I in parallel to carry out a gelling reaction to obtain slurry II, adding an organic phosphorus compound, and aging; (4) drying, shaping, and calcining the obtained material to obtain a phosphide catalyst precursor; (5) reducing the obtained material by hydrogen program temperature rise to obtain a hydrorefining catalyst; the catalyst prepared by this method has more active centers, but its surface metal content is small, and the hydrogenation activity needs to be further improved.

[0005] CN106694004A discloses a transition metal phosphide catalyst and a preparation method thereof, wherein the catalyst is prepared by a coprecipitation-programmed temperature reduction method, wherein the precipitation method is as follows: under stirring, a mixed solution of Mg(NO3)2·6H2O, Al(NO3)3·9H2O and transition metal (Fe, Co and Ni) salts and a precipitant NaOH solution are slowly added dropwise to a Na2HPO4 solution to perform a precipitation reaction. This method directly performs a coprecipitation reaction on the metal solution, which is likely to cause local agglomeration of the active metal, thereby affecting the performance of the catalyst.

[0006] At present, the number of active centers of phosphide catalysts prepared by coprecipitation can be greatly increased. However, compared with supported phosphide catalysts, although the phosphide catalysts prepared by coprecipitation have a high content of active metals, their pore volume and specific surface area are smaller, the phosphide particles are of different sizes, and the content of phosphide in the surface phase is small, which affects the utilization rate of active metals. Therefore, how to improve the pore volume and specific surface area of ​​phosphide catalysts prepared by coprecipitation, increase the content of active metals in the catalyst surface phase, and reduce the size of phosphide grains are the main problems faced by the preparation of phosphide catalysts by coprecipitation. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention provides a method for preparing a phosphide hydrorefining catalyst. The catalyst prepared by the method of the present invention is a bulk hydrogenation catalyst with a high surface phosphide content, more active centers, and a small phosphide grain size, and is suitable for use in ultra-deep hydrodesulfurization and denitrogenation reactions of diesel fractions.

[0008] The preparation method of the phosphide hydrorefining catalyst of the present invention comprises the following contents: (1) adding a W-Ni-Al solution to a reaction tank, dripping a mixed precipitant into the reaction tank to perform a pH value increasing gelling reaction, increasing the pH value by at least 3 times, adding a portion of the nickel-containing solution each time, adding a phosphate compound at the beginning of the penultimate increasing step, and obtaining a slurry after the gelling reaction is completed; wherein the mixed precipitant is a mixture of ammonia water and sodium phosphate solution; (2) The slurry obtained in step (1) is subjected to at least two "pH decreasing aging" processes, wherein the pH decreasing aging process is as follows: in the first step, a portion of sodium aluminate solution is dripped into the slurry, the pH is controlled at 11.5-13.5, and the aging is performed for 0.05-0.5 hours; in the second step, the pH is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; in the third step, the pH is adjusted to 4.5-6.3, and the aging time is 0.05-0.5 hours; after the aging is completed, an aged product is obtained; (3) The aged product is filtered, dried, formed, washed, and calcined to obtain a phosphide catalyst precursor, which is then subjected to a hydrogen programmed temperature reduction to obtain a phosphide hydrogenation refining catalyst.

[0009] In the method of the present invention, the concentration of the aqueous ammonia in step (1) is 5wt% to 10wt%, the weight concentration of the sodium phosphate solution is 8wt% to 20wt%, and the molar ratio of ammonia to sodium phosphate in the mixed precipitant is 0.15:1 to 0.6:1.

[0010] In the method of the present invention, in the W, Ni, Al solution described in step (1), the weight concentration of W calculated as WO3 is 5 to 120 g / L, preferably 10 to 110 g / L, the weight concentration of Ni calculated as NiO is 5 to 90 g / L, preferably 10 to 80 g / L, and the weight concentration of Al calculated as Al2O3 is 2 to 90 g / L, preferably 6 to 85 g / L; wherein, when preparing the solution containing W, Ni, Al, the tungsten source generally used is ammonium metatungstate, the aluminum source is one or more of aluminum nitrate, aluminum sulfate, aluminum chloride and aluminum acetate, and the nickel source generally is one or more of nickel sulfate, nickel nitrate and nickel chloride.

[0011] In the method of the present invention, the pH value increasing interval of the pH value increasing gelation reaction described in step (1) is an initial value of 5.0-6.5 to a final value of 8.0-10.5, and is kept constant for 0.05-0.5 hours after each increase. The pH value increasing increment each time can be the same or different, and preferably the pH value increasing increment is not greater than the last pH increasing increment. At the beginning, the pH value is first adjusted to the initial value using a precipitant.

[0012] In the method of the present invention, the number of increments in step (1) is preferably 4 to 8 times.

[0013] In the method of the present invention, the pH value increasing gelling reaction conditions in step (1) are: reaction temperature is 40-90° C., and reaction time is 0.3-5.0 hours.

[0014] In the method of the present invention, in the nickel-containing solution described in step (1), the weight concentration of Ni in terms of NiO is 5 to 150 g / L, preferably 15 to 145 g / L; when preparing the nickel-containing solution, the nickel source is generally one or more of nickel sulfate, nickel nitrate, and nickel chloride. The number of portions of the nickel-containing solution is the same as the number of pH value increments, and the volume of each portion of the nickel-containing solution added can be the same or different. The Ni added through the nickel-containing solution accounts for 53% to 83% of the total Ni in the obtained hydrorefining catalyst in terms of NiO, preferably 58% to 80%.

