Wet screening method for size and layer number selection of electrochemical stripping two-dimensional material
The wet sieving method is used to sieve the electrochemically exfoliated two-dimensional materials step by step, which solves the problem of difficulty in size and layer classification in the existing technology, realizes efficient and low-cost separation, purification and classification of two-dimensional materials, and improves the efficiency Material performance and application suitability.
Patent Information
- Application Number
- CN202410879055.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technology is difficult to realize the size and layer classification of electrochemical graphene oxide and other two-dimensional materials with high efficiency, low cost and large batches, resulting in poor consistency in sheet size and difficulty in meeting different application needs.
The wet sieving method is used to sieve the electrochemically exfoliated two-dimensional materials step by step through screens of different apertures. The flexible characteristics of the two-dimensional materials are used to select the size and number of layers, and the unstripped crystals and intercalations are removed to obtain Different levels of graded products.
It achieves efficient, low-cost separation, purification, size and layer classification of two-dimensional materials, and obtains two-dimensional material sheets with narrow size distribution and few or single layers, which improves the performance and application applicability of the materials.
Smart Images

Figure CN118808097A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of two-dimensional material preparation, and specifically relates to a wet screening method for electrochemically stripping two-dimensional materials to select size and number of layers. Background Art
[0002] In recent years, the preparation of electrochemical graphene oxide by electrochemical oxidation has become an attractive method for preparing electrochemical graphene oxide due to its safety, environmental protection and cost advantages. However, compared with the traditional chemical oxidation method, the electrochemical graphene oxide prepared by the electrochemical oxidation method has the key problems of small flake size, poor consistency of layer number and size, which makes it difficult to meet the requirements of subsequent processing and application. Moreover, the preparation of other electrochemically exfoliated two-dimensional materials besides graphene also faces the pain point of difficult separation and purification. Therefore, the study of efficient, low-cost separation, purification and size classification of electrochemically oxidized graphene and other exfoliated two-dimensional materials is the key to promoting the development of controlled preparation technology of two-dimensional materials.
[0003] The size of two-dimensional material sheets has an important influence on the performance of macroscopic structural materials (such as fibers, films, and aerogels) obtained by their assembly. On the one hand, a narrower size distribution (i.e., the size of the two-dimensional material sheets is highly consistent and the size distribution is concentrated) can improve the performance of macroscopic structural materials. On the other hand, different application fields have different requirements for the size of two-dimensional material sheets. Taking conductivity as an example, larger two-dimensional material sheets reduce the connection between sheets, making the contact resistance between sheets smaller. For electrochemical sensing and biological applications, smaller two-dimensional material sheets are more advantageous because they have higher electrochemically active edge positions and better biocompatibility. Therefore, the separation and purification of two-dimensional materials is extremely important for their subsequent applications.
[0004] The existing separation and purification methods for two-dimensional materials mainly include high-speed centrifugation and static stratification, but since neither of them can achieve high efficiency, low cost and large-scale separation and purification while achieving good separation and purification effects, it is difficult to achieve large-scale layer purification and size classification requirements for two-dimensional materials. Therefore, the development of new separation and purification methods is extremely important for the controlled preparation of electrochemical graphene oxide and other two-dimensional materials. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a wet screening method for electrochemically exfoliating two-dimensional materials to select size and number of layers.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection comprises the following steps:
[0008] (1) dispersing the electrochemically exfoliated two-dimensional material in a dispersion liquid to obtain a two-dimensional material dispersion liquid;
[0009] (2) The two-dimensional material dispersion is wet-sieved step by step using sieves with pore sizes of 40 μm, 20 μm, 15 μm, 10 μm, 7.5 μm and 5 μm.
[0010] As a preferred embodiment of the present invention, the two-dimensional material is electrochemically exfoliated graphene oxide, electrochemically exfoliated NbSe2 or electrochemically exfoliated In2Se3.
[0011] As a preferred embodiment of the present invention, the dispersion liquid is water or propylene carbonate.
