Method for preparing graphene oxide-based solid-liquid composite super-smooth surface through ultrafast laser texturing-dry film coating
By using ultrafast laser texturing technology to prepare a graphene oxide-based solid-liquid composite ultra-slippery surface on a metal substrate, the problems of existing SLIPS in terms of wear resistance, antifouling, liquid repellency and anti-icing properties have been solved, and a higher level of performance has been achieved. Long service life and lower preparation costs simplify the process.
Patent Information
- Application Number
- CN202410444220.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-22
AI Technical Summary
Existing super-slippery surfaces (SLIPS) are prone to defects due to external force damage, environmental erosion and long-term use, resulting in lubricant loss, short service life, high construction costs, and complex preparation processes, making it difficult to meet the needs of large-scale equipment and mass production.
Ultrafast laser texturing technology is used to prepare a rough structure on a metal substrate, and a graphene oxide coating is sprayed, combined with an organosilane sol binder and perfluoropolyether lubricant, to form a graphene oxide-based solid-liquid composite ultra-smooth surface.
It significantly improves the wear resistance, anti-fouling, liquid-repellent and anti-icing properties of the ultra-slippery surface, extends the service life, reduces the preparation cost, simplifies the process flow, and maintains the chemical stability of the lubricant and the reduction of the friction coefficient.
Smart Images

Figure CN118808092A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a graphene oxide-based solid-liquid composite ultra-smooth surface by ultrafast laser texturing-dry film coating, and belongs to the technical field of special processing and surface engineering. Background Art
[0002] Slippery liquid infused porous surfaces (SLIPS) have the characteristics of low friction coefficient and high fluidity. They can not only reduce surface roughness and friction resistance, but also show good anti-wear and anti-icing and anti-fouling properties. They are a new type of protective surface with special wetting function and have broad research prospects in the fields of marine protection, medical devices, anti-fouling and anti-icing, microfluidic manipulation, etc. Since Aizenberg et al. first prepared a slippery liquid infused porous surface (SLIPS) inspired by Nepenthes in 2011, SLIPS has attracted widespread attention due to its special wetting and flow characteristics. A large number of researchers use methods including electrospinning, chemical etching, and photolithography to construct rough structures on the substrate, and then graft or directly infuse lubricants into the rough structures to prepare superslippery surfaces. However, in actual production applications, SLIPS still has some problems that need to be solved: 1) The rough structure of the substrate is prone to defects under the action of external force damage, long-term service, environmental erosion, etc., resulting in the loss of the lubricant stored therein, which causes the service life of SLIPS to be reduced. 2) Although the lubricant stored in the rough structure of SLIPS has a certain degree of chemical inertness, the diffusion of molecules is always ongoing, and the lubricant is in contact with the environmental medium for a long time. The lubricant will be lost due to factors such as entrainment of the external medium, fluid shear, and volatilization, affecting the long-term service of SLIPS. 3) The construction cost of the rough structure of SLIPS is high and time-consuming, which limits its application in large-scale equipment or mass production.
[0003] In order to solve the above problems that SLIPS encounters during service, relevant researchers have proposed to prepare SLIPS by constructing a coating on a substrate to improve the stability of the rough structure and lubricant of SLIPS. Liu et al. prepared SLIPS with excellent liquid-repellent properties by spin coating a polytetrafluoroethylene suspension on various substrates and then infusing perfluoropolyether. After being damaged by various mechanical loads, the liquid repellency of SLIPS still exists. Gaurav et al. constructed SLIPS on a methylated SiO2 porous coating. After multiple mechanical load stimulations, the rough structure was destroyed and SLIPS lost its liquid repellency. The SLIPS prepared by Liu et al., which mimics the structure of human skin, reduced the ice adhesion strength due to its excellent self-lubricating properties. However, as the number of deicing increases, the ice adhesion strength continues to increase, and SLIPS loses its anti-deicing performance.