[0015] In the method of the present invention, the phosphate compound described in step (1) is one or more of octadecyl ether phosphate (O-5P), alkylphenol ether phosphate (TXP-4, TXP-10), isomeric tridecanol ether phosphate (E-1310P), lauryl alcohol ether phosphate (MOA-3P, MOA-9P), castor oil phosphate, octadecyl phosphate, and lauryl phosphate, preferably one or more of alkylphenol ether phosphate (TXP-4, TXP-10), isomeric tridecanol ether phosphate (E-1310P), lauryl alcohol ether phosphate (MOA-3P, MOA-9P), and castor oil phosphate. The molar ratio of the added amount of the phosphate compound to the Ni in the nickel-containing solution is 0.6:1 to 5.0:1, preferably 1.2:1 to 4.5:1.

[0016] In the method of the present invention, the temperature of the aging process in step (2) is 60 to 98° C., preferably 65 to 92° C.

[0017] In the method of the present invention, the number of "pH decreasing aging" described in step (2) is generally 2 to 8 times. In the aging process, except for the use of sodium aluminate solution in the first step of pH adjustment, the acid and alkali used for adjusting the pH value can be inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements. The inorganic acid can be hydrochloric acid and acetic acid, and the inorganic alkali can be one or more of sodium carbonate, sodium bicarbonate, ammonia water, and sodium hydroxide. The concentration and amount of the acid and alkali solution can be adjusted according to the actual preparation needs.

[0018] In the method of the present invention, the number of portions of the sodium aluminate solution in step (2) is the same as the number of aging times.

[0019] In the method of the present invention, in step (2), the Al added via the sodium aluminate solution accounts for 5% to 50%, preferably 6% to 45%, of the total Al in the obtained hydrorefining catalyst calculated as Al2O3.

[0020] In the method of the present invention, the drying, molding and washing described in step (3) can be carried out by conventional methods in the art. The drying conditions are as follows: drying at 40-150°C for 1-48 hours, preferably drying at 50-120°C for 4-36 hours. During the molding process, conventional molding aids, such as one or more of peptizers, extrusion aids, etc., can be added as needed. The peptizer is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the extrusion aid refers to a substance that is conducive to extrusion molding, such as one or more of sesbania powder, carbon black, graphite powder, citric acid, etc., and the amount of the extrusion aid accounts for 1wt% to 10wt% of the total material dry basis. Washing is generally performed with deionized water or a solution containing decomposable salts (such as ammonium acetate, ammonium chloride, ammonium nitrate, etc.) until neutral.

[0021] In the method of the present invention, the roasting conditions in step (3) are: the roasting temperature is 350-700° C., preferably 400-650° C., and the roasting time is 1-24 hours, preferably 2-12 hours.

[0022] In the method of the present invention, the hydrogen temperature-programmed reduction process described in step (3) is as follows: the precursor is heated from room temperature to 300-550°C under a hydrogen atmosphere with a hydrogen purity greater than 99% by volume, a hydrogen flow rate of 150-700 mL / min, preferably 250-600 mL / min, a heating rate of 3-10°C / min, and maintained at a constant temperature for 1-5 hours. The temperature is then raised to 600-750°C at a heating rate of 0.5-5°C / min and maintained at a constant temperature for 2-8 hours. The heating rate in the second stage is at least 1°C / min lower than that in the first stage, preferably at least 2°C / min lower.

[0023] In the method of the present invention, in order to prevent the phosphide from undergoing a violent oxidation reaction when in contact with air, the prepared catalyst sample is first passivated with O2 / N2 passivation gas with an oxygen volume concentration of 0.5% to 3% for 1 to 5 hours before being exposed to air.

[0024] The hydrorefining catalyst of the present invention is used in ultra-deep hydrodesulfurization, denitrogenation reaction and hydrodearomatization of heavy diesel fractions, wherein the aromatic content in the heavy diesel fraction is 50wt% to 85wt% and the cetane number is less than 24.

[0025] Compared with the prior art, the present invention has the following advantages: 1. The present invention uses a step-by-step pH value gelling method to precipitate a solution containing W, Ni and Al at a specific pH value, thereby preventing the generation of large-particle oxides during the gelling process, and making the active metals dispersed evenly. The addition of a portion of the active metal Ni during the step-by-step pH value increase process is more conducive to the dispersion of the active metals, thereby greatly improving the hydrogenation activity of the catalyst. During the gelling reaction, a phosphate compound is added, which can be used as a phosphorus source and evenly distributed on the catalyst surface. At the same time, due to the increase in the surface active metal content, the addition of the phosphate compound makes the surface active metals in the precursor evenly dispersed. At the same time, the interaction between W, Ni and the carrier is weakened, making W and Ni easy to phosphide, thereby preventing the phosphide from aggregating on the catalyst surface.

[0026] 2. When the catalyst is prepared by the co-precipitation method, a specific molar ratio of ammonia water and sodium phosphate is used to control the properties of the generated materials. The metal oxide particles are small and uniform, which increases the pore volume and specific surface area of ​​the bulk catalyst. The appropriate pore size can improve the diffusion efficiency of the catalytic process.