[0012] As a preferred embodiment of the present invention, the dispersion specifically includes the following steps: dispersing the electrochemically exfoliated two-dimensional material in a dispersion liquid, then stirring at a speed of 300 rpm for 10 min, and finally shear dispersing at a speed of 3000 rpm for 10 min.
[0013] As a preferred embodiment of the present invention, the step-by-step wet screening process is performed by stirring with external force or by static screening by flushing with dispersion liquid.
[0014] Principle of the invention:
[0015] Compared with traditional powder material screening (rigidity), only materials with a size smaller than the sieve hole diameter can pass through the sieve. Two-dimensional materials have the characteristics of low bending stiffness (flexibility), and the bending stiffness increases with the number of material layers (thickness). Therefore, during the wet screening of two-dimensional materials, a few layers of two-dimensional materials with a size slightly larger than the sieve hole diameter can also pass through the sieve. In addition to controlling the average size, screening can also effectively control the number of material layers (thickness).
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention utilizes the characteristics of the difference in the flexible bending of two-dimensional materials with different numbers of layers to wet screen the two-dimensional material dispersion step by step with screens of different apertures, thereby obtaining two-dimensional material flakes of different sizes and numbers of layers, and realizing the separation and purification of two-dimensional materials and the classification of sizes and numbers of layers in a green, efficient and low-cost method. In addition, the present invention separates and purifies the electrochemically stripped two-dimensional material dispersion, effectively removing the unstripped crystals and intercalations in the two-dimensional material dispersion and the two-dimensional material blocks with poor stripping effects, and obtaining two-dimensional material flakes of different levels with narrow size distribution and few layers and / or single layers in the screening and grading products. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1(a)-(d) are optical micrographs of the graded products of electrochemical graphene oxide after wet sieving, which are: electrochemical graphene oxide original sample, 20 μm undersize-15 μm oversize, 10 μm undersize-7.5 μm oversize, 5 μm undersize; Figure 1 (e)-(h) are SEM images of the graded products of electrochemical graphene oxide after wet sieving, from left to right: electrochemical graphene oxide original sample, 20 μm undersize-15 μm oversize, 10 μm undersize-7.5 μm oversize, 5 μm undersize; Figure 1 (i)-(l) are the size distribution diagrams of the graded products of electrochemical graphene oxide after wet screening, from left to right: electrochemical graphene oxide original sample, 20μm undersize-15μm oversize, 10μm undersize-7.5μm oversize, 5μm undersize.
[0019] Figure 2 (a) is the XRD spectrum of graphite paper and electrochemical graphene oxide screening and grading products; (b) is the comparison chart of the maximum flake size and sieve hole diameter of electrochemical graphene oxide screening and grading products; (c) is the XRD spectrum of electrochemical graphene oxide screening and grading products at various levels; (d) is the comparison chart of the maximum flake size and sieve hole diameter of electrochemical graphene oxide screening and grading products at various levels.
[0020] Figure 3 The invention relates to separating and purifying electrochemically oxidized graphene by centrifugal separation.
[0021] Figure 4 (a)-(d) are optical micrographs of the graded products of electrochemically stripped NbSe2 after wet screening, which are: original electrochemically stripped NbSe2 sample, 20μm undersize-15μm oversize, 10μm undersize-7.5μm oversize, 5μm undersize; Figure 4 (e)-(h) are SEM images of the graded products of electrochemically stripped NbSe2 after wet screening, which are: electrochemically stripped NbSe2 original sample, 20μm under-15μm oversize, 10μm under-7.5μm oversize, 5μm undersize; Figure 4 (i)-(l) are the size distribution diagrams of the graded products of electrochemically stripped NbSe2 after wet screening, which are: electrochemically stripped NbSe2 original sample, 20μm undersieve-15μm oversieve, 10μm undersieve-7.5μm oversieve, 5μm undersieve.
