System and method for efficiently preparing bottom-layer-free raw materials of oriented silicon steel thin strip
Through a combination of mechanical grinding and pickling, shallow flow turbulent pickling technology is used to remove the bottom layer of the glass film of the oriented silicon steel strip, which solves the problems of low production efficiency and high cost in the existing technology, and achieves high efficiency and low cost. Preparation of base-free raw materials supports large-scale production.
Patent Information
- Application Number
- CN202410934609.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-22
AI Technical Summary
In the existing technology, the preparation method of oriented silicon steel thin strip without bottom layer raw materials has the problems of low production efficiency, high cost, environmental pollution and difficulty in large-scale production. In particular, there is a lack of efficient method for removing the bottom layer of Mg2SiO4 glass film.
Using a system that combines mechanical grinding and pickling, online continuous grinding with a broadband sander and shallow flow turbulent pickling technology, combined with real-time detection and feedback of steel strip thickness by a PLC controller, achieves efficient removal of the glass film of oriented silicon steel. Ground floor.
It achieves efficient and continuous preparation of oriented silicon steel without bottom-layer raw materials, reduces production costs, improves production efficiency, avoids environmental pollution, and supports large-scale production.
Smart Images

Figure CN118808348A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of oriented silicon steel preparation, and in particular to a system and method for efficiently preparing oriented silicon steel thin strips without bottom layer raw materials. Background Art
[0002] In the production process of special oriented silicon steel, oriented silicon steel finished products are often used as raw materials and are produced through cold rolling, annealing or siliconization processes. For example, oriented silicon steel ultra-thin strips (thickness ≤ 0.10mm) are made from thick oriented silicon steel finished products through cold rolling and annealing processes; oriented silicon steel with high silicon content is made from ordinary oriented silicon steel finished products as the base material through siliconization processes. However, in the traditional industrial production of oriented silicon steel, an oxide layer is formed on the surface of the steel plate during the decarburization annealing stage, which reacts with the coated MgO isolation agent in the high-temperature annealing stage to form a Mg2SiO4 glass film bottom layer. This causes great difficulties in the processing of special oriented silicon steel, and the Mg2SiO4 bottom layer must be removed before cold rolling, annealing or siliconization and other processing processes can be carried out. In addition, the Mg2SiO4 bottom layer has a high hardness, which greatly reduces the number of punching sheets of the blade die at one time. Based on the above phenomenon, in recent years, many companies have controlled the decarburization annealing process to prevent the oxide layer from existing on the surface of the steel plate, and finally obtained oriented silicon steel without a bottom layer. However, this type of bottom-free oriented silicon steel has problems such as unstable inhibitors, imperfect secondary recrystallization, high cost and difficulty in large-scale production.
[0003] In the prior art, the raw materials of special oriented silicon steel are still mainly oriented silicon steel products produced by traditional processes, but there is still a lack of methods for efficiently removing the bottom layer of Mg2SiO4 glass film. The traditional method is to remove the bottom layer by long-term immersion in hot hydrochloric acid. This method has high production cost, cumbersome process, low production efficiency, and serious environmental pollution. CN109112395A discloses a method for preparing oriented silicon steel thin strip without bottom layer raw materials by physical sandblasting, which is completed by two sandblasting machines in series, that is, the first sandblasting machine performs surface rough processing, and the second sandblasting machine performs surface fine processing, and then annealing is used to eliminate the stress introduced by sandblasting. Among them, on the one hand, multiple sandblasting machines are required to be connected in series for multi-stage sandblasting, resulting in increased cost and increased space requirements. On the other hand, there is a serious dust problem, which requires a dust removal system. On the other hand, the conveying speed of the steel strip is only 0.5m / min~5m / min, which has the problems of low production efficiency and high cost. CN113215374B uses a physical method of laser scoring to prepare bottom-free oriented silicon steel. This process requires stress relief annealing to compensate for the plastic deformation of the steel strip during the laser scoring process, which prolongs the production process. At the same time, the laser scoring equipment is expensive, which brings a large economic burden to the enterprise and is difficult to carry out large-scale production.
[0004] In view of the urgent need for a method for preparing oriented silicon steel thin strips without a bottom layer in the current material preparation field, we urgently need to develop a new method that can efficiently prepare oriented silicon steel thin strips without a bottom layer. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a system and method for efficiently preparing oriented silicon steel thin strips without bottom layer raw materials. The system of the present invention can continuously and efficiently prepare oriented silicon steel without bottom layer raw materials online by combining mechanical grinding and pickling, has extremely high production efficiency, and can realize large-scale production.
[0006] The technical solution of the present invention is as follows:
[0007] A system for efficiently preparing an oriented silicon steel thin strip without a bottom layer raw material, the system comprising a mechanical grinding system 5, a pickling system 6, a looper 7, a tension roller 8, a tail shear 9, a steering pinch roller 10, a coiler 11 and an oriented silicon steel thin strip 12; the mechanical grinding system 5 comprises a wide-band sander 13, a thickness gauge 14, a PLC controller 15 and a display screen 16; the pickling system 6, the looper 7, the tension roller 8, the tail shear 9, the steering pinch roller 10 and the coiler 11 are sequentially distributed after the mechanical grinding system 5; after the oriented silicon steel thin strip 12 passes through the steering pinch roller 10, it is coiled by the coiler 11.
[0008] Furthermore, the system also includes an uncoiler 1, a steering pinch roller 2, a nine-roller straightener 3, and a crop shear 4; after the oriented silicon steel strip 12 is loaded onto the uncoiler 1, it enters the crop shear 4 under the action of the steering pinch roller 2 and the nine-roller straightener 3, and then enters the mechanical grinding system 5.