[0027] 3. In the present invention, the pH value is swung during aging and sodium aluminate solution is added in batches. The pH value swing is used to dissolve amorphous oxides in the oxide particles. The addition of sodium aluminate solution re-modifies the size of the oxide particles. After multiple pH swings, the growth of the oxide particles is controlled to make the oxide particles more uniform and small, exposing more active metals to the surface phase, increasing the macropores in the bulk catalyst and making it easier for macromolecular reactants to pass through the pores. At the same time, the aluminum introduced by the sodium aluminate solution increases the surface hydroxyl groups, further enhancing the adhesion of the oxide, which is beneficial to the catalyst molding.

[0028] The method of the present invention achieves a smaller particle size of phosphide particles in the obtained bulk catalyst by comprehensive control of the preparation steps and preparation conditions, and the active metals in the catalyst surface phase are evenly dispersed, thereby improving the metal utilization rate. The catalyst surface phase has a higher hydrogenation active site, thereby improving the hydrogenation activity for treating heavy oil and reducing the catalyst preparation cost. The method is particularly beneficial to the aromatic saturation of heavy oil, effectively reducing the content of polycyclic aromatic hydrocarbons and improving the cetane number. DETAILED DESCRIPTION

[0029] In the present invention, the specific surface area, pore volume and pore distribution are determined by low-temperature liquid nitrogen adsorption method, the mechanical strength is determined by lateral pressure method, and the diameter of transition metal phosphide particles is determined by TEM technology. In the present invention, wt% is the mass fraction and v% is the volume fraction. The phosphide content of the catalyst surface phase is determined by X-ray photoelectron spectroscopy (XPS), and the phosphide content of the catalyst bulk phase is determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES). First, the surface phase and bulk active metal content of the transition metal oxide of the catalyst precursor of the present invention are determined, and then converted into the transition metal phosphide content in the surface phase and bulk phase of the catalyst. Example 1

[0030] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in the solution containing W, Ni and Al is 42 g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 34.6 g / L, and the weight concentration of Al in terms of Al2O3 is 53.2 g / L. A solution containing Ni is prepared, wherein the Ni in the solution contains 70% of the total Ni in terms of NiO in the obtained hydrorefining catalyst, and the solution is divided into 5 equal parts by volume. The Al in the sodium aluminate solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 5 equal parts by volume. Deionized water is placed in a reaction tank, and the solution containing W, Ni, and Al is placed in the reaction tank. The reaction temperature is 60°C, and ammonia water and sodium phosphate solution are dripped in. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.29:1. The pH value is controlled to 5.5, and ammonia water and sodium phosphate solution are continued to be dripped in. The pH value is adjusted upward 5 times to adjust the final pH value to 9.0 at the end. The pH value is adjusted upward by 0.7 each time. After each increase to the adjusted value, a portion of Ni-containing solution is added. , keep the adjusted pH value of the reaction slurry constant for 10 minutes, add castor oil phosphate at the beginning of the fourth pH increase, the molar ratio of castor oil phosphate to the total number of Ni atoms in the Ni-containing solution is 2.9, generate a precipitate slurry containing nickel, tungsten and aluminum, and age the resulting slurry at an aging temperature of 76°C. During aging, add an equal portion of sodium aluminate solution to control the pH value to 13.1. After aging for 0.15 hours, control the aging pH value to 9.5. After aging for 0.2 hours, then control the pH value to 5.0, and the aging time is 0.2 hours. Repeat the above operation process 5 times to end aging. Filter the aged slurry, dry the filter cake at 100°C for 8 hours, roll it, and extrude it into strips. Wash with deionized water at room temperature until neutral. After washing, dry the molded product at 80°C for 9.0 hours, and calcine the dried material at 530°C for 5 hours to obtain a phosphide catalyst precursor A. Precursor A was heated from room temperature to 430°C in a pure hydrogen atmosphere at a hydrogen flow rate of 320 mL / min and a heating rate of 7°C / min. After being kept at this temperature for 3.0 hours, the temperature was raised to 700°C at a heating rate of 3.0°C / min and kept at this temperature for 5 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2% for 3 hours before being exposed to air to obtain a hydrorefining catalyst A. The catalyst composition and main physicochemical properties are shown in Table 1. Example 2

