Casting technology of thin-walled grey iron castings and thin-walled grey iron castings

By using a combination of ferrosilicon incubator, strontium silicon incubator and accelerator in the casting molding process of thin-wall gray castings, the pore and white mouth problems of thin-wall castings are solved, and the content of A-type graphite and pearlite is improved , improves the overall quality of the castings.

CN118808568BActive Publication Date: 2024-12-06ANHUI HELI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411314315.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-06
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Large-size, high-drop thin-wall castings are prone to pore defects and white mouth problems during casting, and the existing technology is difficult to effectively solve.

Method used

The casting molding process of thin-walled gray cast iron parts is adopted. The first incubator and second incubator are added respectively through the steps of incubation of iron and incubation with the flow, including ferrosilicon incubator, strontium silicon incubator and promoter, and their quality is adjusted. The ratio and particle size are to increase the A-type graphite and pearlite content of the casting.

Benefits of technology

It effectively solves the pore defects and white mouth problems of thin-wall castings, and at the same time improves the A-type graphite and pearlite content of the castings, improving the overall quality of the castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808568B_ABST
    Figure CN118808568B_ABST
Patent Text Reader

Abstract

The invention discloses a casting forming process of a thin-walled grey iron casting and the thin-walled grey iron casting. The process obtains the thin-walled grey iron casting by smelting molten iron, refining molten iron, ladle inoculation, inverted ladle flow inoculation and casting forming. A primary inoculant is added in the ladle inoculation step, the primary inoculant comprises a ferrosilicon inoculant, a silicon strontium inoculant and an accelerator, the accelerator comprises a silicon-barium inoculant of 20% by mass, a silicon-zirconium inoculant of 10%, ferromanganese of 10% and vanadium of 1% by mass, and the remainder is ferrosilicon. The ferrosilicon is selected from FeSi75-B or FeSi75-A or a combination of the two, and the ferromanganese is selected from FeMn68. A secondary inoculant is added in the inverted ladle flow inoculation step, the secondary inoculant is a silicon strontium inoculant, the particle size of the silicon strontium inoculant in the primary inoculant is 3-8 mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2-0.8 mm. The present application can effectively solve the problems of pore defects and chilling tendency at thin-walled parts of castings, while ensuring that the castings have a higher content of A-type graphite and pearlite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal casting, and in particular relates to a casting molding process of a thin-walled grey iron casting and the thin-walled grey iron casting. Background Art

[0002] The gearbox housing on the backhoe loader is a casting with a large-scale thin-wall structure. The outer contour dimensions are large, with the maximum and minimum contour dimensions both reaching tens of centimeters, and the minimum wall thickness is only a few millimeters. This type of casting has obvious thin-wall characteristics and large height differences. The conventional top casting process is prone to casting defects such as sand blasting and slag inclusion.

[0003] The inventor improved the process and adopted a bottom casting process. The casting system includes multiple ingates and a cross runner. The cross runner is connected to the straight runner. The cross runner surrounds the periphery of the casting and is connected to the casting cavity through multiple ingates. This has a very obvious improvement effect on casting defects such as sand blasting and slag inclusion caused by conventional casting processes.

[0004] But it also brings new problems. After adopting the bottom casting process, the thin-walled part is prone to pore defects and white cast tendencies, and this situation has not been effectively improved.

[0005] Prior art document CN 103572139 A discloses a composite inoculation method for small thin-walled castings, comprising the following processes: in a vertical parting flaskless shot-pressing molding line, molten iron is smelted in a medium frequency furnace in the form of scrap steel, a carburizer and recycled materials; in production, a primary inoculant accounting for 0.2% of its weight is added to each bag of molten iron; in continuous inoculation, a strontium-containing inoculant accounting for 0.1% of its weight is added to each mold pouring weight; the metallographic structure of the finally produced thin-walled casting is mainly graphite type A (more than 80%) and pearlite is more than 90%, and can effectively prevent white cast iron.

[0006] However, in the process of applying the above-mentioned prior art, the inventors found that the huge differences in the shape and size of the castings and the differences in the pressure during molding resulted in some substantial differences in the filling effect and cooling effect of the thin-walled parts, and could not effectively improve the pores and white spots in the thin-walled parts of the gearbox housing in this application. Summary of the invention

[0007] Aiming at the problem that the above-mentioned gearbox housing or similar large-sized, high-drop, and thin-walled castings are prone to porosity defects and white cast iron tendencies during the casting process, the present application proposes a casting molding process and a thin-walled gray iron casting.