[0009] Furthermore, the wide-band sander 13 and the thickness gauge 14 are sequentially arranged behind the head shear 4; the PLC controller 15 and the display screen 16 are electrically connected to realize the processing and display of the detection data; the wide-band sander 13 is provided with an annular sanding belt and an abrasive roller above and below; the annular sanding belt is fastened to the surface of the abrasive roller and rotated by the driving motor.
[0010] Furthermore, the pickling system 6 includes a 1# pickling tank 21, a 2# pickling tank 22, an acid tank I19, an acid tank II 20, a rinsing tank and a drying box; the 1# pickling tank 21, the 2# pickling tank 22, the rinsing tank and the drying box are sequentially distributed after the mechanical polishing system 5; the acid tank II 20 is sequentially connected with the 2# pickling tank 22, the acid tank I19 and the 1# pickling tank 21 through a pipeline.
[0011] Furthermore, the pickling liquid in the 2# pickling tank 22 is used for pickling the oriented silicon steel strip 12, and then flows into the acid tank I19 through a pipeline for storage as the pickling liquid of the 1# pickling tank 21.
[0012] A method for efficiently preparing oriented silicon steel thin strip without bottom layer raw material by the system, characterized in that the method comprises the following steps:
[0013] S1: The hot-rolled billet is pickled to remove surface iron oxide and then rolled, and then decarburized, coated with a separator, annealed at high temperature, and hot stretched to obtain an oriented silicon steel strip 12 with a glass film bottom layer;
[0014] S2: The oriented silicon steel strip 12 enters the system, is unrolled, adjusted in direction, and then straightened, and then the redundant head area of the oriented silicon steel strip 12 is removed;
[0015] S3: After the redundant head area is removed, the oriented silicon steel strip 12 enters the mechanical grinding system 5, and the oriented silicon steel strip 12 passes through the gap between the annular abrasive belts arranged above and below to be ground. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14;
[0016] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16; when the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally and obtains the oriented silicon steel strip 12 without the bottom layer; otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without the bottom layer raw material.
[0017] Furthermore, in step S3, the mesh number of the annular sanding belts arranged up and down in the wide-band sanding machine 13 in the mechanical grinding system 5 is 80-200 meshes, and the conveying speed of the oriented silicon steel strip 12 during the grinding is 30-130 m / min.
[0018] Further, in step S4, the normal operation of the system is specifically as follows: when the thickness fluctuation value is within the preset thickness fluctuation value range, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in sequence for pickling, then enters the rinsing tank for rinsing, and then enters the drying box for drying, passes through the tension roller 8 after being corrected by the looper 7, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer.
[0019] Furthermore, the pickling solution used in the pickling is hydrochloric acid; the volume percentage concentration of the pickling solution is 25-40%; the pickling temperature is 60-90°C; the conveying speed of the oriented silicon steel strip 12 during the pickling is 30-130m / min, and the time is 0.6-2.6min.
[0020] The beneficial technical effects of the present invention are:
[0021] The present invention adopts a combination of mechanical grinding and pickling to continuously and efficiently prepare oriented silicon steel bottom layer-free raw materials online; a wide-band sander is used to continuously grind the bottom layer of the oriented silicon steel strip online, the thickness of the steel strip is detected in real time by a thickness gauge, and a PLC controller is used to feed back the uniformity of the steel strip thickness online. The oriented silicon steel strip is continuously pickled and rinsed by adopting a shallow flow turbulence method, that is, by increasing the flow rate of the pickling solution, the pickling solution flows on the surface of the oriented silicon steel strip to form turbulence, thereby promoting material transfer, causing the surface of the strip to heat up rapidly, and the turbulence effect causes the pickling solution in contact with the surface of the oriented silicon steel strip to be continuously renewed, thereby accelerating the reaction between the oriented silicon steel strip and the acid, and greatly improving the pickling efficiency; at the same time, the pickling tank is designed as a two-stage countercurrent structure, that is, new hydrochloric acid is input into the 2# pickling tank after heating from the acid tank II, and after the reaction, the hydrochloric acid in the 2# pickling tank enters the acid tank I, and then is heated and input into the 1# pickling tank. Therefore, the ground steel strip first enters the 1# pickling tank with the lowest concentration and the most turbidity for pickling, and then enters the 2# pickling tank with high concentration and high purity for cleaning, which is beneficial to improving the pickling efficiency and quality. The subsequent rinsing tank adopts shallow flow turbulent water washing, and the acid washing liquid remaining on the surface of the steel strip is washed away by the high flow rate of reverse water. The drying box adopts hot air drying method, that is, hot air heated by the heater is blown to the steel strip, taking away the water on the surface to obtain a dry steel strip.
[0022] The method of the present invention adopts a more mature and lower-cost sanding belt machine to grind the bottom layer of the oriented silicon steel thin strip, causing the bottom layer to rupture and creating conditions for the subsequent pickling solution to fully contact with the bottom layer. On the one hand, this avoids the problem of the sandblasting machines in CN109112395A being connected in series and requiring a large space; on the other hand, the subsequent pickling can remove stress without the need for stress relief annealing, which can significantly reduce production costs; on the other hand, the conveying speed of the steel strip reaches 30 to 130 m / min, has extremely high production efficiency, and can be mass-produced.
[0023] The present invention provides real-time feedback on the uniformity of the thickness of the steel strip after grinding by setting a PLC controller 15 in the mechanical grinding system 5, and adjusts the grinding thickness according to the feedback result, thereby realizing precise control of the plate shape of the oriented silicon steel thin strip. At the same time, the present invention provides a pickling system 6, and uses a shallow flow turbulence method to continuously pickle the oriented silicon steel thin strip after grinding by the mechanical grinding system 5, so that the pickling liquid can evenly and efficiently clean the remaining bottom layer, avoiding the problem of excessive cleaning of the thin strip matrix. In addition, the present invention optimizes and controls the process parameters of mechanical grinding and pickling, so that mechanical grinding and pickling are highly coordinated, and on the basis of effectively removing the bottom layer of oriented silicon steel, the removal efficiency of the bottom layer is greatly improved, thereby realizing the continuous production of oriented silicon steel raw materials without bottom layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the overall structure of the present invention.
