Non-noble metal dehydrogenation catalyst as well as preparation method and application thereof
Through the combination of non-noble metal transition metals and non-metallic or rare earth metals on the carrier, the problems of low selectivity and short life of the existing catalysts are solved, an efficient and economical LOHCs addition and dehydrogenation process is achieved, the service life of the catalyst is extended and Reduce side effects.
Patent Information
- Application Number
- CN202310390753.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-22
AI Technical Summary
Existing LOHCs addition and dehydrogenation catalysts have problems such as low selectivity, many side reactions, and short lifespan, resulting in poor hydrogen purity and increased costs, making it difficult to achieve long-cycle cyclic addition and dehydrogenation applications.
Non-noble transition metals A and B are combined with non-metal or rare earth metal C and loaded on a specific carrier. The catalyst is prepared through a simple one-pot method, using dispersants and synergistic effects to improve the activity and selectivity of the catalyst and reduce side reactions. .
It realizes the efficient addition and dehydrogenation process of LOHCs, improves the stability and selectivity of the catalyst, reduces the cost, extends the service life of the catalyst, and achieves ultra-long sustainable recycling application.
Smart Images

Figure BDA0004175639860000071
Abstract
Description
Technical Field
[0001] The invention belongs to the field of dehydrogenation catalysts, and particularly relates to a non-precious metal dehydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] The basis of the "hydrogen economy" is to use hydrogen as a new clean energy for storage, transportation, and power generation. Therefore, hydrogen needs to be produced in tons. Traditional hydrogen storage and transportation technologies such as high-pressure gaseous hydrogen storage, low-temperature liquefied hydrogen storage, and solid hydrogen storage restrict the application of hydrogen energy due to high costs and safety requirements. Organic liquid hydrogen storage materials (LOHCs) are a type of hydrogen storage material with a fully reversible hydrogenation-dehydrogenation cycle. In recent years, they have become the focus of hydrogen research due to their reversibility and zero CO2 emissions. The principle is to achieve hydrogen storage (chemical bonding) through the reversible reaction and hydrogenation reaction of unsaturated liquid organic matter such as olefins, alkynes or aromatic hydrocarbons and hydrogen, and to achieve hydrogen release through dehydrogenation reactions, making hydrogen storage and release safe and efficient. Since the hydrogenated Hn-LOHCs compounds have similar properties to crude oil derivatives (such as diesel and gasoline), they can be transported over long distances using existing liquid fuel transportation logistics (such as pipelines, ships, and trucks). Therefore, it is very feasible to transition to the "hydrogen economy" with existing infrastructure.
[0003] Organic liquid hydrogen storage materials mainly include traditional organic liquid hydrogen storage materials and new organic liquid hydrogen storage materials. Traditional organic liquid hydrogen storage molecules are mainly aromatic benzene-cyclohexane, toluene-methylcyclohexane, naphthalene-decalin, dibenzyltoluene-perhydrodibenzyltoluene systems. Such traditional organic liquid hydrogen storage molecules can change the properties of organic compounds by changing the number of substituents, bridging methods, etc. At present, there are still problems such as high temperature required for the dehydrogenation process and easy occurrence of side reactions such as cracking and disproportionation, resulting in reduced purity of the generated hydrogen. New organic liquid hydrogen storage materials are mainly condensed aromatic molecules containing heteroatoms (O, N, S), among which N-heterocyclic systems such as quinoline and its derivatives, indole and its derivatives, carbazole and its derivatives are the most studied new organic liquid hydrogen storage materials. The hydrogen storage capacity is usually expressed in mass fraction (wt%), and the reaction enthalpy ΔH in kJ / mol H2 represents the energy value released in the hydrogenation reaction, and the energy value required in the dehydrogenation reaction. For example, the dehydrogenation temperature of methylcyclohexane used by Chiyoda in Japan is as high as 350℃~400℃. The selection of LOHCs with more than 4wt% hydrogen storage and low reaction enthalpy (-15kcal / mol H2≤ΔH≤-10kcal / mol H2) has low external energy demand, and the hydrogen storage capacity can meet most of the actual needs, thereby improving the overall efficiency of the dehydrogenation process and facilitating the industrial application of the hydrogen energy industry chain.