[0004] Although researchers at home and abroad have prepared super-slippery surfaces by different methods and applied them in the fields of liquid repellency and anti-fouling, wear resistance and anti-icing, the SLIPS prepared at present still have problems such as poor surface oil film stability, complex rough structure preparation, and easy destruction of the structure under mechanical load. Therefore, the present invention first laser textures the rough structure on the metal substrate, then sprays the graphene oxide coating, and then pours the lubricant to prepare the super-slippery surface. Graphene oxide can enhance the wear resistance of SLIPS, and directly laser texturing on the metal substrate can enhance the mechanical properties of the structure. The synergistic effect of the two greatly improves the long-term service performance of SLIPS. The SLIPS prepared by the present invention has excellent wear resistance, anti-fouling and liquid repellency and anti-icing properties. Summary of the invention
[0005] The present invention aims to develop a method for preparing a graphene oxide-based solid-liquid composite super-smooth surface by ultrafast laser texturing-dry film coating, firstly using an organic silane coupling agent to react with silica sol in a wet chemical reaction to obtain an organic silane sol binder, using an ultrafast laser to prepare a rough structure on the metal surface, then mixing graphene oxide, organic silane sol binder, and fluorinated organic silane modifier and spraying them onto the textured metal surface, and finally pouring lubricating oil to prepare a super-smooth surface. The graphene oxide-based solid-liquid composite super-smooth surface prepared by the present invention can meet the requirements of wear resistance, anti-fouling, liquid repellency and anti-icing of metal substrates, and has a simple processing technology and high stability.
[0006] The purpose of the present invention is to provide a method for preparing a graphene oxide-based solid-liquid composite super-smooth surface by laser texturing.
[0007] In order to achieve the purpose of the present invention, the technical solution adopted is:
[0008] A method for preparing a graphene oxide-based solid-liquid composite super-slippery surface by ultrafast laser texturing-dry film coating comprises the following steps:
[0009] Step 1: Preparation of textured metal sheet:
[0010] Pre-treating the metal sheet, and performing laser texturing on the pre-treated metal sheet to obtain a textured metal sheet;
[0011] Step 2: Preparation of organosilane sol binder:
[0012] Deionized water is added to the silica sol solution, and the mixed solution is dispersed in a n-propanol solvent, and finally an organic silane coupling agent is slowly added to obtain an organic silane sol binder after sufficient reaction;
[0013] Step 3: Preparation of fluorinated modified graphene oxide hydrophobic coating:
[0014] The graphene oxide is dispersed in anhydrous ethanol, and the organosilane sol binder obtained in step 2 is compounded with the graphene oxide solution, and then a fluorinated organosilane modifier is added. After sufficient ultrasonic stirring and mixing, the mixture is sprayed on the surface of the textured metal sheet described in step 1. Finally, the fluorinated modified graphene oxide hydrophobic coating is obtained after curing in an oven.
[0015] Step 4: Immerse the fluorinated modified graphene oxide hydrophobic coating obtained in step 3 in perfluoropolyether lubricating oil, place it in a vacuum box and filter it for a certain period of time to obtain a laser textured graphene oxide-based graphene oxide-based solid-liquid composite super-smooth surface.
[0016] In one embodiment of the present invention, the metal sheet in step one includes one or more of a magnesium sheet, an aluminum sheet, and a titanium sheet.
[0017] In one embodiment of the present invention, the pretreatment described in step one is to polish the metal sheet with sandpaper of 100, 200, 500, 1000, 2000 and 5000 meshes in sequence, then immerse it in anhydrous ethanol for ultrasonic treatment for 1 hour to remove the particles generated during polishing, and finally pickle it with dilute hydrochloric acid to remove the oxide film on the surface of the metal sheet.
[0018] In one embodiment of the present invention, the laser used in the laser texturing in step 1 is one or more of a picosecond laser and a femtosecond laser.
[0019] In one embodiment of the present invention, the processing parameters of the laser texturing in step 1 are a laser energy density of 0.5-5 J / cm 2 , frequency 1KHz-1MHz, pulse width 500-2000ps, scanning times 1-25 times, scanning speed 50-200mm / s.
[0020] In one embodiment of the present invention, the laser texturing pattern in step 1 is one or more of a discrete pit structure, a continuous groove structure, and a bionic structure. The discrete pit structure is one or more of a circle, a rhombus, a rectangle, an ellipse, a triangle, and a hexagon; the continuous groove structure includes one or more of a straight line, a sinusoid, a mesh, and a rhombus; and the bionic structure is a fish scale texture.
[0021] In one embodiment of the present invention, the solvent in step 2 is n-propanol.
[0022] In one embodiment of the present invention, the organic silane coupling agent in step 2 includes one or more of octyltriethoxysilane, methyltriethoxysilane, decyltriethoxysilane, vinyltriethoxysilane, and methylpropyltriethoxysilane.
[0023] In one embodiment of the present invention, the mass ratio of the deionized water, silica sol, solvent and organic silane coupling agent in step 2 is 0.1-3:1:0.5-5:0.5-8.