[0031] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in the solution containing W, Ni and Al is 50 g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 25.2 g / L, and the weight concentration of Al in terms of Al2O3 is 58.5 g / L. A solution containing Ni is prepared, wherein the Ni in the solution containing Ni accounts for 65% of the total Ni in the obtained hydrorefining catalyst in terms of NiO, and the solution is divided into 6 equal parts by volume. The Al in the sodium aluminate solution accounts for 25% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 6 equal parts by volume. Deionized water is placed in a reaction tank, and the solution containing W, Ni, and Al is placed in the reaction tank. The reaction temperature is 65°C, and ammonia water and sodium phosphate solution are dripped in. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.30:1. The pH value is controlled to 5.2, and ammonia water and sodium phosphate solution are continued to be dripped in. The pH value is adjusted up 6 times to adjust the final pH value to 10.0 at the end. The pH value is adjusted up by 0.8 each time. After each adjustment to the adjusted value, a portion of Ni-containing solution is added. The adjusted pH value of the reaction slurry is kept constant for 12 minutes. When the pH value is adjusted up for the fifth time, lauryl alcohol ether phosphate is added. The molar ratio of lauryl alcohol ether phosphate to the total number of Ni atoms in the Ni-containing solution is 2.5, and a precipitate slurry containing nickel, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 80°C. During aging, an equal portion of sodium aluminate solution is first added to control the pH value to 13.3. After aging for 0.2 hours, the aging pH value is controlled at 9.7. After aging for 0.15 hours, the pH value is then controlled to 5.4, and the aging time is 0.2 hours. Repeat the above operation process 6 times to end aging. The aged slurry is filtered, the filter cake is dried at 90°C for 9 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The washed molded product is dried at 80°C for 10.0 hours, and the dried material is roasted at 520°C for 5 hours to obtain a phosphide catalyst precursor B. Precursor B was heated from room temperature to 450°C in a pure hydrogen atmosphere at a hydrogen flow rate of 350 mL / min and a heating rate of 6°C / min. After being kept at this temperature for 3.5 hours, the temperature was raised to 660°C at a heating rate of 3.0°C / min and kept at this temperature for 6 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated for 4 hours with an oxygen volume concentration of 2.5% O2 / N2 passivation gas before contacting air to obtain a hydrorefining catalyst B. The catalyst composition and main physical and chemical properties are shown in Table 1. Example 3

[0032] Ammonium metatungstate, nickel chloride and aluminum chloride are added to the dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in the solution containing W, Ni and Al is 30 g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 34.0 g / L, and the weight concentration of Al in terms of Al2O3 is 50.7 g / L. A solution containing Ni is prepared, wherein the Ni in the solution containing Ni accounts for 63% of the total Ni in the obtained hydrorefining catalyst in terms of NiO, and the solution is divided into 5 equal parts by volume. The Al in the sodium aluminate solution accounts for 35% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 6 equal parts by volume. Deionized water is placed in a reaction tank, and the solution containing W, Ni, and Al is placed in the reaction tank. The reaction temperature is 55°C, and ammonia water and sodium phosphate solution are dripped in. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.28:1. The pH value is controlled to 5.7, and ammonia water and sodium phosphate solution are continued to be dripped in. The pH value is adjusted upward for 5 times, and the final pH value is adjusted to 9.2 at the end. The pH value is increased by 0.7 each time. After each increase to the adjusted value, a portion of Ni-containing solution is added. The pH value of the reaction slurry after adjustment is kept constant for 15 minutes. When the pH value is adjusted for the fourth time, octadecyl ether phosphate is added. The molar ratio of octadecyl ether phosphate to the total number of Ni atoms in the Ni-containing solution is 2.6, and a precipitate slurry containing nickel, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 83°C. During aging, an equal portion of sodium aluminate solution is first added to control the pH value to 12.8. After aging for 0.15 hours, the aging pH value is controlled at 9.8. After aging for 0.15 hours, the pH value is then controlled to 5.3, and the aging time is 0.2 hours. The above operation process is repeated 6 times to end aging. The aged slurry is filtered, the filter cake is dried at 80°C for hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The washed molded product is dried at 110°C for 9.0 hours, and the dried material is roasted at 510°C for 4 hours to obtain a phosphide catalyst precursor C. Precursor C was heated from room temperature to 440°C in a pure hydrogen atmosphere at a hydrogen flow rate of 450 mL / min and a heating rate of 6°C / min. After being kept at this temperature for 3.6 hours, the temperature was raised to 680°C at a heating rate of 3.5°C / min and kept at this temperature for 4 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2.2% for 4 hours before being exposed to air to obtain a hydrorefining catalyst C. The catalyst composition and main physicochemical properties are shown in Table 1. Example 4

[0033] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in the solution containing W, Ni and Al is 46 g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 20.0 g / L, and the weight concentration of Al in terms of Al2O3 is 53.6 g / L. A solution containing Ni is prepared, wherein the Ni in the solution containing Ni accounts for 73% of the total Ni in the obtained hydrorefining catalyst in terms of NiO, and the solution is divided into 6 equal parts by volume. The Al in the sodium aluminate solution accounts for 33% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 5 equal parts by volume. Deionized water is placed in a reaction tank, and the solution containing W, Ni, and Al is placed in the reaction tank. The reaction temperature is 68°C, and ammonia water and sodium phosphate solution are dripped in. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.38:1. The pH value is controlled to 5.2, and ammonia water and sodium phosphate solution are continued to be dripped in. The pH value is adjusted up 6 times to adjust the final pH value to 8.8 at the end. The pH value is adjusted up by 0.6 each time. After each increase to the adjusted value, a portion of Ni-containing solution is added to adjust the pH value. The pH value of the reaction slurry is kept constant for 13 minutes. When the pH value is adjusted up for the fifth time, isomeric tridecanol ether phosphate is added. The molar ratio of isomeric tridecanol ether phosphate to the total number of Ni atoms in the Ni-containing solution is 2.7, and a precipitate slurry containing nickel, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 82°C. During aging, an equal portion of sodium aluminate solution is first added to control the pH value to 13.0. After aging for 0.2 hours, the aging pH value is controlled at 9.3. After aging for 0.15 hours, the pH value is then controlled to 4.8, and the aging time is 0.15 hours. Repeat the above operation process 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 110°C for 7 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The washed molded product is dried at 85°C for 9.5 hours, and the dried material is roasted at 540°C for 4 hours to obtain a phosphide catalyst precursor D. Precursor D was heated from room temperature to 450°C in a pure hydrogen atmosphere at a hydrogen flow rate of 380 mL / min and a heating rate of 6°C / min. After being kept at this temperature for 4.0 hours, the temperature was raised to 690°C at a heating rate of 3.2°C / min and kept at this temperature for 6 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated for 4 hours with an oxygen volume concentration of 2.2% O2 / N2 passivation gas before being exposed to air to obtain a hydrorefining catalyst D. The catalyst composition and main physicochemical properties are shown in Table 1.