[0004] The key to realizing the hydrogenation and dehydrogenation of LOHCs is to add dehydrogenation catalysts. Catalysts can not only reduce the reaction temperature, but also improve the reaction rate of chemical hydrogen storage technology. The hydrogenation and dehydrogenation of LOHCs are reversible reactions. They follow Le Chatelier's principle. Hydrogenation releases heat and dehydrogenation absorbs heat. By changing the temperature, pressure and concentration of the reactants, the equilibrium direction of the reaction can be effectively controlled to move toward hydrogenation or dehydrogenation. Under pressurized conditions, the catalyst adsorbs LOHCs, causing the unsaturated bonds to vibrate and break, and H2 is added; under normal pressure conditions, the catalyst adsorbs Hn-LOHCs, CH vibrates and breaks, and H2 is removed.
[0005] The essence of the hydrogenation and dehydrogenation process is the bond vibration breaking to achieve H2 storage and release. In theory, it can catalyze hydrogenation and dehydrogenation at the same time, but because the hydrogenation and dehydrogenation reaction pathways are opposite, based on cost, yield and other considerations, the choice of catalyst is generally different. Hydrogenation catalysts mainly include nickel catalysts, palladium and platinum catalysts, ruthenium catalysts and rhodium catalysts. Conventional hydrogenation catalysts are nickel metal catalysts with aluminum as the carrier, while for deep aromatics catalysis, precious metal catalysts are the first choice. Dehydrogenation catalysts are mainly precious metal catalysts, non-precious metal catalysts and mixed catalysts. Precious metal catalysts have high activity and can improve the dehydrogenation efficiency of organic liquid hydrogen storage materials. In theory, catalysts that can be used for hydrogenation can also be used for dehydrogenation, but in fact, the reaction pathways of hydrogenation and dehydrogenation processes are opposite, so it is very demanding to meet the requirements of catalysts for both hydrogenation and dehydrogenation processes. Most of the applicable bifunctional catalysts are based on precious metals as the main components, mostly for the research of Pt, Pd, and Ir, and are rarely used in practice. Hydrogenation and dehydrogenation bifunctional catalysts based on non-precious metal elements have not been used.
[0006] The currently commonly used LOHCs dehydrogenation catalysts have problems such as low selectivity, many side reactions, and short life, which lead to large LOHCs losses, increased costs, and poor hydrogen purity. To address these problems, we have improved the LOHCs dehydrogenation catalysts by selecting suitable systems, additives, and preparation methods to effectively improve the activity and selectivity, reduce side reactions, and realize the long-term cyclic dehydrogenation application of LOHCs. Summary of the invention
[0007] The purpose of the present invention is to provide a non-precious metal dehydrogenation catalyst and a preparation method and application thereof in view of the defects of the prior art.
[0008] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a non-precious metal dehydrogenation catalyst, wherein the catalyst is two different transition metals A and B combined or coordinated with a non-metal or rare earth metal C and loaded on a carrier; the mass ratios of components A, B, and C to the carrier are 10% to 80%, 1% to 50%, and 0.1% to 5%, respectively.
[0009] Furthermore, transition metal A is Cr, Mn, Fe, Co, Ni or Cu, transition metal B is Cr, Mn, Fe, Ni, Cu, Zn, Zr, Nb, Mo or W, and C is one of non-metal B, C, N, P, Cl, Br, I or rare earth metals Y, La, Ce.
[0010] Furthermore, the carrier is a powder with a particle size of 2 μm to 150 μm and a specific surface area of 200 to 850 m 2 / g, average pore size: 5-15nm, pore volume: 0.35-1.5cm 3 / g.
[0011] Furthermore, the carrier is a mixture of one or more of a silica-alumina carrier and a carbon-containing material carrier, the silica-alumina carrier is Al2O3 powder, SiO2 molecular sieve, pseudo-boehmite, silica-alumina dry gel powder, ZIFs, ZSM-5 molecular sieve, Beta molecular sieve, X-type molecular sieve, Y-type molecular sieve or A-type molecular sieve, and the carbon-containing material carrier is graphene, carbon nanotubes, activated carbon powder, g-C3N4, MOFs or COFs.