[0024] In one embodiment of the present invention, the mass ratio of the graphene oxide to anhydrous ethanol in step three is 1:5-20.
[0025] In one embodiment of the present invention, the mass ratio of the organosilane sol binder, the graphene oxide solution and the fluorine-containing organosilane modifier in step three is 1-10:1:0.05-2.
[0026] In one embodiment of the present invention, the sufficient ultrasonic stirring in step three is ultrasonic treatment for 5-30 minutes and magnetic stirring for 5-30 minutes.
[0027] In one embodiment of the present invention, the oven curing temperature in step three is 60-200° C., and the curing time is 0.5-8 h.
[0028] In one embodiment of the present invention, the fluorine-containing organic silane modifier described in step three includes one or more of perfluorododecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, perfluorododecyltrimethoxysilane, and perfluorodecyltriethoxysilane.
[0029] In one embodiment of the present invention, the filtration air pressure in step 4 is -100 kPa.
[0030] In one embodiment of the present invention, the perfluoropolyether lubricant in step 4 includes one or more of krytox GPL-103 perfluoropolyether lubricant, krytox GPL-101 perfluoropolyether lubricant, Fomblin YL VAC 25 / 6 perfluoropolyether lubricant, and Fomblin YL VAC14 / 6 perfluoropolyether lubricant.
[0031] Beneficial effects of the present invention:
[0032] (1) The metal substrate of the graphene oxide-based solid-liquid composite super-smooth surface prepared by the present invention can not only improve the hardness after laser texturing, but also provide a storage site for the lubricant, which plays a protective role for the lubricant stored therein; the fluorinated organic silane can improve the chemical affinity of the coating surface to the perfluoropolyether lubricant. After deionized water flushing, shear force test, brush friction, and various oil film stability tests, the graphene oxide-based solid-liquid composite super-smooth surface still maintains liquid repellency.
[0033] (2) The present invention uses graphene oxide as a protective coating for the textured metal substrate. The photothermal properties of graphene oxide enable the super-slippery surface to slide and fall off ice at a light intensity of only 10 degrees. This has an excellent passive de-icing function. At the same time, as a typical two-dimensional material, graphene oxide has good tribological properties. The friction coefficient of the prepared graphene oxide-based solid-liquid composite super-slippery surface is reduced by 70% compared with the original surface.
[0034] (3) The present invention uses perfluoropolyether as a lubricant for the graphene oxide-based solid-liquid composite super-slippery surface. Its good chemical stability enables organic reagents with different surface tensions to slide on its surface.
[0035] In the anti-fouling test, the ultra-smooth surface was immersed in yogurt, coffee, ketchup, and honey for 5 seconds and then taken out. There was no residue on the surface, showing excellent anti-fouling performance. DETAILED DESCRIPTION
[0036] In order to more clearly understand the technical content of the present invention, the following embodiments are given in detail, the purpose of which is only to better understand the content of the present invention but not to limit the protection scope of the present invention.
[0037] Examples of what is included in the claims
[0038] Test method:
[0039] Surface morphology observation: The morphology of the particles was observed using a scanning electron microscope (SEM), a laser spectral confocal microscope, a transmission electron microscope (TEM), and an ultra-depth-of-field microscope.
[0040] Chemical composition test: X-ray photoelectron spectroscopy (XPS), X-ray energy dispersive spectroscopy (EDS), Raman spectroscopy, and X-ray diffraction (XRD) are used to test the chemical composition of particles.
[0041] Surface oil film stability test: The prepared super-slip sample was placed on a desktop glue coating machine for spin coating (KW-4T, Institute of Microelectronics, Chinese Academy of Sciences, 300rpm), and the mass loss of the lubricant on the sample surface was measured every 10 seconds; the sample was rinsed with deionized water (height 10cm), and the mass loss of the sample was weighed after each 10ml of deionized water was rinsed. After the spin coating and deionized water flushing test, the sliding angle was measured. The super-slip surface was rubbed with a brush, and the oil film loss and sliding angle change were measured every 10 times. Each sample was tested five times, and the average value was taken to calculate the standard deviation.
[0042] Self-healing test: Use a brush to rub the super-slippery surface and measure the sliding angle. Then put it in an oven and heat it at 60 degrees Celsius for 1 minute before measuring its sliding angle.