[0008] The specific technical solutions are as follows:

[0009] The casting process of thin-walled gray iron castings is to obtain thin-walled gray iron castings by melting molten iron, refining molten iron, ladle inoculation, ladle flow inoculation, and casting;

[0010] A primary inoculant is added in the ladle inoculation step, wherein the primary inoculant includes a ferrosilicon inoculant, a silicon strontium inoculant and a promoter, wherein the promoter includes a silicon-barium inoculant of 20% by mass, a silicon-zirconium inoculant of 10% by mass, a ferromanganese of 10% by mass, and a vanadium inoculant of 10% by mass, with the remainder being ferrosilicon; the ferrosilicon is selected from FeSi75-B or FeSi75-A or a combination of the two, and the ferromanganese is selected from FeMn68;

[0011] A secondary inoculant is added in the inverted package flow inoculation step, wherein the secondary inoculant is a silicon strontium inoculant, the particle size of the silicon strontium inoculant in the primary inoculant is 3-8 mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2-0.8 mm.

[0012] In some embodiments with better effects, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron. Appropriately increasing the amount of the inoculant can help improve the effect.

[0013] In some embodiments with better effects, the mass ratio of the ferrosilicon inoculant, the strontium silicon inoculant and the accelerator in the primary inoculant is 1:1:(2-3.5).

[0014] In some embodiments with better effects, the mass ratio of the ferrosilicon inoculant, the strontium silicon inoculant and the accelerator in the primary inoculant is 1:1:(2.5~3).

[0015] In some embodiments with better effects, the strontium content of the silicon-strontium inoculant in the primary inoculant is greater than 1%, and the strontium content of the silicon-strontium inoculant in the secondary inoculant is greater than 1.3%.

[0016] In some embodiments with better effects, the strontium content of the silicon-strontium inoculant in the primary inoculant is 1.1%, and the strontium content of the silicon-strontium inoculant in the secondary inoculant is 1.5%.

[0017] In addition, the present application also provides a thin-walled grey iron casting, which is cast by the casting process described above.

[0018] The beneficial effects of the present invention are as follows: for thin-walled gray iron castings with obvious thin-wall characteristics and large height difference, while adopting the bottom casting process to solve the casting defects such as sand blasting and slag inclusion, by respectively adding the primary inoculant and the secondary inoculant in the ladle inoculation and the inverted ladle flow inoculation steps, the porosity defects and the white cast iron tendency problems at the thin wall of the casting can be effectively solved, and at the same time, it can be ensured that the casting has a higher content of type A graphite and pearlite. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Shown is a schematic diagram of the structure of the gearbox housing;

[0020] Figure 2 Shown are the pores on the casting surface produced in Example 1;

[0021] Figure 3 Shown is the metallographic structure diagram of the graphite morphology of the casting in Example 1;

[0022] Figure 4 Shown is the metallographic structure diagram of the carburized layer of the casting in Example 1;

[0023] Figure 5 Shown are pinholes in the casting produced in Example 2;

[0024] Figure 6 Shown are pinholes in the casting produced in Example 3;

[0025] Figure 7 Shown is the metallographic structure diagram of the graphite morphology of the casting in Example 3;

[0026] Figure 8 Shown is the metallographic structure diagram of the graphite morphology of the casting in Example 5;

[0027] Fig. 9 Shown is the metallographic structure diagram of the graphite morphology of the casting of Example 11;

[0028] Fig.10 Shown is the metallographic structure diagram of the carburized layer of the casting of Example 11;

[0029] Fig.11 Shown is the metallographic structure diagram of the graphite morphology of the casting of Example 8;

[0030] Fig.12 Shown is the metallographic structure of the carburized layer of the casting of Example 8. DETAILED DESCRIPTION

[0031] Figure 1 The structure diagram of the gearbox housing 100 on the backhoe loader is shown, which is a casting with a large-scale thin-wall structure, and the outer contour size is 605*579*302mm. Figure 1 The area A in the middle is a relatively obvious large-scale thin-walled structure. In addition to this area, the gearbox housing 100 also has other thin-walled structures. The minimum wall thickness of the thin-walled structure of the gearbox housing 100 is only 6 mm. This type of casting has obvious thin-wall characteristics and large height difference. The conventional top casting process is prone to casting defects such as sand blasting and slag inclusion. Figure 1The bottom casting process is shown in FIG. 1 , in which the runner structure 200 is connected to the bottom of the casting cavity.