[0025] In the figure: 1. Uncoiler; 2. Steering pinch roller; 3. Nine-roller straightener; 4. Head crop shear; 5. Mechanical grinding system; 6. Pickling system; 7. Looper; 8. Tension roller; 9. Tail crop shear; 10. Steering pinch roller; 11. Winder; 12. Oriented silicon steel strip; 13. Wide belt sander; 14. Thickness gauge; 15. PLC controller; 16. Display screen.
[0026] Figure 2 Schematic diagram of the flow pattern of the pickling liquid in the pickling system 6 of the present invention.
[0027] In the figure: 12, oriented silicon steel strip; 17, heater; 18, waste liquid pool; 19, acid tank I; 20, acid tank II; 21, 1# pickling tank, 22, 2# pickling tank. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.
[0030] It should be noted that, in the description of the present invention, unless otherwise specified, the terms "connection" and "setting" should be understood in a broad sense, for example, it can be a fixed connection, or a detachable connection or other connection methods. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0031] In the first aspect, the present invention provides a system for efficiently preparing oriented silicon steel strip without bottom layer raw materials, characterized in that the system includes a mechanical grinding system 5, a pickling system 6, a looper 7, a tension roller 8, a tail shear 9, a steering pinch roller 10, a winder 11 and an oriented silicon steel strip 12; the mechanical grinding system 5 includes a wide band sander 13, a thickness gauge 14, a PLC controller 15 and a display screen 16; the pickling system 6, the looper 7, the tension roller 8, the tail shear 9, the steering pinch roller 10, and the winder 11 are distributed in sequence after the mechanical grinding system 5; after the oriented silicon steel strip 12 passes through the steering pinch roller 10, it is wound by the winder 11.
[0032] In one example, the system also includes an uncoiler 1, a steering pinch roller 2, a nine-roll straightener 3, and a crop shear 4; after the oriented silicon steel strip 12 is loaded onto the uncoiler 1, it enters the crop shear 4 under the action of the steering pinch roller 2 and the nine-roll straightener 3, and then enters the mechanical grinding system 5.
[0033] In one of the examples, the wide-band sander 13 and the thickness gauge 14 are sequentially arranged behind the head shear 4; the PLC controller 15 and the display screen 16 are electrically connected to realize the processing and display of the detection data; the wide-band sander 13 is provided with annular sanding belts and sanding rollers on the upper and lower parts; the annular sanding belt is fastened on the surface of the sanding roller and rotated by the driving motor; the oriented silicon steel strip 12 passes through the gap between the annular sanding belts arranged on the upper and lower parts for grinding, and the thickness of the ground oriented silicon steel strip 12 is measured online by the thickness gauge 14, and the thickness data is displayed in real time on the display screen 16 and the thickness uniformity is fed back online through the PLC controller 15.
[0034] In one example, the pickling system 6 includes a 1# pickling tank 21, a 2# pickling tank 22, an acid tank I 19, an acid tank II 20, a rinsing tank and a drying box; the 1# pickling tank 21, the 2# pickling tank 22, the rinsing tank and the drying box are sequentially distributed after the mechanical polishing system 5; the acid tank II 20 is sequentially connected to the 2# pickling tank 22, the acid tank I 19 and the 1# pickling tank 21 through a pipeline.
[0035] In one example, the pickling liquid in the 2# pickling tank 22 is used for pickling the oriented silicon steel strip (12), and then flows into the acid tank I19 through a pipeline for storage as the pickling liquid of the 1# pickling tank 21.
[0036] In one example, the acid tank II 20 is filled with pickling liquid, and the pickling liquid in the acid tank II 20 enters the 2# pickling tank 22 through a pipeline. The pickling liquid in the 2# pickling tank 22 is used for the second pickling of the oriented silicon steel strip 12, and then enters the acid tank I19 through a pipeline for storage. The pickling liquid in the acid tank I19 enters the 1# pickling tank 21 through a pipeline, and is used as the pickling liquid of the 1# pickling tank 21 for the first pickling of the oriented silicon steel strip 12.
[0037] In a second aspect, the present invention further provides a method for efficiently preparing a raw material without a bottom layer of an oriented silicon steel thin strip by the above system, which specifically comprises the following steps:
[0038] S1: The hot-rolled billet is pickled to remove surface iron oxide, then rolled once, and then decarburized annealed, cold rolled twice, coated with a separator, annealed at high temperature, and hot stretched and flattened to obtain an oriented silicon steel strip 12 with a glass film bottom layer;
[0039] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the excess head area;
[0040] S3: After the redundant head area is removed, the oriented silicon steel strip 12 enters the mechanical grinding system 5, and the oriented silicon steel strip 12 passes through the gap between the annular abrasive belts arranged above and below to be ground. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14;
[0041] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16; when the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally and obtains the oriented silicon steel strip 12 without the bottom layer; otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without the bottom layer raw material.
[0042] In one of the examples, the specific method for preparing the oriented silicon steel strip 12 with a glass film bottom layer in step S1 is as follows: a hot-rolled strip with a thickness of 2.2 to 3.0 mm and a width of 1100 to 1250 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.55 to 0.80 mm by a single cold rolling; at a temperature of 800 to 900°C and a dew point temperature of 35-40°C, the carbon content in the strip is reduced to below 30 ppm by a mixed gas of wet nitrogen and hydrogen; the strip is rolled to a thickness of 0.15 to 0.35 mm by a secondary cold rolling; an isolation agent containing magnesium oxide and additives is coated on the surface of the strip; under the protection of a temperature of 1000 to 1100°C and ammonia decomposition gas, a magnesium silicate glass bottom layer is formed, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained.