[0043] Liquid repellency test: The static contact angle and sliding angle of the coating were measured using a JC2000DM contact angle meter (Shanghai Zhongchen Digital Technology Co., Ltd.). The test liquid volume was 10 microliters, and the contact angle was read after the droplet fell onto the coating. The sample inclination angle of the rotating table was then changed, and the angle at which the droplet began to slide was the sliding angle of the droplet. Each sample was tested five times, and the average value was taken and the standard deviation was calculated.
[0044] Tribological performance test: The friction coefficient of different samples was tested using a pin-on-disc friction and wear tester (Anton Pear TRB3). The surface hardness of the coating was measured using a 200HVS-5 digital microhardness tester. The surface morphology of the sample after friction was observed using an ultra-depth of field microscope (OLYMPUSDSX1000), and the wear loss was calculated based on the three-dimensional profile.
[0045] Antifouling performance test: The prepared super-smooth surface was immersed in liquids such as yogurt, honey, coffee, ketchup, etc. for 5 seconds, then taken out and the residual liquid on the surface was observed.
[0046] Anti-icing and de-icing performance test: A self-built refrigeration station, a digital push-pull force gauge (HP-200) and a xenon light source system (CEL-S500) were used to characterize the anti-icing and de-icing performance. The sample was placed on a cooling table and cooled to -20°C at 50% humidity, and then a 20-microliter drop of water was dropped on the surface of the sample. The freezing time was monitored and recorded with a camera. The sample was cooled to -20 degrees Celsius on a cooling table with 50% humidity, and then an ice column with a diameter of 10 mm and a height of 40 mm was placed on the surface of the sample. The ice column was pushed down with a thrust measurement device and the ice adhesion strength of the ice column was measured. A xenon light source system was used to simulate 1 sun illumination intensity to study the photothermal de-icing characteristics of the sample. The ice adhesion strength of 20 de-icing cycles was measured to characterize its anti-icing durability.
[0047] Coating mechanical properties test: According to GB / T 9286-1998 standard, a grid scratch test was carried out to test the bonding strength of the Mxene coating. A Vickers hardness tester (200HVS-5) was used to measure the hardness of the graphene oxide-based solid-liquid composite super-slippery surface.
[0048] Example 1
[0049] A method for preparing a magnesium sheet with a graphene oxide-based solid-liquid composite super-slippery surface comprises the following steps:
[0050] The magnesium sheet was pretreated, and then a picosecond laser was used to texture the surface of the magnesium sheet with bionic fish scale structures of different spacing and diameters. Figure 1As shown, the spacing of the fish scale structure is 460-955 microns, and the diameter is 320-780 microns, respectively named T1-T9. Subsequently, an organosilane sol binder is prepared, 8g of deionized water is added to 56g of silica sol solution and stirred for 5min, and then 60g of n-propanol solution is slowly dripped into the solution, and finally 76.4g of methyltriethoxysilane (MTES) solution is added dropwise and stirred until a slightly blue clear solution is obtained to prepare an organosilane sol binder. After 10g of the organosilane sol binder is dispersed in 5g of n-propanol and magnetically stirred for 30 minutes, it is dripped dropwise into 5g of graphene oxide composite ethanol solution (6%), and then 1g of tridecafluorooctyl trimethoxysilane is dispersed in 20g of deionized water and dripped into the solution. After ultrasonic treatment for 15 minutes, magnetic stirring was performed for 15 minutes, and the solution was sprayed on the surface of the textured magnesium sheet using a spray gun, and finally cured in an oven at 150 degrees to obtain a fluorinated modified graphene oxide hydrophobic coating. The fluorinated modified graphene oxide hydrophobic coating was immersed in krytox GPL-103 perfluoropolyether lubricant, placed in a vacuum drying oven at -100 kPa, vacuum filtered for 3 minutes, and then taken out to obtain a graphene oxide-based solid-liquid composite super-slippery surface.
[0051] Table 1 Different laser processing parameters
[0052]
[0053]
[0054] Table 1 shows the nine laser parameters of picosecond laser texturing, such as Figure 2 Texture effect plan and Figure 3 As shown in the cross-sectional view of the texture effect, the fish-scale structure textured by the processing parameters 1*-4* is shallow and cannot meet the needs of storing lubricants. 5*-9* has a certain depth, but from the plan view, it can be seen that the surface of 7*-9* is severely laser ablated. The existence of the heat-affected zone and the molten material on the surface increase the surface roughness, affecting the wetting properties of the graphene oxide-based solid-liquid composite super-slippery surface. Therefore, the laser processing parameters of 6* are selected for texturing.