[0022] Figure 5(a) is the XRD spectrum of electrochemically stripped NbSe2 crystals and electrochemically stripped NbSe2 screening and grading products; (b) is the comparison chart of the maximum lamella size and sieve hole diameter of electrochemically stripped NbSe2 screening and grading products; (c) is the XRD spectrum of electrochemically stripped NbSe2 screening and grading products of various levels; (d) is the comparison chart of the maximum lamella size and sieve hole diameter of electrochemically stripped NbSe2 screening and grading products of various levels.
[0023] Figure 6 To separate and purify electrochemically stripped NbSe2 by centrifugal separation.
[0024] Figure 7 (a)-(d) are optical micrographs of the graded products of electrochemically stripped In2Se3 after wet screening, which are: electrochemically stripped In2Se3 original sample, 20μm under-15μm over-10μm under-7.5μm over-5μm under-5μm; Figure 7 (e)-(h) are SEM images of the graded products of electrochemically stripped In2Se3 after wet screening, which are: electrochemically stripped In2Se3 original sample, 20μm under-15μm oversize, 10μm under-7.5μm oversize, 5μm undersize; Figure 7 (i)-(l) are the size distribution diagrams of the graded products of electrochemically stripped In2Se3 after wet screening, which are: electrochemically stripped In2Se3 original sample, 20μm undersieve-15μm oversieve, 10μm undersieve-7.5μm oversieve, 5μm undersieve.
[0025] Figure 8 (a) is the XRD spectrum of electrochemically stripped In2Se3 crystals and electrochemically stripped In2Se3 screening and grading products; (b) is the comparison chart of the maximum flake size and sieve hole diameter of electrochemically stripped In2Se3 screening and grading products; (c) is the XRD spectrum of electrochemically stripped In2Se3 screening and grading products of various levels; (d) is the comparison chart of the maximum flake size and sieve hole diameter of electrochemically stripped In2Se3 screening and grading products of various levels.
[0026] Fig. 9 To separate and purify electrochemically stripped In2Se3 by static stratification.
[0027] Fig.10 Schematic diagram of size and layer number selection for electrochemical exfoliation of 2D materials using the wet sieving method. DETAILED DESCRIPTION
[0028] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0029] Example 1
[0030] A wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection comprises the following steps:
[0031] (1) dispersing the electrochemically exfoliated electrochemically oxidized graphene in ultrapure water, stirring at a speed of 300 rpm for 10 min, and then shearing and dispersing at a speed of 3000 rpm for 10 min to obtain an electrochemically oxidized graphene dispersion;
[0032] (2) The electrochemical graphene oxide dispersion was wet-sieved step by step using sieves with apertures of 40 μm, 20 μm, 15 μm, 10 μm, 7.5 μm and 5 μm under external stirring. The 20 μm undersieve and 15 μm oversieve, the 10 μm undersieve and 7.5 μm oversieve, and the 5 μm undersieve were taken as the electrochemical graphene oxide sieving and grading products. The samples dispersed on the surface of Si / SiO2 sheets were obtained through liquid-gas interface assembly. The sheet conditions were observed by optical microscopy and SEM, and the sheet size was counted. The sheet thickness was compared by observing the color.
[0033] like Figure 1 (a) Figure 1 (e) and Figure 1 As shown in (i), in the original sample of electrochemically oxidized graphene, the flake size distribution is wide, and the flake thickness varies, including large flakes with a size of more than 200 μm and three-dimensional blocks. Among them, the maximum flake size is 343.03 μm, and the average flake size is 37.85±52.27 μm.
[0034] like Figure 1 (b) Figure 1 (f) and Figure 1 As shown in (j), in the electrochemical graphene oxide 20μm under-15μm sieve, the flake size is large, the flake thickness is mostly multi-layer, and the flake thickness is less than the original electrochemical graphene oxide sample, and some few flakes can be observed. Among them, the maximum flake size is 83.21μm, and the average flake size is 42.81±18.33μm. The flake size distribution is narrower than that of the original electrochemical graphene oxide sample, and the screening process removes most of the small flakes (less than 20μm in size).