[0034] Comparative Example 1 According to the preparation method of Example 3 of CN111822015A, reference agent G, the specific process is as follows: According to the component content ratio of catalyst C in Table 1, nickel nitrate and ammonium metatungstate were added to dissolving tank 1 to prepare mixed solution A, in which the weight concentration of Ni in NiO was 23.4 g / L, and the weight concentration of W in WO3 was 20 g / L. Nickel nitrate was added to dissolving tank 2 to prepare mixed solution B, in which the weight concentration of Ni in NiO was 28 g / L. Tetrapropylammonium bromide and deionized water were added to the reaction tank, the total molar ratio of tetrapropylammonium bromide to tungsten and nickel in mixed solution A was 1.5:1, and sodium metaaluminate solution with a weight concentration of 30 g / L in Al2O3 and mixed solution A were added to the reaction tank in parallel, the gelling temperature was maintained at 53°C, the pH value was controlled at 7.5 during the parallel gelling reaction, and the gelling time was controlled at 1.3 hours to generate precipitate slurry I. The obtained precipitate slurry I was aged under stirring, the stirring speed was 215 rpm, the aging temperature was 72°C, the aging pH value was controlled at 7.1, and the aging time was 0.4 hours. After the aging was completed, solution B, phenylethylamine, and a sodium aluminate solution with a weight concentration of 24 g / L in terms of Al2O3 were added to the slurry I in parallel, the molar ratio of phenylethylamine to nickel in the mixed solution B was 1.3:1, the gelling temperature was maintained at 52°C, the pH value was controlled at 8.7 during the parallel gelling reaction, and the gelling time was controlled at 2.7 hours to obtain precipitate slurry II, hexamethylenediaminetetramethylenephosphonic acid was added to the precipitate slurry II, the molar ratio of hexamethylenediaminetetramethylenephosphonic acid to the transition metal in the finally prepared hydrorefining catalyst was 4.0:1, the stirring speed was 380 rpm, the aging temperature was 75°C, the pH value was controlled at 9.1, the aging time was 4.6 hours, and the obtained material was dried at 160°C for 10 hours, rolled, and extruded into strips. After forming, the catalyst was calcined at 490°C for 6 hours to obtain a phosphide catalyst precursor C. Precursor C was heated from room temperature to 510°C in a hydrogen atmosphere at a hydrogen flow rate of 450 mL / min and a heating rate of 5.8°C / min. After being kept at this temperature for 5 hours, the temperature was increased to 710°C at a heating rate of 3.2°C / min and kept at this temperature for 6 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated for 4 hours with an oxygen volume concentration of 1.1% O2 / N2 passivation gas before contacting air to obtain a hydrorefining catalyst E, wherein the weight of nickel and tungsten introduced by the mixed solution A accounted for 55% of the weight of nickel and tungsten in the hydrorefining catalyst E, and the weight of Al in the precipitate I accounted for 62% of the weight of Al in the hydrorefining catalyst E. The catalyst composition and main physicochemical properties are shown in Table 1.

[0035] Comparative Example 2 The reference agent F was prepared in the same manner as in Example 1. All the sodium aluminate solution was added at once during the aging process of the precipitate slurry containing nickel, tungsten and aluminum. The aging pH value was fixed. The specific preparation process was as follows: Ammonium metatungstate, nickel chloride and aluminum chloride are added to the dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al, wherein the weight concentration of W in the solution containing W, Ni and Al is 42 g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 34.6 g / L, and the weight concentration of Al in terms of Al2O3 is 53.2 g / L. A solution containing Ni is prepared, wherein the Ni in the solution containing Ni accounts for 70% of the total Ni in the obtained hydrorefining catalyst in terms of NiO, and the solution is divided into 5 equal parts by mass. Al in the sodium aluminate solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst. Deionized water is placed in the reaction tank, and the solution containing W, Ni, and Al is placed in the reaction tank. The reaction temperature is 60°C, and ammonia water and sodium phosphate solution are dripped in. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.29:1. The pH value is controlled to 5.5, and ammonia water and sodium phosphate solution are continued to be dripped in. The pH value is adjusted up 5 times, and the final pH value is adjusted to 9.0 at the end. The pH value is adjusted up each time. The values ​​are all 0.7. After each adjustment to the adjusted value, a portion of Ni-containing solution is added. The adjusted pH value of the reaction slurry is kept constant for 10 minutes. When the pH value is adjusted for the fourth time, castor oil phosphate is added. The molar ratio of castor oil phosphate to the total number of Ni atoms in the Ni-containing solution is 2.9, and a precipitate slurry containing nickel, tungsten and aluminum is generated. The resulting slurry is aged at an aging temperature of 76°C. During aging, all sodium aluminate solution is added, and the aging pH value is controlled at 8.5. The aging time is 2 hours, and the aging is terminated. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The washed molded product is dried at 80°C for 9.0 hours, and the dried material is calcined at 530°C for 5 hours to obtain a phosphide catalyst precursor F. Precursor F was heated from room temperature to 430°C in a pure hydrogen atmosphere at a hydrogen flow rate of 320 mL / min and a heating rate of 7°C / min. After being kept at this temperature for 3.0 hours, the temperature was raised to 700°C at a heating rate of 3.0°C / min and kept at this temperature for 5 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2% for 3 hours before being exposed to air to obtain a hydrorefining catalyst F. The catalyst composition and main physicochemical properties are shown in Table 1.