[0055] Table 2 Laser textured bionic fish scale structures with different diameters and spacings
[0056]
[0057] Table 2 shows nine fish-scale textures with different diameters and spacings, such as Figure 4 As shown, fish-scale structures with different diameters and spacings have different connectivity.
[0058] The performance of magnesium sheets with graphene oxide-based solid-liquid composite super-slippery surfaces was tested. The test results of their liquid repellency, oil film stability, tribological properties, anti-icing properties, anti-fouling properties and coating mechanical properties are as follows: Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 , Fig.10 shown.
[0059] from Figure 1 It can be seen that the diameter and spacing of the fish-scale structure will affect the connectivity between each unit, thereby affecting the flow of lubricant therein.
[0060] from Figure 2 It can be seen from the plane diagram of the laser texturing effect that the surface of 7*-9* is severely laser ablated. The existence of the heat-affected zone and the molten material on the surface increase the surface roughness, affecting the wetting properties of the graphene oxide-based solid-liquid composite super-smooth surface.
[0061] from Figure 3 The cross-sectional view of the laser texturing effect shows that the fish scale structure textured by the processing parameters 1*-4* is shallow and cannot meet the needs of storing lubricants. 5*-9* has a certain depth, combined with Figure 2 Plan view of laser texturing effect. Finally, the laser processing parameters of 6* were selected for texturing.
[0062] from Figure 4 It can be seen that each fish scale of samples 1, 4, and 7 is connected, which can meet the flow replenishment of lubricant at other locations when defects appear in the oil film of the graphene oxide-based solid-liquid composite super-slippery surface.
[0063] from Figure 5 It can be seen that after laser texturing, the appearance of grooves makes the droplets infiltrate the surface, and the contact angle is greatly reduced; the contact angle increases after spraying the fluorinated modified graphene oxide coating, and the contact angle slightly decreases after perfusing the perfluoropolyether lubricant. At the same time, liquids with different surface tensions can slide on the graphene oxide-based solid-liquid composite super-slippery surface.
[0064] from Figure 6 It can be seen that in the deionized water flushing and centrifugal tests, the lubricant mass of the fish-scale structured graphene oxide-based solid-liquid composite super-slippery surfaces with 9 different geometric parameters was reduced, but the reduction in structure No. 4 was the smallest; after the oil film stability test, the sliding angles of the 9 structures were measured, and the sliding angle of structure No. 4 was also the smallest.
[0065] from Figure 7 It can be seen that the average friction coefficient of the graphene oxide-based solid-liquid composite super-slippery surface is the smallest at 1N and 200RPM; while the wear amount is the lowest at 7N and 200RPM.
[0066] from Figure 8It can be seen that the performance of the fish-scale structured graphene oxide-based solid-liquid composite super-slippery surfaces with 9 different geometric parameters in reducing ice adhesion strength and prolonging freezing time is related to the mass loss rate of the surface lubricant. The No. 4 structure sample with the lowest lubricant mass loss rate in the deionized water flushing and centrifugal tests has the best anti-icing performance. Moreover, the graphene oxide-based solid-liquid composite super-slippery surface prepared by the present invention only needs to be tilted 10 degrees under the intensity of one sun for ice to slide on the surface.
[0067] from Fig. 9 It can be seen that after the graphene oxide-based solid-liquid composite ultra-smooth surface was immersed in honey, coffee, yogurt, and ketchup and then taken out, there was no liquid residue on the surface, while the liquid residue on the surface of the magnesium sheet was serious.
[0068] from Fig.10 It can be seen that according to the GB / T 9286-1998 standard, a grid scratch test was used to test the bonding strength of the graphene oxide coating. The test results showed that the adhesion of the fluorinated modified graphene oxide coating reached 1-degree.