[0035] like Figure 1 (c) Figure 1 (g) and Figure 1As shown in (k), in the electrochemical graphene oxide 10μm under-7.5μm oversize, the lamella size is smaller than that of the 20μm under-15μm oversize, the lamella size is medium, and the lamella is mainly a few layers, indicating that the lamella thickness is less than that of the 20μm under-15μm oversize, in which some single-layer lamellae can also be observed. Among them, the maximum lamella size is 57.42μm, and the average lamella size is 26.78±10.34μm. Compared with the 20μm under-15μm oversize, it can be seen that the screening process further reduces the lamella size and lamella thickness of the electrochemical graphene oxide, and the lamella size distribution is narrow.
[0036] like Figure 1 (d) Figure 1 (h) and Figure 1 As shown in (l), in the electrochemical graphene oxide 5μm undersize, the lamella size is small, and the lamella is mainly single-layer. Among them, the maximum lamella size of the 5μm undersize is 26.26μm, and the average lamella size is 8.34±4.60μm. Compared with the 10μm undersize-7.5μm oversize, it can be seen that the screening process further reduces the lamella size, and the lamella size distribution is narrow. The lamellae are mainly about 8μm in size, accounting for about 36% of the total number of lamellae.
[0037] Therefore, as the screening process proceeds, the size and thickness of the electrochemically oxidized graphene sheets decrease step by step, the sheet size distribution gradually narrows, the sheet size gradually concentrates, and the separation and purification effect is better.
[0038] And by Figure 2 (a) The XRD spectra of the graphite paper and electrochemical graphene oxide screening and classification products show that the original electrochemical graphene oxide sample is composed of three phases: electrochemical graphene oxide (10.8°), weakly oxidized electrochemical graphene oxide (22.4°) and graphite (26.0°), while the 40μm sieve contains two phases: electrochemical graphene oxide (10.8°) and graphite (26.0°), and the graphite content is much higher than that of electrochemical graphene oxide. The 40μm sieve undersize only contains two phases: electrochemical graphene oxide (10.8°) and weakly oxidized electrochemical graphene oxide (22.4°). Therefore, the 40μm aperture sieve was used for screening and purification, and the graphite phase in the original electrochemical graphene oxide sample was successfully separated without causing almost no loss of electrochemical graphene oxide.
[0039] Figure 2(b) is a comparison chart of the maximum lamella size and sieve hole diameter of the electrochemical graphene oxide screening and grading products, among which the maximum lamella size of the untreated original sample (343.03μm) is larger than the maximum lamella size of the 40μm undersize (153.72μm), and 40μm is the largest grading pore size in the screening and grading. Therefore, it can be considered that the graded products smaller than this size will not be affected by the liquid-gas interface assembly, and the microscopic morphology is authentic and objective.
[0040] Depend on Figure 2 (c) From the XRD spectra of the electrochemical graphene oxide grading products at each level, it can be seen that the three-level grading products only contain electrochemical graphene oxide and weakly oxidized electrochemical graphene oxide. This is because all the graphite phases in the original electrochemical graphene oxide sample have been successfully separated through the 40μm pore size sieve.
[0041] Figure 2 (d) is a comparison chart of the maximum flake size and sieve hole diameter of the electrochemical graphene oxide screening and grading products at each level. It can be clearly found that a good regularity is maintained in the three-level classification products, and the maximum flake size of electrochemical graphene oxide decreases step by step with the decrease of the sieve hole diameter.
[0042] like Figure 3 As shown, compared with the separation and purification of electrochemically exfoliated graphene oxide by centrifugal separation, the graphite phase in the untreated original sample of electrochemically oxidized graphene can only be completely removed when the centrifugal speed reaches 6500rpm or more, but the centrifugation also causes a large amount of electrochemically oxidized graphene to be lost. Moreover, the amount of graphite phase removed from the electrochemically oxidized graphene dispersion by wet screening is about 5 times the amount of centrifugal treatment. In addition, the wet screening process is scalable, and the wet screening process can be effectively increased by increasing the screen area, and the wet screening process is less affected by the concentration of the dispersion than centrifugation.