[0036] Comparative Example 3 The reference agent J was prepared in the same manner as in Example 1. During the preparation process, nickel was added to all the W, Ni, and Al solutions, and no Ni-containing solution was prepared. The gelling reaction was no longer performed with a pH value increasing stepwise, but was performed at a fixed pH value. The specific preparation process is as follows: Ammonium metatungstate, nickel chloride and aluminum chloride are added to the dissolution tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. The weight concentration of W in the solution containing W, Ni and Al is 42g / L in terms of WO3, the weight concentration of Ni in terms of NiO is 82.0g / L, and the weight concentration of Al in terms of Al2O3 is 53.2g / L. The Al in the sodium metaaluminate solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrorefining catalyst, and it is divided into 5 equal parts by volume. Deionized water is placed in the reaction tank, and the solution containing W, Ni and Al is placed in the reaction tank. The reaction temperature is 60°C, and ammonia water and sodium phosphate solution are added dropwise. The molar ratio of ammonia to sodium phosphate in the ammonia water and sodium phosphate solution is 0.25:1. At the end, the pH value is controlled to be 8.0, the reaction time is 2.0 hours, castor oil phosphate is added at the end, the molar ratio of castor oil phosphate to the total number of Ni atoms in the solution containing W, Ni, and Al is 2.0, and a precipitate slurry containing nickel, tungsten, and aluminum is generated. The resulting slurry is aged at an aging temperature of 76°C. During aging, an equal portion of sodium aluminate solution is first added to control the pH value to 13.1. After aging for 0.15 hours, the aging pH value is controlled to 9.5. After aging for 0.2 hours, the pH value is then controlled to 5.0, and the aging time is 0.2 hours. Repeat the above operation process 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The washed molded product is dried at 80°C for 9.0 hours, and the dried material is roasted at 530°C for 5 hours to obtain a phosphide catalyst precursor G. Precursor G was heated from room temperature to 430°C in a pure hydrogen atmosphere at a hydrogen flow rate of 320 mL / min and a heating rate of 7°C / min. After being kept at this temperature for 3.0 hours, the temperature was raised to 700°C at a heating rate of 3.0°C / min and kept at this temperature for 5 hours. In order to prevent the phosphide from having a violent oxidation reaction when in contact with air, the catalyst sample was passivated with an O2 / N2 passivation gas with an oxygen volume concentration of 2% for 3 hours before being exposed to air to obtain a hydrorefining catalyst G. The catalyst composition and main physical and chemical properties are shown in Table 1.

[0037] Comparative Example 4 The same method as in Example 1 was used to prepare reference agent H., except that aqueous ammonia was used as a precipitant.

[0038] Comparative Example 5 The same method as in Example 1 was used to prepare reference agent I, except that sodium phosphate solution was used as a precipitant.

[0039] Comparative Example 6 The same method as in Example 1 was used, except that the molar ratio of ammonia water (calculated as NH3) to sodium phosphate was 0.8:1, and reference agent J was prepared. Example 5

[0040] This example is an activity evaluation experiment of the catalyst of the present invention, and is compared with the catalyst of the comparative example. The catalysts A, B, C, D of the present invention and the catalysts E, F, G, H, I, J of the comparative examples are respectively used to conduct comparative evaluation tests on a 200mL small hydrogenation device. The experimental process is as follows: 60mL of the hydrorefining catalyst is evenly mixed with 340mL of quartz sand and then loaded into a small fixed bed reactor. Hydrogen is introduced into the catalyst before the reaction at 10℃min - 1 The temperature was raised to 660 °C at a rate of 1.5 °C and maintained for 40 minutes to remove the surface passivation layer and obtain a fresh hydrotreating catalyst. Catalyst activity evaluation process conditions: hydrogen partial pressure of 6.4 MPa, reaction temperature of 358 °C, liquid hourly volume space velocity of 1.8 h -1 The volume ratio of hydrogen to oil is 500:1. The evaluation results are shown in Table 3. The types of sulfides and nitrides in the hydrorefined oil were detected by gas chromatography-atomic emission spectrometry detector (GC-AED). The results are shown in Tables 4 and 5.

[0041] From the evaluation results, it can be seen that the catalyst of the present invention has excellent hydrogenation activity, the phosphide particles in the catalyst are small, the phosphide in the surface phase is abundant, and the dispersion is high. It not only has excellent hydrodesulfurization activity and hydrodenitrogenation activity, but also has excellent hydrogenation saturation performance, effectively reducing the aromatic content of heavy distillate oil, and the reduction of polycyclic aromatic hydrocarbon content is more obvious. The catalyst of the present invention is used for processing heavy distillate oil, especially for processing low-quality diesel fractions with high aromatic content and high processing difficulty. It has excellent hydrogenation saturation, hydrodesulfurization and hydrodenitrogenation performance, effectively reduces the content of polycyclic aromatic hydrocarbons, and improves the cetane number of diesel.