[0012] A method for preparing the above-mentioned non-precious metal dehydrogenation catalyst comprises the following steps:
[0013] (1) Weighing soluble salts of A, B, and C in proportion, adding a solvent, dissolving them, and mixing them to obtain a mixed solution of active components;
[0014] (2) adding a dispersant to the mixed solution, stirring at a constant temperature of 40 to 100° C. for 30 min to 12 h to obtain a colloidal solution;
[0015] (3) The carrier is made into powder and added to the colloidal liquid. The mixture is stirred at a constant temperature of 60°C to 200°C for 8h to 72h and aged for 1h to 24h to obtain a paste mixture of the active component and the carrier. The mixture is dried, calcined in an inert atmosphere, and crushed to obtain a powder loaded with the active component. The powder can be used as a catalyst after molding or directly reduced and passivated.
[0016] Furthermore, the solvent in step (1) is one or a mixture of two or more of ionized water, ethanol, ethylene glycol, hydrochloric acid, nitric acid or ammonia water.
[0017] Furthermore, the dispersant in step (2) is a water-soluble organic matter, a surfactant, or a mixture of one or more of a sol, wherein the water-soluble organic matter is polyvinyl pyrrolidone, thiourea, dicyandiamide propanol, butanol or ethylene glycol, and the surfactant is dodecyldimethylbenzyl ammonium chloride, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, polyquaternium-16, polyethylene glycol octylphenyl ether, dodecanol polyoxyethylene ether, tridecanol polyoxyethylene ether, nonylphenol polyoxyethylene ether, alkylphenol polyoxyethylene ether, polyether F127 or polyether P123; the sol is silica sol or aluminum sol; and the amount of the dispersant added is 10% to 500% of the carrier mass.
[0018] Furthermore, the drying temperature in step (3) is 40°C to 150°C, and the drying time is 30min to 36h; the inert gas atmosphere is a nitrogen or argon atmosphere, the roasting temperature is 200 to 800°C, the roasting time is 1h to 24h, and the heating rate is 1 to 6°C / min; the reduction conditions are: reduction temperature 200 to 600°C, hydrogen atmosphere, hydrogen content in the hydrogen atmosphere is 10% to 100%, and the passivation conditions are: room temperature dilute oxygen atmosphere, oxygen content in the oxygen atmosphere is 0.1% to 15%.
[0019] An application of the above non-precious metal dehydrogenation catalyst in a reversible hydrogenation hydrogen storage system.
[0020] Furthermore, the reversible hydrogenation hydrogen storage system includes one or a mixture of two or more π-conjugated reversible hydrogenation hydrogen storage materials; the π-conjugated reversible hydrogenation hydrogen storage material, at 25°C and 1atm, releases 10 to 15 kcal of heat per 1 mol of H2 stored, that is, -15 kcal / mol H2≤ΔH≤-10 kcal / mol H2; and the hydrogen storage density after complete hydrogenation is greater than 4% of the mass of the hydrogen storage material; the π-conjugated reversible hydrogenation hydrogen storage material is solid or liquid, and has a melting point of less than 80°C.
[0021] The catalyst powder can be used directly after reduction, or it can be reduced after grinding, screening and molding and then used in the actual dehydrogenation reaction process. The molding shape can be determined according to demand.
[0022] Application method:
[0023] The prepared modified carrier-loaded noble metal dehydrogenation catalyst can be used for hydrogenation of a reversible hydrogenation hydrogen storage system and dehydrogenation of its hydrogenation product.
[0024] Application example: Taking fixed bed and reactor applications as examples, the hydrogenation raw material and dehydrogenation raw material are respectively N-ethylcarbazole and fully hydrogenated N-ethylcarbazole as examples, but the actual application is not limited to this;
[0025] Fixed bed hydrogenation reaction conditions: liquid space velocity: 0.3 / h~5.0 / h, reaction temperature: 120℃~280℃, reaction pressure: 2Mpa~9Mpa, hydrogenation conversion rate can reach more than 99%, complete hydrogenation product 60%~98%, stable cycle time can reach 10000h.