[0043] In one example, in step S2, the redundant head area refers to the head area of the oriented silicon steel with poor quality. For example, due to the influence of the raw material composition and structure of the oriented silicon steel, the head area is prone to quality problems during the rolling process, such as edge cracking; during the shearing process, the edge of the strip undergoes work hardening due to plastic deformation, and this work hardening phenomenon is particularly obvious in the head area. Therefore, the head area of the oriented silicon steel with poor quality needs to be removed.
[0044] In one example, in step S3, the mesh number of the annular sanding belts arranged up and down in the wide-band sanding machine 13 in the mechanical grinding system 5 is 180-200 meshes, and the conveying speed of the oriented silicon steel strip 12 during the grinding is 30-130 m / min.
[0045] In one of the examples, in step S4, the normal operation of the system is specifically as follows: when the thickness fluctuation value is within the preset thickness fluctuation value range, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn for pickling, then enters the rinsing tank for rinsing, and then enters the drying box for drying. After being corrected by the looper 7, it passes through the tension roller 8, and then the direction is adjusted by the steering clamping roller 10, and the winding is achieved by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer.
[0046] In one example, the pickling solution used for pickling is hydrochloric acid; the volume percentage concentration of the pickling solution is 25-40%; the pickling temperature is 60-90°C; the conveying speed of the oriented silicon steel strip (12) during pickling is 30-130m / min, and the time is 0.6-2.6min.
[0047] In one of the examples, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0048] Example 1
[0049] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the system is as follows Figure 1 As shown, it includes an uncoiler 1, a steering pinch roller 2, a nine-roller straightener 3, a crop shear 4, a mechanical grinding system 5, a pickling system 6, a looper 7, a tension roller 8, a tail shear 9, a steering pinch roller 10, a coiler 11 and a oriented silicon steel strip 12; the pickling system 6, the looper 7, the tension roller 8, the tail shear 9, the steering pinch roller 10, and the coiler 11 are sequentially distributed after the mechanical grinding system 5; after the oriented silicon steel strip 12 passes through the steering pinch roller 10, it is coiled by the coiler 11; after the oriented silicon steel strip 12 is fed to the uncoiler 1, it enters the crop shear 4 under the action of the steering pinch roller 2 and the nine-roller straightener 3, and then enters the mechanical grinding system 5.
[0050] The mechanical grinding system 5 includes a wide-band sanding machine 13, a thickness gauge 14, a PLC controller 15 and a display screen 16; the wide-band sanding machine 13 and the thickness gauge 14 are sequentially arranged behind the head shear 4; the PLC controller 15 and the display screen 16 are electrically connected to realize the processing and display of the detection data; the wide-band sanding machine 13 is provided with annular sanding belts and sanding rollers on the upper and lower sides; the annular sanding belt is fastened on the surface of the sanding roller and rotated by the driving motor; the oriented silicon steel strip 12 passes through the gap between the annular sanding belts arranged on the upper and lower sides for grinding, and the thickness of the oriented silicon steel strip 12 after grinding is measured online by the thickness gauge 14, and the thickness data is displayed in real time on the display screen 16 and the thickness uniformity is fed back online through the PLC controller 15.
[0051] The pickling system 6 includes a 1# pickling tank 21, a 2# pickling tank 22, an acid tank I19, an acid tank II 20, a rinsing tank and a drying box; the 1# pickling tank 21, the 2# pickling tank 22, the rinsing tank and the drying box are sequentially distributed after the mechanical polishing system 5; the acid tank II 20 is sequentially connected with the 2# pickling tank 22, the acid tank I19 and the 1# pickling tank 21 through a pipeline.
[0052] The flow mode of the pickling liquid in the pickling system 6 is as follows Figure 2 As shown, the acid tank II 20 is filled with pickling liquid, and the pickling liquid in the acid tank II 20 enters the 2# pickling tank 22 through a pipeline. The pickling liquid in the 2# pickling tank 22 is used for the second pickling of the oriented silicon steel strip 12, and then enters the acid tank I19 for storage through a pipeline. The pickling liquid in the acid tank I19 enters the 1# pickling tank 21 through a pipeline, and is used as the pickling liquid of the 1# pickling tank 21 for the first pickling of the oriented silicon steel strip 12.
[0053] A method for efficiently preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0054] S1: A hot-rolled strip with a thickness of 2.2 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.60 mm by a single cold rolling; the carbon content in the strip is reduced to 25 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 850°C and a dew point of 38°C; the strip is rolled to a thickness of 0.23 mm by a secondary cold rolling; an insulating agent containing 95% by mass of magnesium oxide and 5% by mass of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1100°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0055] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0056] S3: After the head area with poor quality is removed, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 31 m / min, the oriented silicon steel strip 12 passes through the gap between the 200-mesh annular sanding belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.22 mm.
[0057] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16. When the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally. At a conveying speed of 31 m / min, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn. The pickling liquid pickles the oriented silicon steel strip 12 in a shallow flow turbulent manner for 2.5 minutes, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying. After being corrected by the looper 7, it passes through the tension roller 8, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer. Otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0058] Further, in step S4, the pickling solution is hydrochloric acid with a temperature of 80° C. and a volume percentage concentration of 31%;
[0059] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0060] Example 2
[0061] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the structure of the system is the same as that of Example 1.