[0042] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples Catalyst No. A B C D E F <![CDATA[Ni2P,wt%]]> 41 36 46 37 53 41 WP, wt% 21 25 15 23 18 21 <![CDATA[Al2O3,wt%]]> margin margin margin margin margin margin <![CDATA[Specific surface area, m 2 / g]]> 318 313 325 331 273 254 Pore ​​volume, mL / g 0.446 0.437 0.458 0.464 0.383 0.349 Pore ​​distribution <4nm 5.83 6.43 5.01 4.51 8.92 17.58 4 nm~6 nm 4.45 5.46 4.24 3.92 26.75 30.68 6 nm~10 nm 58.31 57.62 58.47 58.96 16.85 30.12 10 nm~15 nm 16.21 15.01 16.61 16.89 37.68 10.44 >15 nm 15.20 14.48 15.67 15.72 9.80 11.18 Average particle diameter of transition metal phosphide, nm 4.5 4.7 4.3 4.4 5.3 14.5 Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples Catalyst No. G H I J <![CDATA[Ni2P,wt%]]> 41 41 41 41 WP, wt% 21 21 21 21 <![CDATA[Al2O3,wt%]]> margin margin margin margin <![CDATA[Specific surface area, m 2 / g]]> 230 168 308 197 Pore ​​volume, mL / g 0.338 0.245 0.435 0.298 Pore ​​distribution <4nm 19.23 41.24 3.42 30.21 4nm~6nm 33.54 28.62 5.19 23.52 6nm~10nm 26.42 17.13 39.42. 20.12 10nm~15nm 10.89 7.98 23.32 12.40 >15nm 9.92 5.03 28.65 13.75 Average particle diameter of transition metal phosphide, nm 15.2 7.9 24.5 10.8 Table 2 The weight ratio of active metal oxides on the catalyst surface to that in the bulk phase Catalyst No. A B C D E F <![CDATA[Surface I Ni2P / Bulk I Ni2P > 5.91 5.62 5.74 5.85 1.22 2.04 <![CDATA[Surface I WP / Bulk I WP > 4.84 4.71 4.78 4.80 1.13 1.35 Table 2: Ratio of the weight content of active metal oxides on the catalyst surface to that in the bulk phase Catalyst No. G H I J <![CDATA[Surface I Ni2P / Bulk I Ni2P > 2.15 1.52 2.29 1.76 <![CDATA[Surface I WP / Bulk I WP > 1.49 1.18 1.58 1.34 Table 3 Main properties of crude oil project Analyze the results <![CDATA[Density (20 °C), g / cm 3 > 0.9393 Distillation range, ℃ 162-384 S, µg / g 14980 N, µg / g 898 Aromatics, wt% 72.6 PAHs, wt% 46.8 Cetane number <24 Table 4 Catalyst activity evaluation results Catalyst No. A B C D E F <![CDATA[Generated oil density (20 °C), g / cm 3 > 0.8672 0.8676 0.8672 0.8670 0.8682 0.8781 Distillation range, ℃ 166-368 168-369 164-367 163-366 172-371 179-377 S, µg / g 7.0 8.0 6.6 6.0 9.8 80.1 N, µg / g 4.0 4.4 3.8 3.5 8.5 49.7 Aromatics, wt% 34.1 34.8 33.8 33.6 38.8 47.9 PAHs, wt% 4.6 5.2 4.4 4.2 7.5 17.3 Cetane number 39.4 38.7 39.7 39.9 38.1 30.1 Table 4 Catalyst No. G H I J <![CDATA[Generated oil density (20 °C), g / cm 3 > 0.8788 0.8813 0.8804 0.8809 Distillation range, ℃ 182-378 184-382 182-377 183-380 S, µg / g 89.1 154.3 101.2 131.8 N, µg / g 54.8 85.8 62.3 73.6 Aromatics, wt% 48.4 60.7 52.4 57.7 PAHs, wt% 18.2 23.2 19.9 23.2 Cetane number, 29.5 25.2 28.0 25.2 Table 5 Content of different nitrogen compounds in hydrorefined oil Catalyst No. A B C D E F Nitrogen content in hydrorefined oil, µg / g 4.0 4.4 3.8 3.5 8.5 49.7 1- MCB, µg / g 1.9 2.0 1.8 1.7 3.9 22.9 1,8-BMCB, µg / g 1.5 1.3 1.5 1.4 2.7 16.8 1,4,8-TMCB, µg / g 0.6 0.7 0.5 0.4 1.9 10.0 Table 5 Content of different nitrogen compounds in hydrorefined oil Catalyst No. G H I J Nitrogen content in hydrorefined oil, µg / g 54.8 85.8 62.3 73.6 1- MCB, µg / g 24.8 40.2 27.4 35.1 1,8-BMCB, µg / g 17.8 25.4 19.3 22.4 1,4,8-TMCB, µg / g 12.2 20.2 15.6 16.1