[0026] Reactor hydrogenation conditions: The ratio of catalyst to reversible hydrogenation storage system is 1:5-1:50, reaction temperature is 120℃-300℃, reaction pressure is 2Mpa-9Mpa, reaction time is 2h-12h, hydrogenation conversion rate can reach more than 99%, and complete hydrogenation product is 90%-99%
[0027] Fixed bed dehydrogenation reaction conditions: liquid space velocity: 0.3 / h~5.0 / h, reaction temperature 140℃~280℃, reaction pressure less than 3Mpa, dehydrogenation conversion rate can reach more than 99%, complete dehydrogenation product 60%~98%, stable cycle time can reach 10000h.
[0028] Reactor dehydrogenation conditions: The ratio of catalyst to reversible hydrogenation storage system is 1:5-1:50, reaction temperature is 140℃-280℃, reaction pressure is normal pressure, reaction time is 1h-12h, hydrogenation conversion rate can reach more than 99%, and complete dehydrogenation product is 70%-99%.
[0029] Application object requirements
[0030] 1. The reversible hydrogenation hydrogen storage system is one or more π-conjugated reversible hydrogenation hydrogen storage materials; or a combination of one or more π-conjugated reversible hydrogenation hydrogen storage materials and other substances, and the other substances are regarded as solvents or auxiliary materials that do not participate in hydrogenation and dehydrogenation;
[0031] 2. The π-conjugated reversible hydrogenation hydrogen storage material is characterized in that: it is a π-conjugated compound, and at 25°C and 1atm, the heat released by the π-conjugated compound for storing 1 mol of H2 is 10-15kcal, that is, -15kcal / mol H2≤ΔH≤-10kcal / mol H2; and the hydrogen storage density after complete hydrogenation should be greater than 4wt%; the dehydrogenation of LOHCs within the reaction enthalpy range has low external energy demand, avoiding excessive energy required for the dehydrogenation process, and the hydrogen storage density range is conducive to actual industrial application. If the hydrogen storage density is too low, the actual application efficiency will deteriorate.
[0032] Non-precious metals are cheap, but their activity is lower than that of precious metals. They are generally used in high quantities and are difficult to prepare using simple methods.
[0033] The non-precious metal dehydrogenation catalyst prepared by the present invention has the following advantages:
[0034] (1) A simple one-pot method is adopted, which is simple, economical and produces less wastewater;
[0035] (2) Using the viscosity of the dispersant to highly disperse the components and evenly load them onto the carrier, thus avoiding the aggregation and growth of grains;
[0036] (3) The combination of components A and B utilizes the synergistic effect of non-precious metals, which greatly reduces costs and makes the activity comparable to or even better than that of precious metals. Side reactions are reduced, and the system can operate stably for a long time. Moreover, it can be activated and regenerated under certain conditions, and its performance can be restored to more than 98% of its initial state, thus achieving ultra-long-term sustainable use and recycling. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiment of the present application will be clearly and completely described below in combination with the embodiment of the present application. Obviously, the described embodiment is only a part of the embodiment of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present application.
[0038] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or apparatuses.
[0039] Example 1
[0040] 1. Weigh component A containing 80g of soluble salt of Cu (such as copper nitrate, copper chloride), component B containing 10g of soluble salt of Zr (such as copper nitrate, copper chloride), component C containing 3g of soluble substance of B (such as boric acid), add water and ethanol to dissolve to obtain a mixed impregnation solution.
[0041] 2. Add 10 g ethylene glycol, 30 g thiourea and 2 g polyquaternium-16 to the mixed impregnation solution, stir at a constant temperature of 40°C for 8 h to obtain a colloidal solution.
[0042] 3. Add 100 g of Al2O3 powder to the colloidal liquid, stir at a constant temperature of 40°C for 12 hours, age for 12 hours to obtain a paste mixture of the active component and the carrier, dry at 65°C for 18 hours, calcine at 600°C in an inert atmosphere for 8 hours, and heat at a rate of 1°C / min. Grind to obtain a powder loaded with the active component.