[0043] In summary, the wet screening method for size and layer selection of electrochemically exfoliated two-dimensional materials described in the present invention successfully separated the graphite phase in the original sample of electrochemically oxidized graphene. The screening and grading effectively achieved the separation and purification of electrochemically oxidized graphene, and effectively separated and purified the average size and thickness of electrochemically oxidized graphene sheets.
[0044] Example 2
[0045] A wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection comprises the following steps:
[0046] (1) adding electrochemically stripped NbSe2 into propylene carbonate, stirring at a speed of 300 rpm for 10 min, and then shearing and dispersing at a speed of 3000 rpm for 10 min to obtain an electrochemically stripped NbSe2 dispersion;
[0047] (2) The electrochemically stripped NbSe2 dispersion was wet-screened step by step using sieves with apertures of 20 μm, 15 μm, 10 μm, 7.5 μm and 5 μm in sequence. During the step-by-step wet-screening process, the propylene carbonate flushing method was used for static screening. The 20 μm undersieve and 15 μm oversieve, the 10 μm undersieve and 7.5 μm oversieve, and the 5 μm undersieve were taken as the electrochemically stripped NbSe2 screening and grading products. The samples dispersed on the surface of the Si / SiO2 sheet were obtained through liquid-gas interface assembly. The sheet conditions were observed using an optical microscope and a SEM, and the sheet size was statistically analyzed. The sheet thickness was compared by observing the color.
[0048] like Figure 4 (a) Figure 4 (e) and Figure 4 As shown in (i), in the original sample of electrochemically stripped NbSe2, the lamella size distribution is wide and the thickness of the lamella varies. It contains large lamellae with a size of more than 200 μm and three-dimensional blocks. Among them, the maximum lamella size is 249.15 μm and the average lamella size is 43.31±36.69 μm.
[0049] like Figure 4 (b) Figure 4 (f) and Figure 4 As shown in (j), in the 20μm under-15μm oversize of electrochemically stripped NbSe2, the lamella size is relatively large, and the lamellae are mainly multi-layered, indicating that the lamella thickness is relatively thick, including a few layers of small lamellae. The maximum lamella size in the 20μm under-15μm oversize is 176.71μm, and the average lamella size is 59.08±34.23μm. The lamella size distribution is narrower than that of the original sample of electrochemically stripped NbSe2, and the screening process removes most of the small lamellae (less than 20μm in size).
[0050] like Figure 4 (c) Figure 4 (g) and Figure 4 As shown in (k), in the 10μm undersize-7.5μm oversize of electrochemically stripped NbSe2, the lamella size is smaller than that of the 20μm undersize-15μm oversize, the lamella size is medium, and the lamella is mainly a few layers, indicating that the lamella thickness is smaller than that of the 20μm undersize-15μm oversize, and the lamella thickness is medium. Some single-layer small lamellae can also be observed, which is similar to the 20μm undersize-15μm oversize. Among them, the maximum lamella size is 71.65μm, and the average lamella size is 34.11±18.45μm. Compared with the 20μm undersize-15μm oversize, it can be seen that the screening process further reduces the lamella size and lamella thickness of electrochemically stripped NbSe2, and the lamella size distribution is narrow.
[0051] like Figure 4 (d) Figure 4 (h) and Figure 4 As shown in (l), in the 5μm undersize of electrochemically stripped NbSe2, the lamella size is smaller than that of the 10μm undersize-7.5μm oversize, the lamella size is smaller, and the lamella is mainly single-layer, indicating that the lamella thickness is smaller than that of the 10μm undersize-7.5μm oversize, and the lamella thickness is thinner. Among them, the maximum lamella size is 32.44μm, and the average lamella size is 10.93±4.84μm. Compared with the 10μm undersize-7.5μm oversize, it can be seen that the screening process further reduces the lamella size and lamella thickness, and the lamella size distribution is narrow. The lamellae are mainly 10μm in size, accounting for about 60% of the total number of lamellae.