Claims

1. A method for preparing a phosphide hydrorefining catalyst, characterized in that The method comprises the following contents: (1) adding W-Ni-Al solution into a reaction tank, dripping a mixed precipitant into the reaction tank to perform a pH value increasing gelling reaction, increasing the pH value by at least 3 times, adding a portion of nickel-containing solution each time, adding a phosphate compound at the beginning of the penultimate increasing step, and obtaining a slurry after the gelling reaction is completed; wherein the mixed precipitant is a mixture of ammonia water and sodium phosphate solution; (2) the slurry obtained in step (1) is subjected to at least two "pH value decreasing aging" steps, and the pH value decreasing aging process is as follows: in the first step, dripping a portion of sodium aluminate solution into the slurry, controlling the pH value at 11.5-13.5, and aging for 0.05-0.5 hours; in the second step, adjusting the pH value to 8.5-10.5, and aging for 0.05-0.5 hours; in the third step, adjusting the pH value to 4.5-6.3, and aging for 0.05-0.5 hours; after the aging is completed, obtaining an aging product; (3) The aged product is filtered, dried, formed, washed, and calcined to obtain a phosphide catalyst precursor, which is then subjected to a hydrogen programmed temperature reduction to obtain a phosphide hydrogenation refining catalyst.

2. The method according to claim 1, characterized in that: The concentration of the aqueous ammonia in step (1) is 5wt% to 10wt%, the weight concentration of the sodium phosphate solution is 8wt% to 20wt%, and the molar ratio of ammonia to sodium phosphate in the mixed precipitant is 0.15:1 to 0.6:

1.

3. The method according to claim 1, characterized in that: In the W, Ni and Al solution described in step (1), the weight concentration of W calculated as WO3 is 5 to 120 g / L, preferably 10 to 110 g / L, the weight concentration of Ni calculated as NiO is 5 to 90 g / L, preferably 10 to 80 g / L, and the weight concentration of Al calculated as Al2O3 is 2 to 90 g / L, preferably 6 to 85 g / L.

4. The method according to claim 1, characterized in that: The pH value increasing range of the pH value increasing gelling reaction in step (1) is from an initial value of 5.0 to 6.5 to a final value of 8.0 to 10.5, and is kept constant for 0.05 to 0.5 hours after each increase. The increment of the pH value each time is the same or different.

5. The method according to claim 1, characterized in that: The pH value increment shall not be greater than the previous pH value increment.

6. The method according to claim 1, characterized in that: The number of increments in step (1) is 4 to 8 times.

7. The method according to claim 1, characterized in that: The pH value increasing gelling reaction conditions in step (1) are: reaction temperature of 40-90° C., and reaction time of 0.3-5.0 hours.

8. The method according to claim 1, characterized in that: In the nickel-containing solution described in step (1), the weight concentration of Ni in terms of NiO is 5 to 150 g / L; the number of portions of the nickel-containing solution is the same as the number of times the pH value is increased, the volume of each portion of the nickel-containing solution added is the same or different, and the Ni added through the nickel-containing solution accounts for 53% to 83% of the total Ni in the obtained hydrorefining catalyst in terms of NiO.

9. The method according to claim 1, characterized in that: The phosphate compound described in step (1) is one or more of octadecyl ether phosphate, alkylphenol ether phosphate, isomeric tridecyl alcohol ether phosphate, lauryl alcohol ether phosphate, castor oil phosphate, octadecyl phosphate, and lauryl phosphate; the molar ratio of the added amount of the phosphate compound to the Ni in the nickel-containing solution is 0.6:1 to 5.0:

1.

10. The method according to claim 1, characterized in that: The temperature of the aging process in step (2) is 60-98°C, preferably 65-92°C.

11. The method according to claim 1, characterized in that: The number of "pH decreasing aging" described in step (2) is 2 to 8 times; in the aging process, except for the use of sodium aluminate solution in the first step of pH adjustment, the acids and bases used for adjusting the pH value are inorganic salts, inorganic acids and inorganic bases that do not contain aluminum elements.

12. The method according to claim 1, characterized in that: The number of portions of sodium aluminate solution in step (2) is the same as the number of aging times.

13. The method according to claim 1, characterized in that: In step (2), the Al added via the sodium aluminate solution accounts for 5% to 50% of the total Al in the obtained hydrotreating catalyst calculated as Al2O3.

14. The method according to claim 1, characterized in that: The calcination conditions in step (3) are as follows: the calcination temperature is 350-700° C., preferably 400-650° C., and the calcination time is 1-24 hours, preferably 2-12 hours.

15. The method according to claim 1, characterized in that: The hydrogen programmed temperature reduction process described in step (3) is as follows: the precursor is placed in a hydrogen atmosphere with a hydrogen purity greater than 99v%, a hydrogen flow rate of 150-700mL / min, a heating rate of 3-10°C / min, and is heated from room temperature to 300-550°C. After being kept constant for 1-5 hours, the temperature is then raised to 600-750°C at a heating rate of 0.5-5°C / min and kept constant for 2-8 hours.

16. The method according to claim 1, characterized in that: Before the prepared phosphide hydrorefining catalyst contacts the air, it is first passivated with O2 / N2 passivation gas having an oxygen volume concentration of 0.5% to 3% for 1 to 5 hours.

Citation Information

Patent Citations

  • Preparation method of hydrofining catalyst

    CN111822015A

  • Hydrofining catalyst and preparation method thereof

    CN112619676A

  • Preparation method of hydrofining catalyst

    CN114433116A

  • Hydro-refining catalyst, carrier for use therein and method for production thereof

    US20040186014A1