[0032] The casting method of the thin-walled grey iron casting provided by the invention comprises the following steps in sequence: smelting molten iron, allowing the molten iron to stand, inoculating in a molten iron ladle, inoculating with the ladle flow, and casting.

[0033] Among them, smelting molten iron is to melt scrap steel, recycled materials, ferrosulfide alloy, ferromanganese alloy, ferrochrome alloy and ferrosilicon alloy into molten iron.

[0034] Conventional processes are used for molten iron and for its static state. The temperature of the molten iron is controlled between 1520 and 1550°C and is kept warm for more than 10 minutes.

[0035] Ladle inoculation: Add a specified amount of inoculant to the molten iron after it has been stationary, based on the total mass of the molten iron, and perform an inoculation treatment.

[0036] Inoculation during pouring: During the pouring process of molten iron after the completion of the first inoculation, a specified amount of inoculant is added according to the total mass of the molten iron for secondary inoculation. After the inoculation, the molten iron enters the next step for casting and molding.

[0037] During the casting step, the temperature is controlled between 1420 and 1440°C, and the molding is performed by natural cooling.

[0038] Before the ladle is inoculated, the composition of the molten iron in front of the furnace is analyzed to control the mass percentage content of the chemical composition in front of the furnace to be: C3.2%, Si1.6%, Mn0.78%, S0.035%, P0.03%. Unless otherwise specified, the composite components recorded in the embodiments of the present application are expressed in mass percentage.

[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments.

[0040] Comparative Example 1

[0041] The gearbox housing is obtained by adopting the process steps of smelting molten iron, refining molten iron, ladle inoculation, inverted ladle inoculation and casting as recorded in this application, wherein a primary inoculant is added in the ladle inoculation step, and a secondary inoculant is used in the inverted ladle inoculation step, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron.

[0042] The primary inoculant is composed of 75 ferrosilicon inoculant and silicon strontium inoculant in a mass ratio of 1:1, and the secondary inoculant is a silicon strontium inoculant. The same silicon strontium inoculant is used in the primary inoculant and the secondary inoculant, and the silicon strontium inoculant contains 1.5% strontium. The mass percentage content of the components in the silicon strontium inoculant is: 75% Si, 1.5% Sr, 2% Mn, 0.1% Ca, 0.3% Al, and the balance is iron. The particle size of the silicon strontium inoculant in the primary inoculant is 3~8mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2~0.8mm. Example 1

[0043] The gearbox housing is obtained by adopting the process steps of smelting molten iron, refining molten iron, ladle inoculation, inverted ladle inoculation and casting as recorded in this application, wherein a primary inoculant is added in the ladle inoculation step, and a secondary inoculant is used in the inverted ladle inoculation step, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron.

[0044] The primary inoculant is composed of 75 ferrosilicon inoculant, silicon strontium inoculant and accelerator in a mass ratio of 1:1:1, and the secondary inoculant is a silicon strontium inoculant. The same silicon strontium inoculant is used in the primary inoculant and the secondary inoculant, and the silicon strontium inoculant contains 1.5% strontium. The mass percentage content of the components in the silicon strontium inoculant is: 75% Si, 1.5% Sr, 2% Mn, 0.1% Ca, 0.3% Al, and the balance is iron. The particle size of the silicon strontium inoculant in the primary inoculant is 3~8mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2~0.8mm.

[0045] The accelerator includes 20% by mass of silicon-barium inoculant, 10% of silicon-zirconium inoculant, 10% of ferromanganese, and 1% of vanadium, with the balance being ferrosilicon. In this embodiment and all subsequent embodiments, the silicon-barium inoculant is BINAI 3-8, and the silicon-zirconium inoculant is Foseco INOCULIN 900.

[0046] The ferrosilicon can be selected from FeSi75-B or FeSi75-A or a combination of the two. FeSi75-A is used in this embodiment and subsequent embodiments, and the ferromanganese is FeMn68.