[0043] 4. The catalyst powder can be used directly after reduction, or it can be used in the actual dehydrogenation reaction process after grinding, sieving, molding, and reduction. The molding shape can be determined according to the needs. In this embodiment, the catalyst powder is molded into microspheres with a diameter of 2 mm, and then nitrogen is replaced, reduced at 600°C in a 10% hydrogen atmosphere for 6 hours, and passivated in a 0.5% oxygen atmosphere for 10 hours to obtain the catalyst product CuZr-B / Al2O3.
[0044] Example 2
[0045] 1. Weigh component A containing 60g of Ni soluble salt (such as nickel nitrate, nickel chloride), component B containing 20g of Cu soluble salt (such as copper nitrate, copper chloride), component C containing 3g of N soluble substance (such as soluble azide salt), add water to dissolve and obtain a mixed impregnation solution.
[0046] 2. Add 10g polyvinyl pyrrolidone, 20g dicyandiamide, and 2g polyether F127 to the mixed impregnation solution, stir at a constant temperature of 60°C for 5h to obtain a colloidal solution.
[0047] 3. Add 90g SiO2 powder and 10g activated carbon to the colloidal liquid, stir at a constant temperature of 80℃ for 8h, age for 18h to obtain a paste mixture of active component and carrier, dry at 65℃ for 18h, calcine at 600℃ in inert atmosphere for 4h, heat at a rate of 2℃ / min, and grind to obtain a powder loaded with active component.
[0048] 4. The catalyst powder can be used directly after reduction, or it can be used in the actual dehydrogenation reaction process after grinding, sieving, molding, and reduction. The molding shape can be determined according to the needs. In this embodiment, the catalyst powder is molded into microspheres with a diameter of 2 mm, and then nitrogen is replaced, reduced at 600°C in a 10% hydrogen atmosphere for 6 hours, and passivated in a 0.5% oxygen atmosphere for 10 hours to obtain the catalyst product NiCu-N / SiO2.
[0049] Example 3
[0050] 1. Weigh component A containing 60g of soluble salt of Co (such as nickel nitrate, nickel chloride), component B containing 2g of soluble salt of Cr (such as copper nitrate, copper chloride), component C containing 3g of soluble substance of Br (such as bromic acid), add water to dissolve and obtain a mixed impregnation solution.
[0051] 2. Add 10g polyvinyl pyrrolidone, 20g dicyandiamide, and 2g polyether F127 to the mixed impregnation solution, stir at a constant temperature of 60°C for 5h to obtain a colloidal solution.
[0052] 3. Add 90g SiO2 powder and 10g activated carbon to the colloidal liquid, stir at a constant temperature of 80℃ for 8h, age for 18h to obtain a paste mixture of active component and carrier, dry at 65℃ for 18h, calcine at 600℃ in inert atmosphere for 4h, heat at a rate of 2℃ / min, and grind to obtain a powder loaded with active component.
[0053] 4. The catalyst powder can be used directly after reduction, or it can be used in the actual dehydrogenation reaction process after grinding, sieving, molding, and reduction. The molding shape can be determined according to the needs. In this embodiment, the catalyst powder is molded into microspheres with a diameter of 2 mm, and then nitrogen is replaced, reduced at 600°C in a 10% hydrogen atmosphere for 6 hours, and passivated in a 0.5% oxygen atmosphere for 10 hours to obtain the catalyst product CoCr-Br / SiO2.
[0054] Comparative Example 1
[0055] 1. Weigh component A containing 60g of Ni soluble salt (such as nickel nitrate, nickel chloride) and component B containing 20g of Cu soluble salt (such as copper nitrate, copper chloride), add water to dissolve, stir at a constant temperature of 60°C for 5h to obtain a mixed impregnation solution.
[0056] 2. Add 90g SiO2 powder and 10g activated carbon to the mixed impregnation solution, stir at a constant temperature of 80℃ for 8h, age for 18h to obtain a mixture of active components and carriers, dry at 65℃ for 18h, calcine at 600℃ in an inert atmosphere for 4h, heat at a rate of 2℃ / min, and grind to obtain a powder loaded with active components.