[0069] Embodiment 2:
[0070] A method for preparing a titanium sheet having a graphene oxide-based solid-liquid composite super-slippery surface comprises the following steps:
[0071] The titanium sheet was pretreated, and then a femtosecond laser was used to texture the bionic fish scale structure on the surface of the iron sheet. Figure 1 As shown, the spacing of the fish scale structure is 675 microns and the diameter is 540 microns. Subsequently, an organosilane sol binder is prepared, and 8g of deionized water is added to 56g of silica sol solution and stirred for 5min, then 60g of n-propanol solution is slowly dripped into this solution, and 80g of octyl triethoxymethyl silicon is finally added dropwise to obtain an organosilane sol binder. After 10g of organosilane sol binder is dispersed in 5g of n-propanol and magnetically stirred for 30 minutes, 5g of graphene oxide composite ethanol solution (6%) is dripped dropwise, and then 12g of perfluorododecyl triethoxysilane is dispersed in 30g of deionized water and the solution is dripped. After ultrasonic treatment for 15 minutes, magnetic stirring is carried out for 15 minutes, and the solution is sprayed on the surface of the titanium sheet after the texture using a spray gun, and finally a fluorinated modified graphene oxide hydrophobic coating is obtained after high temperature curing in an oven at 150 degrees. The fluorinated modified graphene oxide hydrophobic coating was immersed in Krytox GPL-101 perfluoropolyether lubricant, placed in a vacuum drying oven at -100 kPa, and vacuum filtered for 3 minutes before being taken out to obtain a graphene oxide-based solid-liquid composite super-slippery surface.
[0072] Embodiment 3:
[0073] A method for preparing an aluminum sheet having a graphene oxide-based solid-liquid composite super-slippery surface comprises the following steps:
[0074] The aluminum sheet is pretreated, and then a femtosecond laser is used to texture the surface of the iron sheet. Fig.10 The circular pit structure shown. Subsequently, an organosilane sol binder was prepared, and 8g of deionized water was added to 56g of silica sol solution and stirred for 5min, and then 60g of n-propanol solution was slowly dripped into the solution, and finally 60g of methyltriethoxymethylsilicon was added dropwise to obtain an organosilane sol binder. After 10g of the organosilane sol binder was dispersed in 5g of n-propanol and magnetically stirred for 30 minutes, 5g of graphene oxide composite ethanol solution (6%) was dripped dropwise, and then 20g of tridecafluorooctyl triethoxysilane was dispersed in 30g of deionized water and dripped into the solution. After ultrasonic treatment for 15 minutes, magnetic stirring was performed for 15 minutes, and the solution was sprayed on the surface of the textured aluminum sheet using a spray gun, and finally a fluorinated modified graphene oxide hydrophobic coating was obtained after high-temperature curing in an oven at 150 degrees. The fluorinated modified graphene oxide hydrophobic coating was immersed in Fomblin YL VAC 25 / 6 perfluoropolyether lubricant, placed in a vacuum drying oven under -100 kPa environment, and vacuum filtered for 3 minutes before being taken out to obtain a graphene oxide-based solid-liquid composite super-slippery surface.
[0075] Embodiment 4:
[0076] A method for preparing an aluminum sheet having a graphene oxide-based solid-liquid composite super-slippery surface comprises the following steps:
[0077] The aluminum sheet was pretreated, and then a femtosecond laser was used to texture the groove structure on the surface of the copper sheet. Then, an organic silane sol binder was prepared. 8g of deionized water was added to 56g of silica sol solution and stirred for 5min, and then 60g of n-propanol solution was slowly dripped into the solution, and finally 45g of decyltriethoxysilane was added dropwise to obtain an organic silane sol binder. After 10g of the organic silane sol binder was dispersed in 5g of n-propanol and magnetically stirred for 30 minutes, 5g of graphene oxide composite ethanol solution (6%) was dripped dropwise, and then 32g of perfluorododecyltrimethoxysilane was dispersed in 30g of deionized water and dripped into the solution. After ultrasonic treatment for 15 minutes, magnetic stirring was performed for 15 minutes, and the solution was sprayed on the surface of the textured aluminum sheet using a spray gun, and finally a fluorinated modified graphene oxide hydrophobic coating was obtained after high-temperature curing in an oven at 150 degrees. The fluorinated modified graphene oxide hydrophobic coating was immersed in Fomblin YL VAC 14 / 6 perfluoropolyether lubricant, placed in a vacuum drying oven under -100 kPa environment, and vacuum filtered for 3 minutes before being taken out to obtain a graphene oxide-based solid-liquid composite super-slippery surface.
[0078] Embodiment 5:
[0079] A method for preparing a magnesium sheet having a graphene oxide-based solid-liquid composite super-slippery surface comprises the following steps:
[0080] The magnesium sheet was pretreated, and then a picosecond laser was used to texture a square groove structure on the surface of the magnesium sheet.