[0062] A method for efficiently preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0063] S1: A hot-rolled strip with a thickness of 3.0 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.80 mm by a single cold rolling; the carbon content in the strip is reduced to 30 ppm by a wet mixed gas of 70% nitrogen and 30% hydrogen at a temperature of 880°C and a dew point of 35°C; the strip is rolled to a thickness of 0.35 mm by a secondary cold rolling; an insulating agent containing 95% by mass of magnesium oxide and 5% by mass of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1000°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0064] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0065] S3: After the head area with poor quality is removed, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 40 m / min, the oriented silicon steel strip 12 passes through the gap between the 200-mesh annular abrasive belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.34 mm.
[0066] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16. When the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally. At a conveying speed of 40 m / min, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn. The pickling liquid pickles the oriented silicon steel strip 12 for 2 minutes in a shallow flow turbulent manner, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying. After being corrected by the looper 7, it passes through the tension roller 8, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer. Otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0067] Further, in step S4, the pickling solution is hydrochloric acid with a temperature of 70° C. and a volume percentage concentration of 25%;
[0068] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0069] Comparative Example 1
[0070] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the structure of the system is the same as that of Example 1.
[0071] A method for efficiently preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0072] S1: A hot-rolled strip with a thickness of 2.6 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.62 mm by a single cold rolling; the carbon content in the strip is reduced to 27 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 830°C and a dew point of 40°C; the strip is rolled to a thickness of 0.27 mm by a secondary cold rolling; an insulating agent containing 95% by mass of magnesium oxide and 5% by mass of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1050°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0073] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0074] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 30 m / min, the oriented silicon steel strip 12 passes through the gap between the 200-mesh annular sanding belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.26 mm.
[0075] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16. When the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally. At a conveying speed of 30 m / min, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn. The pickling liquid pickles the oriented silicon steel strip 12 in a shallow flow turbulent manner for 2.6 minutes, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying. After being corrected by the looper 7, it passes through the tension roller 8, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer. Otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0076] Further, in step S4, the pickling solution is hydrochloric acid with a temperature of 70° C. and a volume percentage concentration of 20%;
[0077] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0078] Comparative Example 2
[0079] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the structure of the system is the same as that of Example 1.
[0080] A method for efficiently preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0081] S1: A hot-rolled strip with a thickness of 2.5 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.65 mm by a single cold rolling; the carbon content in the strip is reduced to 28 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 830°C and a dew point of 40°C; the strip is rolled to a thickness of 0.23 mm by a secondary cold rolling; an insulating agent containing 95% by mass of magnesium oxide and 5% by mass of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed under the protection of ammonia decomposition gas at a temperature of 1100°C, and after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0082] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0083] S3: After the head area with poor quality is removed, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 180 m / min, the oriented silicon steel strip 12 passes through the gap between the 200-mesh annular sanding belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.22 mm.
[0084] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16. When the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally. At a conveying speed of 180 m / min, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn. The pickling liquid pickles the oriented silicon steel strip 12 in a shallow flow turbulent manner for 0.4 min, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying. After being corrected by the looper 7, it passes through the tension roller 8, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer. Otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0085] Further, in step S4, the pickling solution is hydrochloric acid with a temperature of 70° C. and a volume percentage concentration of 25%;
[0086] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0087] Comparative Example 3
[0088] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the structure of the system is the same as that of Example 1.
[0089] A method for efficiently preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0090] S1: A hot-rolled strip with a thickness of 2.6 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.70 mm by a single cold rolling; the carbon content in the strip is reduced to 30 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 830°C and a dew point of 40°C; the strip is rolled to a thickness of 0.23 mm by a secondary cold rolling; an insulating agent containing 95% by mass of magnesium oxide and 5% by mass of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed under the protection of ammonia decomposition gas at a temperature of 1000°C, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0091] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0092] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 180 m / min, the oriented silicon steel strip 12 passes through the gap between the 100-mesh annular abrasive belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.22 mm.
[0093] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays it on the display screen 16. When the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally. At a conveying speed of 180 m / min, the oriented silicon steel strip 12 enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn. The pickling liquid pickles the oriented silicon steel strip 12 in a shallow flow turbulent manner for 0.4 min, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying. After being corrected by the looper 7, it passes through the tension roller 8, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer. Otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0094] Further, in step S4, the pickling solution is hydrochloric acid with a temperature of 70° C. and a volume percentage concentration of 25%;
[0095] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0096] Comparative Example 4
[0097] A method for preparing a raw material without a bottom layer of oriented silicon steel thin strip by mechanical grinding,
[0098] The specific steps include:
[0099] S1: A hot-rolled strip with a thickness of 2.2 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.60 mm by a single cold rolling; the carbon content in the strip is reduced to 25 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 850°C and a dew point of 38°C; the strip is rolled to a thickness of 0.22 mm by a secondary cold rolling; an isolating agent containing an isolating agent of 95% by mass magnesium oxide and 5% borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1100°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0100] S2: The oriented silicon steel strip 12 enters the system (the structure of the system is the same as that of Example 1, but the oriented silicon steel strip 12 is controlled not to enter the pickling system), firstly uncoiled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening treatment, and then the oriented silicon steel strip 12 is removed from the head area with poor quality by the head shear 4;
[0101] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 5m / min, the oriented silicon steel strip 12 passes through the gap between the 100-mesh annular sand belts arranged above and below for grinding. The thickness is measured online by the thickness gauge 14, and the oriented silicon steel strip is ground to 0.21mm.
[0102] S4: The oriented silicon steel strip 12 enters the pickling system 6 at a conveying speed of 5m / min (the oriented silicon steel strip 12 enters the subsequent steps directly without pickling treatment) for 16 minutes, and then passes through the tension roller 8 after being corrected by the looper 7, and then adjusts the direction through the steering pinch roller 10, and is wound by the winder 11.