[0047] Examples 2 to 7 are obtained by adjusting the components based on Example 1, and the adjustment object is the mass ratio of the ferrosilicon inoculant, the strontium silicon inoculant and the accelerator in the primary inoculant, as follows:

[0048] In Example 2, the mass ratio of ferrosilicon inoculant, strontium silicon inoculant and accelerator is 1:1:1.5;

[0049] In Example 3, the mass ratio of ferrosilicon inoculant, strontium silicon inoculant and accelerator is 1:1:2;

[0050] In Example 4, the mass ratio of ferrosilicon inoculant, strontium silicon inoculant and accelerator is 1:1:2.5;

[0051] In Example 5, the mass ratio of ferrosilicon inoculant, strontium silicon inoculant and accelerator is 1:1:3;

[0052] In Example 6, the mass ratio of ferrosilicon inoculant, strontium silicon inoculant and accelerator is 1:1:3.5;

[0053] In Example 7, the mass ratio of ferrosilicon inoculant, strontium silicon inoculant and accelerator is 1:1:4.

[0054] The metallographic structure of the thin wall of the gearbox housing obtained in Examples 1 to 7 and Comparative Example 1 was inspected to obtain the performance parameters shown in Table 1.

[0055]

[0056] Table 1: Performance parameters of Examples 1 to 7 and Comparative Example 1

[0057] in addition, Figure 2 The pores on the casting surface produced in Example 1 are shown. Figure 3 What is shown is the metallographic structure diagram of the graphite morphology of the casting in Example 1, Figure 4 The metallographic structure diagram of the carburized layer of the casting in Example 1 is shown. It can be seen that the casting surface has relatively obvious pores in this state, the internal A-type graphite content is less than 70%, and the rest is mostly D-type graphite; the cementite content is 5%, and the pearlite content is 85%.

[0058] Figure 5 The pinholes in the casting produced in Example 2 are shown. Figure 6 The pinholes in the casting produced in Example 3 are shown. Figure 7 Shown is the metallographic structure diagram of the graphite morphology of the casting in Example 3, Figure 8 Shown is the metallographic structure diagram of the graphite morphology of the casting in Example 5, wherein Figure 2 , Figure 5 and Figure 6 The pores or pinholes in the casting are indicated by dotted circles. Figure 7 Compared to Figure 3 The internal A-type graphite content has been significantly improved. Figure 8 and Figure 7 The content of type A graphite is quite high.

[0059] In combination with Examples 1 to 7 and Comparative Example 1, it can be seen that, compared with the primary inoculant composed of ferrosilicon inoculant and silicon strontium inoculant, the primary inoculant composed of ferrosilicon inoculant, silicon strontium inoculant and accelerator combined with the secondary inoculant in the casting application process of the gearbox housing can significantly reduce the cementite content and increase the type A graphite content and pearlite content to a certain extent, and this improvement effect shows a trend of first increasing and then decreasing with the addition of accelerator in the primary inoculant, especially when the mass ratio of ferrosilicon inoculant, silicon strontium inoculant and accelerator is in the range of 1:1:(2.5~3), the purpose of solving the white cast and porosity problems of the casting can be basically achieved.

[0060] Comparative Example 2

[0061] The gearbox housing is obtained by adopting the process steps of smelting molten iron, refining molten iron, ladle inoculation, inverted ladle inoculation and casting as recorded in this application, wherein a primary inoculant is added in the ladle inoculation step, and a secondary inoculant is used in the inverted ladle inoculation step, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron.

[0062] The primary inoculant is composed of 75 ferrosilicon inoculant and silicon strontium inoculant in a mass ratio of 1:1, and the secondary inoculant is composed of silicon strontium inoculant and accelerator in a mass ratio of 1:1. The same silicon strontium inoculant is used in the primary inoculant and the secondary inoculant, and the silicon strontium inoculant contains 1.5% strontium. The mass percentage content of the components in the silicon strontium inoculant is: 75% Si, 1.5% Sr, 2% Mn, 0.1% Ca, 0.3% Al, and the balance is iron. The particle size of the silicon strontium inoculant in the primary inoculant is 3~8mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2~0.8mm.

[0063] The accelerator includes 20% by mass of silicon-barium inoculant, 10% by mass of silicon-zirconium inoculant, 10% by mass of ferromanganese, 1% by mass of vanadium, and the balance is ferrosilicon.