[0052] Therefore, as the screening process proceeds, the flake size and thickness of the electrochemically stripped NbSe2 decrease step by step, the flake size distribution gradually narrows, the flake size gradually concentrates, and the separation and purification effect is better.
[0053] And by Figure 5 (a) From the XRD spectra of NbSe2 crystals and the screening and grading products of electrochemically stripped NbSe2, it can be seen that the large flakes with a size of more than 200μm and the three-dimensional blocks in the original sample of electrochemically stripped NbSe2 are not crystals without electrochemical reaction, but intercalation compounds that are not fully stripped. According to the diffraction peaks of the above-mentioned layered materials, the interlayer spacing can be calculated by the Bragg equation (2dsinθ=nλ). The diffraction peaks of the XRD spectrum of the original sample of electrochemically stripped NbSe2 at around 6° and 12° correspond to the (001) and (002) diffraction of the phase with an interlayer spacing of 1.49nm. The group of diffraction peaks at around 7° and 15° are the (001) and (002) diffraction peaks of the phase with an interlayer spacing of 1.20nm. Analysis shows that the 20μm sieve of NbSe2 is mainly composed of intercalation compounds with an interlayer spacing of 1.07nm, which corresponds to the large pieces and three-dimensional blocks in the optical microscope characterization. In the 20μm sieve, the XRD characterization results show that the interlayer spacing is mainly 1.54nm. Combined with the characterization results of the optical microscope, it can be seen that the interlayer spacing of the overlapping few layers (single layer) of NbSe2 should be 1.54nm. Therefore, the 20μm sieve effectively separates the NbSe2 thick flakes with poor intercalation and stripping effects in the original electrochemical stripping product.
[0054] Figure 5(b) is a comparison chart of the maximum lamella size and sieve hole diameter of the electrochemically stripped NbSe2 screening and grading products. Among them, the maximum lamella size of the original sample of electrochemically stripped NbSe2 (249.15μm) is larger than the maximum lamella size of the 20μm sieve material (179.67μm), and 20μm is the largest grading pore size in the screening and grading. Therefore, it can be considered that the graded products smaller than this size will not be affected by the liquid-gas interface assembly, and the microscopic morphology is authentic and objective.
[0055] Depend on Figure 5 (c) XRD patterns of the electrochemically stripped NbSe2 products at various screening stages show that, by calculating the Bragg equation (2dsinθ=nλ), the diffraction peak at 6° corresponds to an interlayer spacing of 1.54nm, while the diffraction peak at 12° is the secondary diffraction of this interlayer spacing. Similarly, the peaks at around 7° and 15° correspond to the primary and secondary diffraction peaks with an interlayer spacing of 1.22nm, respectively. Figure 5 From the analysis of (a), the peak around 6° is caused by the interlamellar spacing after overlapping NbSe2 lamellae with smaller lamellae size or thinner thickness; while the peak around 7° represents the interlamellar spacing after overlapping NbSe2 lamellae with medium lamellae size or medium thickness, which is consistent with the results observed in light microscopy and SEM.
[0056] Figure 5 (d) is a comparison chart of the maximum flake size and sieve hole diameter of the electrochemical stripping NbSe2 screening and grading products at each level. It can be clearly found that a good regularity is maintained in the three-level grading products, and the maximum flake size of electrochemically stripped NbSe2 decreases step by step with the decrease of the sieve hole diameter.
[0057] like Figure 6 As shown in the figure, compared with the separation and purification of electrochemically stripped NbSe2 by centrifugal separation, it can be seen from the XRD spectrum that when the centrifugal speed reaches more than 2000rpm, the NbSe2 thick flakes with poor intercalation and stripping effects in the electrochemically stripped NbSe2 can be completely removed, and centrifugation causes a large amount of NbSe2 loss. In addition, the treatment capacity of removing NbSe2 thick flakes with poor intercalation and stripping effects in the NbSe2 dispersion by wet screening is about 3 times that of the centrifugal treatment capacity.