[0057] 3. The catalyst powder can be used directly after reduction, or it can be used in the actual dehydrogenation reaction process after grinding, sieving, molding, and reduction. The molding shape can be determined according to the needs. For the convenience of comparison, the catalyst powder was also molded into microspheres with a diameter of 2 mm, and then nitrogen replaced, reduced at 600°C for 6 hours in a 10% hydrogen atmosphere, and passivated in a 0.5% oxygen atmosphere for 10 hours to obtain the catalyst product NiCu / SiO2.
[0058] Comparative Example 2
[0059] 1. Weigh component A containing 80g of Ni soluble salt (such as nickel nitrate, nickel chloride) and component C containing 3g of N soluble substance (such as soluble azide salt), add water to dissolve, stir at a constant temperature of 60℃ for 5h to obtain a mixed impregnation solution.
[0060] 2. Add 90g SiO2 powder and 10g activated carbon to the mixed impregnation solution, stir at a constant temperature of 80℃ for 8h, age for 18h to obtain a mixture of active components and carriers, dry at 65℃ for 18h, calcine at 600℃ in an inert atmosphere for 4h, heat at a rate of 2℃ / min, and grind to obtain a powder loaded with active components.
[0061] 3. The catalyst powder can be used directly after reduction, or it can be used in the actual dehydrogenation reaction process after grinding, sieving, molding, and reduction. The molding shape can be determined according to the needs. For the convenience of comparison, the catalyst powder was also molded into microspheres with a diameter of 2 mm, and then nitrogen replaced, reduced at 600°C for 6 hours in a 10% hydrogen atmosphere, and passivated in a 0.5% oxygen atmosphere for 10 hours to obtain the catalyst product Ni-N / SiO2.
[0062] Catalyst dehydrogenation cycle test: N-ethylcarbazole system was selected, and two fixed bed reactors were used for hydrogenation and dehydrogenation respectively. The raw material N-ethylcarbazole was first hydrogenated, and the first dehydrogenation used the N-ethylcarbazole hydrogenation product, and the second hydrogenation used the dehydrogenation product, and so on, to achieve the dehydrogenation cycle, liquid space velocity: 0.3 / h, hydrogenation: 200℃, 7MPa, dehydrogenation: 220℃ normal pressure. The values in Table 1 are the lowest values in the cycle process.
[0063] Table 1
[0064]
[0065] By comparison, it can be found that the catalyst using bimetallic synergy without introducing confined components has very poor stability, the catalyst using confined components but not introducing bimetallic synergy has very poor conversion rate and selectivity, and there are many side reactions, but the stability is improved. The catalyst dehydrogenation conversion rate, selectivity and life of the catalyst are greatly improved by introducing component B to construct bimetallic synergy and component C confinement.
[0066] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A non-precious metal dehydrogenation catalyst, characterized in that: The catalyst is two different transition metals A and B combined or coordinated with one C of nonmetal or rare earth metal and loaded on a carrier; the mass ratios of components A, B and C to the carrier are 10% to 80%, 1% to 50% and 0.1% to 5% respectively.
2. The dehydrogenation catalyst according to claim 1, characterized in that: The transition metal A is Cr, Mn, Fe, Co, Ni or Cu, the transition metal B is Cr, Mn, Fe, Ni, Cu, Zn, Zr, Nb, Mo or W, and C is one of non-metal B, C, N, P, Cl, Br, I or rare earth metals Y, La, Ce.
3. The non-precious metal dehydrogenation catalyst according to claim 1, characterized in that: The carrier is powder with a particle size of 2 μm to 150 μm and a specific surface area of 200 to 850 m 2 / g, average pore diameter: 5-15nm, pore volume: 0.35-1.5cm 3 / g.
4. The non-precious metal dehydrogenation catalyst according to claim 1, characterized in that: The carrier is a mixture of one or more of a silicon-aluminum carrier and a carbon-containing material carrier, wherein the silicon-aluminum carrier is Al2O3 powder, SiO2 molecular sieve, pseudo-boehmite, silicon-aluminum dry glue powder, ZIFs, ZSM-5 molecular sieve, Beta molecular sieve, X-type molecular sieve, Y-type molecular sieve or A-type molecular sieve, and the carbon-containing material carrier is graphene, carbon nanotubes, activated carbon powder, g-C3N4, MOFs or COFs.