[0064] Comparative Examples 3 to 8 are obtained by adjusting the components based on Comparative Example 2, and the adjustment object is the mass ratio of the silicon strontium inoculant and the accelerator in the secondary inoculant, as follows:

[0065] In Comparative Example 3, the mass ratio of silicon strontium inoculant to accelerator is 1:1.5;

[0066] In Comparative Example 4, the mass ratio of silicon strontium inoculant to accelerator is 1:2;

[0067] In Comparative Example 5, the mass ratio of silicon strontium inoculant to accelerator is 1:2.5;

[0068] In Comparative Example 6, the mass ratio of silicon strontium inoculant to accelerator is 1:3;

[0069] In Comparative Example 7, the mass ratio of silicon strontium inoculant to accelerator is 1:3.5;

[0070] In Comparative Example 8, the mass ratio of silicon strontium inoculant to accelerator is 1:4.

[0071] The metallographic structure of the thin wall of the gearbox housing obtained in Comparative Examples 2 to 8 was inspected, and the performance parameters shown in Table 2 were obtained.

[0072]

[0073] Table 2: Performance parameters of comparative examples 2 to 8

[0074] Combined with comparative examples 2 to 8, it can be seen that compared with the single-component secondary inoculant using a silicon-strontium inoculant, the secondary inoculant composed of a silicon-strontium inoculant and a accelerator combined with a primary inoculant in the casting application process of the gearbox housing also has a certain improvement effect on the white cast and porosity problems of the casting.

[0075] Furthermore, by adjusting the use of the accelerator with the primary inoculant and the secondary inoculant respectively, it can be seen that the use of the accelerator in combination with the primary inoculant in the ladle inoculation process has a more significant improvement effect on the chill and porosity problems of the casting.

[0076] Specifically, as the content of the accelerator in the secondary inoculant increases, the cementite content can be significantly reduced, the pores can be eliminated, and the content of type A graphite and the content of pearlite can be increased to a certain extent, but the pearlite content cannot reach 95%. The inventors further increased the content of the accelerator in the secondary inoculant in other embodiments and found that there was no obvious trend of further increasing the pearlite content. Example 8

[0077] The gearbox housing is obtained by adopting the process steps of smelting molten iron, refining molten iron, ladle inoculation, inverted ladle inoculation and casting as recorded in this application, wherein a primary inoculant is added in the ladle inoculation step, and a secondary inoculant is used in the inverted ladle inoculation step, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron.

[0078] The primary inoculant is composed of 75 ferrosilicon inoculant, silicon strontium inoculant and accelerator in a mass ratio of 1:1:2.5, the secondary inoculant is silicon strontium inoculant, different silicon strontium inoculants are used in the primary inoculant and the secondary inoculant, the mass percentage content of the components of the silicon strontium inoculant in the primary inoculant is: 75%Si, 1.4%Sr, 2%Mn, 0.1%Ca, 0.3%Al, the balance is iron, the particle size of the silicon strontium inoculant in the primary inoculant is 3~8mm, the silicon strontium inoculant in the secondary inoculant contains 1.5% strontium, the mass percentage content of the components in the silicon strontium inoculant is: 75%Si, 1.5%Sr, 2%Mn, 0.1%Ca, 0.3%Al, the balance is iron, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2~0.8mm.

[0079] The accelerator includes 20% by mass of silicon-barium inoculant, 10% by mass of silicon-zirconium inoculant, 10% by mass of ferromanganese, 1% by mass of vanadium, and the balance is ferrosilicon.

[0080] Examples 9 to 13 are obtained by adjusting the components based on Example 8, and the adjustment object is the content of strontium in the silicon strontium inoculant in the primary inoculant, as follows:

[0081] The content of strontium in the silicon-strontium inoculant in Example 9 is 1.3%;

[0082] The content of strontium in the silicon-strontium inoculant in Example 10 is 1.2%;

[0083] The content of strontium in the silicon-strontium inoculant in Example 11 is 1.1%;

[0084] The content of strontium in the silicon-strontium inoculant in Example 12 is 1%;

[0085] The strontium content in the silicon-strontium inoculant in Example 13 is 0.9%.

[0086] The metallographic structure of the thin wall of the gearbox housing obtained in Examples 8 to 13 was inspected to obtain the performance parameters shown in Table 3.

[0087]

[0088] Table 3: Performance parameters of Examples 8 to 13

[0089] In combination with Examples 8 to 13, it can be seen that the addition of the promoter in the primary inoculant does not have a separate effect on the chilling and porosity problems of the castings, but also has a certain synergistic relationship with the silicon-strontium inoculant used, that is, under the premise that the promoter components are determined to be 20% silicon-barium inoculant, 10% silicon-zirconium inoculant, 10% ferromanganese, 1% vanadium, and the balance is ferrosilicon, compared with Example 4, as the strontium content of the silicon-strontium inoculant in the primary inoculant decreases, cementite and porosity phenomena do not occur, and at the same time, the A-type graphite content and pearlite content are increased to a corresponding extent, and the optimal strontium content of the silicon-strontium inoculant in the primary inoculant is 1.1%. When the strontium content is lower, the chilling and porosity problems of the castings will reappear.