[0081] Subsequently, an organosilane sol binder was prepared. After adding 8g of deionized water to 56g of silica sol solution and stirring for 5min, 60g of n-propanol solution was slowly dripped into the solution, and finally 35g of methylpropyltriethoxysilane was added dropwise to obtain an organosilane sol binder. After 10g of the organosilane sol binder was dispersed in 5g of n-propanol and magnetically stirred for 30 minutes, 5g of graphene oxide composite ethanol solution (6%) was dripped dropwise, and then 12g of trifluoropropyltriethoxysilane was dispersed in 30g of deionized water and dripped into the solution. After ultrasonic treatment for 15 minutes, magnetic stirring was performed for 15 minutes, and the solution was sprayed on the surface of the magnesium sheet after texture using a spray gun, and finally a fluorinated modified graphene oxide hydrophobic coating was obtained after high temperature curing in an oven at 150 degrees. The fluorinated modified graphene oxide hydrophobic coating was immersed in Fomblin YL VAC 14 / 6 perfluoropolyether lubricant, placed in a vacuum drying oven under -100 kPa environment, and vacuum filtered for 3 minutes before being taken out to obtain a graphene oxide-based solid-liquid composite super-slippery surface.
[0082] Description of the drawings
[0083] Figure 1 This is a schematic diagram of the fish-scale structure of the graphene oxide-based solid-liquid composite super-smooth surface in Example 1, with the diameter and spacing as shown in the figure.
[0084] Figure 2 This is a schematic diagram of the plane effect of the fish scale structure textured with different laser processing parameters in Example 1. As shown in the figure, the surface of 7*-9* is severely laser ablated, and the existence of the heat-affected zone and the molten material on the surface increase the surface roughness, which will affect the wetting properties of the graphene oxide-based solid-liquid composite super-slippery surface.
[0085] Figure 3 This is a schematic diagram of the cross-sectional effect of the fish scale structure textured with different laser processing parameters in Example 1. As shown in the figure, the fish scale structure textured with processing parameters 1*-4* is relatively shallow and cannot meet the demand for storing lubricants, while 5*-9* has a certain depth.
[0086] Figure 4 This is a schematic diagram of fish-scale structures with different diameters and spacings in Example 1. As shown in the figure, the connectivity of fish-scale structures with different geometric parameters is different, which will affect the fluidity of the lubricant when defects appear in the surface oil film.
[0087] Figure 5The liquid-repellent properties of the graphene oxide-based solid-liquid composite super-smooth surface in Example 1 are characterized; wherein, (a) is the change in contact angle during the preparation process of the graphene oxide-based solid-liquid composite super-smooth surface; (b) is the contact angle and sliding angle of liquids with different surface tensions on its surface.
[0088] Figure 6 It is a characterization of the oil film stability of the graphene oxide-based solid-liquid composite super-slippery surface in Example 1. Wherein, (a) is the lubricant retention rate of the graphene oxide-based solid-liquid composite super-slippery surface with fish scale structure having different geometric parameters in the centrifugal test; (b) is the lubricant retention rate of the graphene oxide-based solid-liquid composite super-slippery surface with fish scale structure having different geometric parameters in the deionized water flushing test.
[0089] Figure 7 The tribological properties of the graphene oxide-based solid-liquid composite super-slippery surface in Example 1 are characterized. Wherein, (a) is a fluctuation diagram of the friction coefficient of the graphene oxide-based solid-liquid composite super-slippery surface under different loads during the friction process of 3500 seconds; (b) is the average friction coefficient of the graphene oxide-based solid-liquid composite super-slippery surface under different loads during the friction process of 3500 seconds; (c) is the wear amount of the graphene oxide-based solid-liquid composite super-slippery surface under different loads; (d) is a fluctuation diagram of the friction coefficient of the graphene oxide-based solid-liquid composite super-slippery surface under different speeds during the friction process of 3500 seconds; (e) is the average friction coefficient of the graphene oxide-based solid-liquid composite super-slippery surface under different speeds during the friction process of 3500 seconds; (f) is the wear amount of the graphene oxide-based solid-liquid composite super-slippery surface at different speeds.
[0090] Figure 8 Characterization of the anti-icing performance of the graphene oxide-based solid-liquid composite super-slippery surface in Example 1. Among them, (a) is the ice adhesion strength of the graphene oxide-based solid-liquid composite super-slippery surface with fish scale structure of different geometric parameters; (b) is the freezing time of the graphene oxide-based solid-liquid composite super-slippery surface with fish scale structure of different geometric parameters; (c) is the freezing delay in the preparation process of the graphene oxide-based solid-liquid composite super-slippery surface; (d) is a comparison of the sliding conditions of the graphene oxide-based solid-liquid composite super-slippery surface and the untreated magnesium sheet at a light intensity of 10 degrees.