[0103] Comparative Example 5
[0104] A method for preparing a raw material without a bottom layer of an oriented silicon steel thin strip by mechanical grinding, specifically comprising the following steps:
[0105] S1: A hot-rolled strip with a thickness of 2.5 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.65 mm by a single cold rolling; the carbon content in the strip is reduced to 28 ppm by a wet mixed gas of 75% nitrogen and 25% hydrogen at a temperature of 860°C and a dew point of 39°C; the strip is rolled to a thickness of 0.23 mm by a secondary cold rolling; an insulating agent containing 95% by mass of magnesium oxide and 5% by mass of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1050°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0106] S2: The oriented silicon steel strip 12 enters the system (the structure of the system is the same as that of Example 1, but the oriented silicon steel strip 12 is controlled not to be pickled), firstly uncoiled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening, and then the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0107] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 2m / min, the oriented silicon steel strip 12 passes through the gap between the 200-mesh annular sanding belts arranged above and below for grinding. The thickness is measured online by the thickness gauge 14, and the oriented silicon steel strip is ground to 0.21mm.
[0108] S4: The oriented silicon steel strip 12 then enters the pickling system 6 at a conveying speed of 2m / min (the oriented silicon steel strip 12 enters the subsequent steps directly without pickling treatment) for 40min, and then passes through the tension roller 8 after being corrected by the looper 7, and then adjusts the direction through the steering pinch roller 10, and is wound by the winder 11.
[0109] Comparative Example 6
[0110] A method for preparing a raw material without a bottom layer of an oriented silicon steel thin strip by pickling, specifically comprising the following steps:
[0111] S1: A hot-rolled strip with a thickness of 2.2 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.60 mm by a single cold rolling; the carbon content in the strip is reduced to 25 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 850°C and a dew point of 38°C; the strip is rolled to a thickness of 0.22 mm by a secondary cold rolling; an isolating agent containing 95% by mass of magnesium oxide and 5% of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1000°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0112] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0113] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 at a conveying speed of 5m / min (the oriented silicon steel strip 12 is not ground), and enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 at a conveying speed of 5m / min in sequence, and is pickled for 16 minutes by a 40% hydrochloric acid solution at 70°C in a shallow flow turbulent manner, and then enters the rinsing tank at a conveying speed of 5m / min for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying, and after being corrected by the looper 7, passes through the tension roller 8, and then adjusts the direction by the steering pinch roller 10, and is wound by the winder 11.
[0114] Comparative Example 7
[0115] A method for preparing a raw material without a bottom layer of an oriented silicon steel thin strip by pickling, specifically comprising the following steps:
[0116] S1: A hot-rolled strip with a thickness of 2.5 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.62 mm by a single cold rolling; the carbon content in the strip is reduced to 30 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 840°C and a dew point of 40°C; the strip is rolled to a thickness of 0.23 mm by a secondary cold rolling; an isolating agent containing 95% by mass of magnesium oxide and 5% of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1100°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0117] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0118] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 at a conveying speed of 2m / min (the oriented silicon steel strip 12 is not ground), and enters the 1# pickling tank 21 and the 2# pickling tank 22 in the pickling system 6 in turn at a conveying speed of 2m / min, and the oriented silicon steel strip 12 is pickled for 40 minutes by a 30% hydrochloric acid solution at 80°C in a shallow flow turbulent manner, and then enters the rinsing tank at a conveying speed of 2m / min for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying, and after being corrected by the looper 7, passes through the tension roller 8, and then adjusts the direction by the steering pinch roller 10, and is wound by the winder 11.
[0119] Comparative Example 8
[0120] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the structure of the system is the same as that of Example 1.
[0121] A method for preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0122] S1: A hot-rolled strip with a thickness of 2.4 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.60 mm by a single cold rolling; the carbon content in the strip is reduced to 30 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 830°C and a dew point of 40°C; the strip is rolled to a thickness of 0.26 mm by a secondary cold rolling; an isolating agent containing 95% by mass of magnesium oxide and 5% of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1100°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0123] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0124] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 30 m / min, the oriented silicon steel strip 12 passes through the gap between the 200-mesh annular abrasive belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.25 mm.
[0125] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays the feedback through the display screen 16; when the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally, and at a conveying speed of 30m / min, the oriented silicon steel strip 12 enters the 1# pickling tank and the 2# pickling tank in the pickling system 6 in turn, and the pickling liquid pickles the oriented silicon steel strip 12 for 2.6min in a shallow flow turbulent manner, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying, and passes through the tension roller 8 after being corrected by the looper 7, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer; otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0126] Further, in step S4, the pickling solution is a sulfuric acid solution with a temperature of 70° C. and a volume percentage concentration of 30%;
[0127] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0128] Comparative Example 9
[0129] A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, the structure of the system is the same as that of Example 1.
[0130] A method for preparing a oriented silicon steel thin strip without a bottom layer raw material using the above system specifically comprises the following steps:
[0131] S1: A hot-rolled strip with a thickness of 2.4 mm and a width of 1200 mm is pickled to remove surface iron oxide; the hot-rolled strip is rolled to a thickness of 0.60 mm by a single cold rolling; the carbon content in the strip is reduced to 30 ppm by a wet mixed gas of 80% nitrogen and 20% hydrogen at a temperature of 830°C and a dew point of 40°C; the strip is rolled to a thickness of 0.26 mm by a secondary cold rolling; an isolating agent containing 95% by mass of magnesium oxide and 5% of borate is coated on the surface of the strip; a magnesium silicate glass bottom layer is formed at a temperature of 1100°C and under the protection of ammonia decomposition gas, and then after hot stretching and flattening, an oriented silicon steel strip 12 with a glass film bottom layer is obtained;
[0132] S2: The oriented silicon steel strip 12 enters the system, is first unrolled by the uncoiler 1, then adjusted in direction by the steering pinch roller 2, and then horizontally enters the nine-roller straightening machine 3 for straightening. Subsequently, the oriented silicon steel strip 12 passes through the head shear 4 to remove the head area with poor quality;
[0133] S3: After removing the head area with poor quality, the oriented silicon steel strip 12 enters the mechanical grinding system 5 again. At a conveying speed of 30m / min, the oriented silicon steel strip 12 passes through the gap between the 100-mesh annular sanding belts arranged above and below for grinding. The thickness of the ground oriented silicon steel strip 12 is measured online by a thickness gauge 14, and the thickness of the oriented silicon steel strip 12 is measured to be 0.25mm.