[0058] Example 3
[0059] A wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection comprises the following steps:
[0060] (1) adding the electrochemically stripped In2Se3 into propylene carbonate, stirring at a speed of 300 rpm for 10 min, and then shearing and dispersing at a speed of 3000 rpm for 10 min to obtain an electrochemically stripped In2Se3 dispersion;
[0061] (2) The electrochemically stripped In2Se3 dispersion was wet-screened step by step using sieves with apertures of 20μm, 15μm, 10μm, 7.5μm and 5μm in sequence. During the step-by-step wet screening process, the propylene carbonate flushing method was used for static screening. The 20μm undersieve and 15μm oversieve, the 10μm undersieve and 7.5μm oversieve, and the 5μm undersieve were taken as the electrochemically stripped In2Se3 screening and grading products. The samples dispersed on the surface of the Si / SiO2 sheet were obtained through liquid-gas interface assembly. The sheet conditions were observed using an optical microscope and a SEM, and the sheet size was statistically analyzed. The sheet thickness was compared by observing the color.
[0062] like Figure 7 (a) Figure 7 (e) and Figure 7 As shown in (i), in the original sample of electrochemically stripped In2Se3, the lamella size distribution is wide, and the lamella thickness varies, and there are also some blocks. Among them, the maximum lamella size is 105.13μm, and the average lamella size is 17.96±20.68μm.
[0063] like Figure 7 (b) Figure 7 (f) and Figure 7 As shown in (j), in the 20μm undersize-15μm oversize of electrochemically stripped In2Se3, there are mainly multi-layer flakes and few-layer flakes. The maximum flake size in the 20μm undersize-15μm oversize is 84.29μm, and the average flake size is 18.74±18.87μm. The flake size distribution is narrower than that of the original sample of electrochemically stripped In2Se3.
[0064] like Figure 7 (c) Figure 7 (g) and Figure 7 As shown in (k), in the 10μm undersize-7.5μm oversize of electrochemically stripped In2Se3, the flake size is smaller than that of the 20μm undersize-15μm oversize, mainly multi-layer flakes and few-layer flakes, indicating that the flake thickness is smaller than that of the 20μm undersize-15μm oversize, and the flake thickness is medium. Among them, the maximum flake size is 62.80μm, and the average flake size is 14.84±14.79μm. Compared with the 20μm undersize-15μm oversize, it can be seen that the screening process further reduces the flake size and flake thickness of electrochemically stripped In2Se3, and the flake size distribution is similar to that of the 20μm undersize-15μm oversize.
[0065] like Figure 4 (d) Figure 4 (h) and Figure 4As shown in (l), in the 5μm undersize of electrochemically stripped In2Se3, the lamella size is smaller than that of the 10μm undersize-7.5μm oversize, and the lamella size is relatively small, mainly consisting of a few layers and a single layer, indicating that the lamella thickness is smaller than that of the 10μm undersize-7.5μm oversize, and the lamella thickness is relatively thin. Among them, the maximum lamella size is 26.69μm, and the average lamella size is 5.78±3.69μm. Compared with the 10μm undersize-7.5μm oversize, it can be seen that the screening process further reduces the lamella size and lamella thickness, and the lamella size distribution is narrow. The lamellae are mainly 5μm in size, accounting for about 40% of the total number of lamellae.
[0066] Therefore, as the screening process proceeds, the flake size and thickness of the electrochemically stripped In2Se3 gradually decrease, the flake size distribution gradually narrows, the flake size gradually concentrates, and the separation and purification effect is better.
[0067] And by Figure 8 (a) XRD spectrum analysis of In2Se3 crystal and screening and grading products of electrochemically stripped In2Se3 shows that, relative to In2Se3 crystal, the Bragg formula (2dsinθ=nλ) shows that the diffraction peak at about 6° corresponds to a crystal plane spacing of about 1.55nm, which can be attributed to the single layer (few layers) of In2Se3 flakes stripped from the original sample of electrochemically stripped In2Se3, while the strong peak at about 17° is attributed to the (004) plane diffraction peak of the unstripped In2Se3 crystal. This phenomenon indicates that the yield of electrochemically stripped In2Se3 is relatively low, and the initial product contains more unstripped crystals. By comparing the XRD spectra of In2Se3 under and over the 20μm sieve, it is obvious that the unstripped crystals in the original sample of electrochemically stripped In2Se3 can be effectively removed by screening with a 20μm sieve.