[0090] Fig. 9 The graphite metallographic structure of the casting of Example 11 is shown, and the content of type A graphite is stably 95%. Fig.10 The metallographic structure analysis diagram of the carburized layer of the casting of Example 11 is shown, in which no cementite is found and the pearlite content reaches 98%.

[0091] Fig.11 The graphite metallographic structure of the casting of Example 8 is shown, and the content of type A graphite reaches 90%. Fig.12 The metallographic structure analysis diagram of the carburized layer of the casting of Example 8 is shown, in which no cementite is found and the pearlite content reaches 95%.

[0092] Comparative Example 9

[0093] The gearbox housing is obtained by adopting the process steps of smelting molten iron, refining molten iron, ladle inoculation, inverted ladle inoculation and casting as recorded in this application, wherein a primary inoculant is added in the ladle inoculation step, and a secondary inoculant is used in the inverted ladle inoculation step, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron.

[0094] The primary inoculant is composed of 75 ferrosilicon inoculant, silicon strontium inoculant and accelerator in a mass ratio of 1:1:2.5, the secondary inoculant is silicon strontium inoculant, different silicon strontium inoculants are used in the primary inoculant and the secondary inoculant, the mass percentage content of the components of the silicon strontium inoculant in the secondary inoculant is: 75%Si, 1.4%Sr, 2%Mn, 0.1%Ca, 0.3%Al, the balance is iron, the particle size of the silicon strontium inoculant in the secondary inoculant is 3~8mm, the silicon strontium inoculant in the primary inoculant contains 1.5% strontium, the mass percentage content of the components in the silicon strontium inoculant is: 75%Si, 1.5%Sr, 2%Mn, 0.1%Ca, 0.3%Al, the balance is iron, and the particle size of the silicon strontium inoculant in the primary inoculant is 0.2~0.8mm.

[0095] The accelerator includes 20% by mass of silicon-barium inoculant, 10% by mass of silicon-zirconium inoculant, 10% by mass of ferromanganese, 1% by mass of vanadium, and the balance is ferrosilicon.

[0096] Comparative Examples 10 to 14 are obtained by adjusting the components based on Comparative Example 9, and the adjustment object is the content of strontium in the silicon strontium inoculant in the secondary inoculant, as follows:

[0097] The content of strontium in the silicon-strontium inoculant in Comparative Example 10 is 1.3%;

[0098] The content of strontium in the silicon-strontium inoculant in Comparative Example 11 is 1.2%;

[0099] The content of strontium in the silicon-strontium inoculant in Comparative Example 12 is 1.1%;

[0100] The content of strontium in the silicon-strontium inoculant in Comparative Example 13 is 1%;

[0101] The strontium content in the silicon-strontium inoculant in Comparative Example 14 is 0.9%.

[0102] The metallographic structure of the thin wall of the gearbox housing obtained in Comparative Examples 9 to 14 was inspected, and the performance parameters shown in Table 4 were obtained.

[0103]

[0104] Table 4: Performance parameters of comparative examples 9 to 14

[0105] Combined with comparative examples 9 to 14, it can be seen that the change in the strontium content in the secondary inoculant does not play the same role as the change in the strontium content in the primary inoculant. On the contrary, as the strontium content in the secondary inoculant decreases, it not only fails to effectively solve the chill and porosity problems, but also affects the A-type graphite content and pearlite content in the casting.

[0106] Comparative Example 15

[0107] The gearbox housing is obtained by adopting the process steps of smelting molten iron, refining molten iron, ladle inoculation, inverted ladle inoculation and casting as recorded in this application, wherein a primary inoculant is added in the ladle inoculation step, and a secondary inoculant is used in the inverted ladle inoculation step, the amount of the primary inoculant added is 0.4% of the weight of the molten iron, and the amount of the secondary inoculant added is 0.1% of the weight of the molten iron.