[0134] S4: The PLC controller 15 calculates the thickness fluctuation value of the oriented silicon steel strip 12 in real time and displays the feedback through the display screen 16; when the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally, and at a conveying speed of 30m / min, the oriented silicon steel strip 12 enters the 1# pickling tank and the 2# pickling tank in the pickling system 6 in turn, and the pickling liquid pickles the oriented silicon steel strip 12 for 2.6min in a shallow flow turbulent manner, and then enters the rinsing tank for rinsing in a shallow flow turbulent manner, and then enters the drying box for hot air drying, and passes through the tension roller 8 after being corrected by the looper 7, and then adjusts the direction through the steering pinch roller 10, and is wound up by the winder 11 to obtain an oriented silicon steel strip 12 without a bottom layer; otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
[0135] Further, in step S4, the pickling solution is a nitric acid solution with a temperature of 70° C. and a volume percentage concentration of 30%;
[0136] Furthermore, in step S4, the logic analysis in the PLC controller 15 calculates and extracts the real-time thickness fluctuation value online, and automatically compares the real-time thickness fluctuation value with the thickness fluctuation value range set by the system; when the real-time thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain a bottom-free oriented silicon steel strip 12; otherwise, the system alarm platform is activated and the production of abnormal oriented silicon steel strip without bottom-layer raw materials is terminated.
[0137] Table 1 Results of the oriented silicon steel bottom layer in the embodiments and comparative examples
[0138]
[0139] From the results in Table 1, it can be seen that compared with Comparative Example 1, which cannot completely remove the bottom layer due to the low concentration of the pickling solution, and Comparative Examples 2-3, which cannot be fully polished and pickled due to the high conveying speed, the present invention optimizes the mesh size of the sanding belt, the conveying speed, the concentration of the pickling solution and the temperature during mechanical polishing, so that each parameter is efficiently coordinated to achieve efficient removal of the bottom layer of the oriented silicon steel strip. At the same time, Comparative Examples 8-9 respectively use sulfuric acid and nitric acid as pickling solutions, and part of the magnesium silicate bottom layer still remains on the surface of the oriented silicon steel strip. This is because sulfuric acid and nitric acid react strongly with the substrate of the oriented silicon steel strip, causing the substrate of the oriented silicon steel strip to be excessively corroded and deformed. The present invention effectively removes the glass film bottom layer of the oriented silicon steel strip without damaging the substrate of the oriented silicon steel strip by screening the type of pickling solution.
[0140] The present invention adopts a combination of mechanical grinding and pickling to continuously and efficiently prepare oriented silicon steel bottom layer-free raw materials online; a wide-band sander is used to continuously grind the bottom layer of the oriented silicon steel strip online, the thickness of the steel strip is detected in real time by a thickness gauge, and a PLC controller is used to feed back the uniformity of the steel strip thickness online. The oriented silicon steel strip is continuously pickled and rinsed by adopting a shallow flow turbulent mode, that is, by increasing the flow rate of the pickling solution, the pickling solution is made to flow on the surface of the oriented silicon steel strip to form turbulence, thereby promoting material transfer, causing the surface of the strip to heat up rapidly, and the pickling solution in contact with the surface of the oriented silicon steel strip is continuously renewed by the turbulent effect, thereby accelerating the reaction between the oriented silicon steel strip and the acid, and greatly improving the pickling efficiency; at the same time, the pickling tank is designed as a two-stage countercurrent structure, that is, new hydrochloric acid is input into the 2# pickling tank after heating from the acid tank II 20, and after the reaction, the hydrochloric acid in the 2# pickling tank enters the acid tank I19, and then is heated and input into the 1# pickling tank, therefore, the steel strip after grinding first enters the 1# pickling tank with the lowest concentration and the most turbidity for pickling, and then enters the 2# pickling tank with high concentration and high purity for cleaning, which is beneficial to improving the pickling efficiency and quality. The subsequent rinsing tank adopts shallow flow turbulent water washing, and the acid washing liquid remaining on the surface of the steel strip is washed away by the high flow rate of reverse water. The drying box adopts hot air drying method, that is, hot air heated by the heater is blown to the steel strip, taking away the water on the surface to obtain a dry steel strip.
[0141] The method of the present invention adopts a more mature and lower-cost sanding belt machine to grind the bottom layer of the oriented silicon steel thin strip, causing the bottom layer to rupture and creating conditions for the subsequent pickling solution to fully contact with the bottom layer. On the one hand, this avoids the problem of the sandblasting machines in CN109112395A being connected in series and requiring a large space; on the other hand, the subsequent pickling can remove stress without the need for stress relief annealing, which can significantly reduce production costs; on the other hand, the conveying speed of the steel strip reaches 30 to 130 m / min, has extremely high production efficiency, and can be mass-produced.
[0142] The present invention provides real-time feedback on the uniformity of the thickness of the steel strip after grinding by setting a PLC controller 15 in the mechanical grinding system 5, and adjusts the grinding thickness according to the feedback result, thereby realizing precise control of the plate shape of the oriented silicon steel thin strip. At the same time, the present invention provides a pickling system 6, and uses a shallow flow turbulence method to continuously pickle the oriented silicon steel thin strip after grinding by the mechanical grinding system 5, so that the pickling liquid can evenly and efficiently clean the remaining bottom layer, avoiding the problem of excessive cleaning of the thin strip matrix. In addition, the present invention optimizes and controls the process parameters of mechanical grinding and pickling, so that mechanical grinding and pickling are highly coordinated, and on the basis of effectively removing the bottom layer of oriented silicon steel, the removal efficiency of the bottom layer is greatly improved, thereby realizing the continuous production of oriented silicon steel raw materials without bottom layer.