5. A method for preparing the non-precious metal dehydrogenation catalyst according to any one of claims 1 to 4, characterized in that The following steps are involved: (1) Weighing soluble salts of A, B, and C in proportion, adding a solvent, dissolving them, and mixing them to obtain a mixed solution of active components; (2) adding a dispersant to the mixed solution, stirring at a constant temperature of 40 to 100° C. for 30 min to 12 h to obtain a colloidal solution; (3) The carrier is made into powder and added to the colloidal liquid. The mixture is stirred at a constant temperature of 60°C to 200°C for 8h to 72h and aged for 1h to 24h to obtain a paste mixture of the active component and the carrier. The mixture is dried, calcined in an inert atmosphere, and crushed to obtain a powder loaded with the active component. The powder can be used as a catalyst after molding or directly reduced and passivated.
6. The preparation method according to claim 5, characterized in that: The solvent in step (1) is one or a mixture of two or more of ionized water, ethanol, ethylene glycol, hydrochloric acid, nitric acid or ammonia water.
7. The preparation method according to claim 5, characterized in that: The dispersant in step (2) is one or a mixture of two or more of a water-soluble organic matter, a surfactant, and a sol, wherein the water-soluble organic matter is polyvinyl pyrrolidone, thiourea, dicyandiamide propanol, butanol or ethylene glycol, and the surfactant is dodecyl dimethyl benzyl ammonium chloride, hexadecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium bromide, polyquaternium-16, polyethylene glycol octylphenyl ether, dodecanol polyoxyethylene ether, tridecanol polyoxyethylene ether, nonylphenol polyoxyethylene ether, alkylphenol polyoxyethylene ether, polyether F127 or polyether P123; the sol is silica sol or aluminum sol; and the amount of the dispersant added is 10% to 500% of the carrier mass.
8. The preparation method according to claim 5, characterized in that: The drying temperature in the step (3) is 40°C to 150°C, and the drying time is 30min to 36h; the inert gas atmosphere is a nitrogen or argon atmosphere, the roasting temperature is 200 to 800°C, the roasting time is 1h to 24h, and the heating rate is 1 to 6°C / min; the reduction conditions are: a reduction temperature of 200 to 600°C, a hydrogen atmosphere, and the hydrogen content of the hydrogen atmosphere is 10% to 100%; the passivation conditions are: a dilute oxygen atmosphere at room temperature, and the oxygen content of the oxygen atmosphere is 0.1% to 15%.
9. Use of the non-precious metal dehydrogenation catalyst according to any one of claims 1 to 4 in a reversible hydrogenation hydrogen storage system.
10. The use according to claim 9, characterized in that: The reversible hydrogenation hydrogen storage system comprises one or a mixture of two or more π-conjugated reversible hydrogenation hydrogen storage materials; the π-conjugated reversible hydrogenation hydrogen storage material releases 10 to 15 kcal of heat per 1 mol H2 stored at 25°C and 1 atm, i.e. -15 kcal / mol H2≤ΔH≤-10 kcal / molH2; The hydrogen storage density after complete hydrogenation is greater than 4% of the mass of the hydrogen storage material; the π-conjugated reversible hydrogenated hydrogen storage material is solid or liquid, and has a melting point of less than 80°C.
Citation Information
Patent Citations
Method for preparing high-purity hydrogen by using non-noble metal dehydrogenation catalyst
CN111892019A
Nano confinement nickel-based catalyst as well as preparation method and application thereof
CN113559907A
Catalyst for hydrogenation and dehydrogenation of organic hydrogen storage liquid, preparation method of catalyst and hydrogenation and dehydrogenation method of organic hydrogen storage liquid
CN114700084A
Supported non-noble metal catalyst with high catalytic hydrogenation activity as well as preparation method and application thereof
CN114917907A
Catalyst for dehydrogenating organic hydrogen storage raw material, carrier for catalyst, hydrogen storage alloy, and method for providing high purity hydrogen
US20220258133A1