[0108] The primary inoculant is composed of 75 ferrosilicon inoculant, silicon strontium inoculant and accelerator in a mass ratio of 1:1:2.5, and the secondary inoculant is a silicon strontium inoculant. The same silicon strontium inoculant is used in the primary inoculant and the secondary inoculant, and the silicon strontium inoculant contains 1.4% strontium. The mass percentage content of the components in the silicon strontium inoculant is: 75% Si, 1.4% Sr, 2% Mn, 0.1% Ca, 0.3% Al, and the balance is iron. The particle size of the silicon strontium inoculant in the primary inoculant is 3~8mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2~0.8mm.

[0109] The accelerator includes 20% by mass of silicon-barium inoculant, 10% by mass of silicon-zirconium inoculant, 10% by mass of ferromanganese, 1% by mass of vanadium, and the balance is ferrosilicon.

[0110] Comparative Examples 16 to 20 are obtained by adjusting the components based on Comparative Example 15, and the adjustment object is the content of strontium in the silicon-strontium inoculant, as follows:

[0111] The content of strontium in the silicon-strontium inoculant in Comparative Example 16 is 1.3%;

[0112] The content of strontium in the silicon-strontium inoculant in Comparative Example 17 is 1.2%;

[0113] The content of strontium in the silicon-strontium inoculant in Comparative Example 18 is 1.1%;

[0114] The content of strontium in the silicon-strontium inoculant in Comparative Example 19 is 1%;

[0115] The strontium content in the silicon-strontium inoculant in Comparative Example 20 is 0.9%.

[0116] The metallographic structure of the thin wall of the gearbox housing obtained in Comparative Examples 15 to 20 was inspected, and the performance parameters shown in Table 5 were obtained.

[0117]

[0118] Table 5: Performance parameters of comparative examples 15 to 20

[0119] Combined with comparative examples 15 to 20, it can be seen that when the secondary inoculant and the primary inoculant use the same silicon strontium inoculant and as the strontium content decreases, the chilling and pore problems still exist, and the chilling and pore problems become more significant as the strontium content decreases.

[0120] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them.

Claims

1. The casting process of thin-walled gray iron castings is characterized by: Thin-walled grey iron castings are obtained by smelting molten iron, refining molten iron, ladle inoculation, ladle flow inoculation and casting. A primary inoculant is added in the ladle inoculation step, wherein the primary inoculant includes a ferrosilicon inoculant, a silicon strontium inoculant and an accelerator, wherein the accelerator includes a silicon-barium inoculant of 20% by mass, a silicon-zirconium inoculant of 10% by mass, a ferromanganese inoculant of 10% by mass, and a vanadium inoculant of 1% by mass, with the remainder being ferrosilicon; the mass ratio of the ferrosilicon inoculant, the silicon strontium inoculant and the accelerator in the primary inoculant is 1:1:(2-3.5); A secondary inoculant is added in the inverted package flow inoculation step, and the secondary inoculant is a silicon strontium inoculant.

2. The casting process of thin-walled grey iron casting according to claim 1, characterized in that: The added amount of the primary inoculant is 0.4% of the weight of the molten iron, and the added amount of the secondary inoculant is 0.1% of the weight of the molten iron.

3. The casting process of thin-walled grey iron casting according to claim 2, characterized in that: The mass ratio of the ferrosilicon inoculant, the strontium silicon inoculant and the accelerator in the primary inoculant is 1:1:(2.5-3).

4. The casting process of thin-walled grey iron casting according to claim 1, characterized in that: The strontium content of the silicon-strontium inoculant in the primary inoculant is greater than 1%, and the strontium content of the silicon-strontium inoculant in the secondary inoculant is greater than 1.3%.

5. The casting process of thin-walled grey iron casting according to claim 4, characterized in that: The strontium content of the silicon-strontium inoculant in the primary inoculant is 1.1%, and the strontium content of the silicon-strontium inoculant in the secondary inoculant is 1.5%.

6. The casting process of thin-walled grey iron casting according to claim 1, characterized in that: The particle size of the silicon strontium inoculant in the primary inoculant is 3-8 mm, and the particle size of the silicon strontium inoculant in the secondary inoculant is 0.2-0.8 mm.

7. The casting process of thin-walled grey iron casting according to claim 1, characterized in that: The ferrosilicon is selected from FeSi75-B or FeSi75-A or a combination of the two, and the ferromanganese is selected from FeMn68.

8. Thin-walled grey iron castings, characterized in that: The thin-walled grey iron casting is cast by the casting process described in any one of claims 1 to 7.