[0143] The above is only a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It is understood that other improvements and changes directly derived or associated by those skilled in the art without departing from the spirit and concept of the present invention should be considered to be included in the protection scope of the present invention.
Claims
1. A system for efficiently preparing oriented silicon steel thin strip without bottom layer raw material, characterized in that: The system comprises a mechanical grinding system (5), a pickling system (6), a looper (7), a tension roller (8), a tail cutting shear (9), a steering pinch roller (10), a coiler (11) and a oriented silicon steel strip (12); the mechanical grinding system (5) comprises a wide-band sanding machine (13), a thickness gauge (14), a PLC controller (15) and a display screen (16); the pickling system (6), the looper (7), the tension roller (8), the tail cutting shear (9), the steering pinch roller (10) and the coiler (11) are sequentially arranged after the mechanical grinding system (5); and after the oriented silicon steel strip (12) passes through the steering pinch roller (10), it is coiled by the coiler (11).
2. The system according to claim 1, characterized in that The system further comprises an uncoiler (1), a steering pinch roller (2), a nine-roller straightener (3), and a crop shear (4); after the oriented silicon steel thin strip (12) is loaded onto the uncoiler (1), it enters the crop shear (4) under the action of the steering pinch roller (2) and the nine-roller straightener (3), and then enters the mechanical grinding system (5).
3. The system according to claim 1, characterized in that The wide-band sanding machine (13) and the thickness gauge (14) are sequentially arranged behind the crop shear (4); the PLC controller (15) and the display screen (16) are electrically connected to realize the processing and display of the detection data; the wide-band sanding machine (13) is provided with an annular sanding belt and an abrasive roller above and below; the annular sanding belt is fastened to the surface of the abrasive roller and rotates under the drive of a driving motor.
4. The system according to claim 1, characterized in that The pickling system (6) comprises a 1# pickling tank (21), a 2# pickling tank (22), an acid tank I (19), an acid tank II (20), a rinsing tank and a drying box; the 1# pickling tank (21), the 2# pickling tank (22), the rinsing tank and the drying box are sequentially distributed after the mechanical polishing system (5); the acid tank II (20) is sequentially connected to the 2# pickling tank (22), the acid tank I (19) and the 1# pickling tank (21) through a pipeline.
5. The system according to claim 4, characterized in that The pickling liquid in the 2# pickling tank (22) is used for pickling the oriented silicon steel strip (12), and then flows into the acid tank I (19) through a pipeline for storage as the pickling liquid of the 1# pickling tank (21).
6. A method for efficiently preparing oriented silicon steel thin strip without bottom layer raw material using the system according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1: The hot-rolled billet is pickled to remove surface iron oxide and then rolled, and then decarburized, coated with a separator, annealed at high temperature, and hot stretched to obtain an oriented silicon steel strip (12) with a glass film bottom layer; S2: the oriented silicon steel strip (12) enters the system, is unrolled, has its direction adjusted, and is then straightened, and then the redundant head area of the oriented silicon steel strip (12) is removed; S3: After the redundant head area is removed, the oriented silicon steel thin strip (12) enters the mechanical grinding system (5), and the oriented silicon steel thin strip (12) passes through the gap between the annular grinding belts arranged above and below to be ground. The thickness of the ground oriented silicon steel thin strip (12) is measured online by a thickness gauge (14); S4: The PLC controller (15) calculates in real time and displays and feeds back the thickness fluctuation value of the oriented silicon steel strip (12) through the display screen (16); when the thickness fluctuation value is within the preset thickness fluctuation value range, the system operates normally to obtain an oriented silicon steel strip (12) without a bottom layer; otherwise, the system alarm platform is activated to terminate the production of abnormal oriented silicon steel strip without a bottom layer raw material.
7. The method according to claim 6, characterized in that In step S3, the mesh number of the annular sanding belts arranged up and down in the wide-band sanding machine (13) in the mechanical grinding system (5) is 80 to 200 meshes, and the conveying speed of the oriented silicon steel strip (12) during grinding is 30 to 130 m / min.
8. The method according to claim 6, characterized in that In step S4, the normal operation of the system is specifically as follows: when the thickness fluctuation value is within a preset thickness fluctuation value range, the oriented silicon steel strip (12) sequentially enters the 1# pickling tank (21) and the 2# pickling tank (22) in the pickling system (6) for pickling, then enters the rinsing tank for rinsing, and then enters the drying box for drying, passes through the tension roller (8) after being corrected by the looper (7), and then adjusts the direction by the steering pinch roller (10), and is wound up by the winder (11) to obtain an oriented silicon steel strip (12) without a bottom layer.
9. The method according to claim 8, characterized in that The pickling solution used in the pickling is hydrochloric acid; the volume percentage concentration of the pickling solution is 25-40%; the pickling temperature is 60-90°C; the conveying speed of the oriented silicon steel strip (12) during the pickling is 30-130m / min, and the time is 0.6-2.6min.
Citation Information
Patent Citations
Assembly and method for grinding a metal strip
CN105073339A
Cold-rolled aluminum steel composite strip production device and application thereof
CN105537290A
Method for preparing bottom-layer-free raw material of oriented silicon steel thin strip in physical sand blasting manner
CN113211325A
Non-oriented silicon steel sheet and preparation method thereof
CN116689486A
Method for continuously pickling common oriented silicon steel
CN116875987A