[0091] Fig. 9 Characterization of the antifouling performance of the graphene oxide-based solid-liquid composite supersmooth surface in Example 1. Among them, (a) is a comparison of the graphene oxide-based solid-liquid composite supersmooth surface and the surface of the untreated magnesium sheet taken out after being immersed in ketchup; (b) is a comparison of the graphene oxide-based solid-liquid composite supersmooth surface and the surface of the untreated magnesium sheet taken out after being immersed in coffee; (c) is a comparison of the graphene oxide-based solid-liquid composite supersmooth surface and the surface of the untreated magnesium sheet taken out after being immersed in yogurt; (d) is a comparison of the graphene oxide-based solid-liquid composite supersmooth surface and the surface of the untreated magnesium sheet taken out after being immersed in honey.
[0092] Fig.10 The mechanical properties of the coating on the graphene oxide-based solid-liquid composite super-slippery surface in Example 1 are characterized.
[0093] Fig.11 This is the circular pit structure laser textured in Example 2.
Claims
1. A method for preparing a graphene oxide-based solid-liquid composite super-slippery surface, It is characterized in that The steps include: Step 1: Preparation of microstructured metal sheet: pre-treat the metal sheet, and laser texture the pre-treated metal sheet to obtain a textured metal sheet; the microstructure includes one or more of a bionic structure, a conventional discrete structure, and a conventional continuous structure. Step 2: Preparation of an organosilane sol binder: add deionized water to the silica sol solution, disperse the solution into a solvent, and finally slowly add an organosilane coupling agent to obtain an organosilane sol binder after sufficient reaction; the organosilane coupling agent includes one or more of octyltriethoxysilane, methyltriethoxysilane, decyltriethoxysilane, vinyltriethoxysilane, and methylpropyltriethoxysilane. Step 3: Preparation of fluorinated modified graphene oxide hydrophobic coating: compound the organosilane sol binder obtained in step 2 with the graphene oxide solution, and then add a fluorinated organosilane modifier. After sufficient ultrasonic stirring and mixing, spray it on the surface of the textured metal sheet described in step 1. Finally, the fluorinated modified graphene oxide hydrophobic coating is obtained after oven curing. Step 4: The fluorinated modified graphene oxide hydrophobic coating obtained in step 3 is immersed in perfluoropolyether lubricating oil, and is placed in a vacuum box for filtration and maintained for a certain period of time to obtain a graphene oxide-based solid-liquid composite super-slippery surface.
2. A method for preparing a graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The metal sheet described in step one includes one or more of a magnesium sheet, an aluminum sheet, and a titanium sheet.
3. The method for preparing a graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The processing parameters of the laser texturing in step 1 are laser energy density of 0.5-5 J / cm 2 , frequency 1KHz-1MHz, pulse width 500-2000ps, scanning times 1-25 times, scanning speed 50-200mm / s.
4. The method for preparing a graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The mass ratio of the deionized water, silica sol, solvent and organic silane coupling agent in step 2 is 0.1-3:1:0.5-5:0.5-8.
5. The method for preparing a graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The mass ratio of the organosilane sol binder, graphene oxide solution and fluorine-containing organosilane modifier described in step three is 1~10:1:0.05~2.
6. The method for preparing a graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The filtration pressure in step 4 is -100 kPa.
7. The method for preparing a graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The fluorine-containing organic silane modifier described in step three includes one or more of perfluorododecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, perfluorododecyltrimethoxysilane, and perfluorodecyltriethoxysilane.
8. The method for preparing the graphene oxide-based solid-liquid composite super-slippery surface according to claim 1, It is characterized in that The perfluoropolyether lubricant in step 4 includes one or more of Krytox GPL-103 perfluoropolyether lubricant, Krytox GPL-101 perfluoropolyether lubricant, Fomblin YL VAC 25 / 6 perfluoropolyether lubricant, and Fomblin YL VAC14 / 6 perfluoropolyether lubricant.
9. Application of the graphene oxide-based solid-liquid composite super-slippery surface described in claim 1 in the fields of liquid repellency and anti-fouling, wear resistance and drag reduction, anti-icing and de-icing, self-healing, and long-term service of coatings.
Citation Information
Cited By
Preparation method of double-layer structure super-hydrophobic photothermal conversion anti-icing and deicing coating containing laser-induced graphene
CN119286292A