[0068] Figure 8 (b) is a comparison chart of the maximum lamella size and sieve hole diameter of the electrochemically stripped In2Se3 screening and grading products. Among them, the maximum lamella size of the original sample of electrochemically stripped In2Se3 (105.13μm) is larger than the maximum lamella size in the 20μm sieve (86.51μm), and 20μm is the largest grading pore size in the screening and grading. Therefore, it can be considered that the graded products smaller than this size will not be affected by the liquid-gas interface assembly, and the microscopic morphology is authentic and objective.
[0069] Depend on Figure 8(c) From the XRD patterns of the electrochemically stripped In2Se3 screening and grading products at various levels, it can be seen that, calculated by the Bragg equation (2dsinθ=nλ), all the In2Se3 screening and grading products have the same phase structure, and all have (001) diffraction with an interlayer spacing of about 1.55 nm at around 6°, corresponding to the completely stripped In2Se3 screening and grading products. Calculated by the Bragg equation (2dsinθ=nλ), it can be seen that the diffraction peaks at around 11° and 17° in the XRD pattern are the second and third order diffraction peaks with an interlayer spacing of 1.55 nm, respectively.
[0070] Figure 8 (d) is a comparison chart of the maximum flake size and sieve hole diameter of the electrochemically stripped In2Se3 screening and grading products at each level. It can be clearly found that a good regularity is maintained in the three-level grading products, and the maximum flake size of the electrochemically stripped In2Se3 decreases step by step with the decrease of the sieve hole diameter.
[0071] like Fig. 9 As shown in the figure, compared with the separation and purification of electrochemically stripped In2Se3 by static stratification, it can be seen from the XRD spectrum that the In2Se3 crystals in the original sample of electrochemically stripped In2Se3 can be completely removed only when the static time reaches more than 45 minutes. In addition, the time for removing the crystals in the original sample of electrochemically stripped In2Se3 by wet sieving is only about one-fifth of that of static stratification.
[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A wet screening method for size and layer selection of electrochemical exfoliation of two-dimensional materials, It is characterized in that The steps include: (1) dispersing the electrochemically exfoliated two-dimensional material in a dispersion liquid to obtain a two-dimensional material dispersion liquid; (2) The two-dimensional material dispersion is wet-sieved step by step using sieves with pore sizes of 40 μm, 20 μm, 15 μm, 10 μm, 7.5 μm and 5 μm.
2. The wet screening method for selecting the size and number of layers of the electrochemically exfoliated two-dimensional material according to claim 1, It is characterized in that The two-dimensional material is electrochemically exfoliated graphene oxide, electrochemically exfoliated NbSe 2 or electrochemically stripped In 2 Se 3 .
3. The wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection as claimed in claim 1, It is characterized in that The dispersion liquid is water or propylene carbonate.
4. The wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection as claimed in claim 1, It is characterized in that The dispersion pretreatment process specifically includes the following steps: dispersing the electrochemically exfoliated two-dimensional material in the dispersion, then stirring at a speed of 300 rpm for 10 minutes, and finally shearing and dispersing at a speed of 3000 rpm for 10 minutes.
5. The wet screening method for electrochemical exfoliation of two-dimensional materials for size and layer selection as claimed in claim 1, It is characterized in that In the step-by-step wet screening process, the screening is carried out by stirring with external force or by static screening by flushing with dispersion liquid.
Citation Information
Patent Citations
Wet sieving method
CN107262264A
Thickness screening method, sheet diameter screening method and diameter-thickness ratio regulation and control method for two-dimensional material
CN113117878A
Method of producing different-fraction magnetic microspheres from thermal power station fly ash
RU2407595C1
Low-temperature method of producing nano-scaled graphene platelets and their nanocomposites