Gradient diamond compact and preparation method thereof

By distributing cobalt elements along the axial gradient in the diamond composite sheet and filling SiC using cobalt wire decobalt channels and atomic layer deposition, the problem of excessive residual stress in the diamond composite sheet is solved and its mechanical and impact resistance properties are improved. Extended service life.

CN118808656APending Publication Date: 2024-10-22河南亚龙金刚石制品股份有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411041276.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

During the high-temperature and high-pressure synthesis process of diamond composite sheets, the residual stress caused by the difference in thermal expansion coefficient of the materials is excessive, affecting its mechanical properties and heat resistance, and it is difficult to effectively reduce it with existing technology.

Method used

By distributing cobalt elements along the axial gradient in the polycrystalline diamond composite layer, using cobalt wires to form cobalt removal channels, and filling SiC with atomic layer deposition, the true gradient distribution and hole filling of metallic cobalt in the diamond layer can be achieved, reducing residual stress. .

Benefits of technology

It effectively reduces the residual stress caused by the different thermal expansion coefficients of the materials, improves the mechanical properties and impact resistance of the diamond composite sheets, prolongs the service life and avoids the performance damage caused by the traditional cobalt removal process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808656A_ABST
    Figure CN118808656A_ABST
Patent Text Reader

Abstract

According to the gradient diamond compact and the preparation method thereof, the gradient diamond compact comprises a hard alloy layer at the bottom and a polycrystalline diamond composite layer on the upper portion in the axial direction of a cylinder, and cobalt elements in the polycrystalline diamond composite layer are distributed in a gradient mode in the axial direction. The preparation method comprises the following steps: 1) obtaining premixed powder; (2) the premixed powder is put into a metal mold layer by layer; (3) the hard alloy layer is put into a metal mold and pressed tightly, and then a combination composed of the metal mold, the hard alloy layer, the premixed powder and the Co powder is put into a synthesis cavity to be subjected to high-temperature and high-pressure synthesis; 4) machining the synthesized blank product; 5) putting the semi-finished product into deposition equipment, and performing deposition repair on holes formed by cobalt removal in the polycrystalline diamond composite layer; 6, the deposited product is subjected to secondary aftertreatment and heat treatment, and the finished diamond compact is obtained.According to the method, real gradient distribution of metal cobalt in a diamond layer is achieved, and the situation that performance is affected by holes formed by traditional cobalt removal is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a diamond composite sheet, in particular a diamond composite sheet with element gradient distribution. Background Art

[0002] Diamond composite (PDC) is composed of polycrystalline diamond and cemented carbide. It has extremely high performance indicators in terms of hardness, wear resistance, impact resistance, strength, thermal stability, etc. It is widely used in various exploration and drilling fields. Compared with traditional products such as cemented carbide drill bits and diamond-impregnated drill bits, it can show obvious advantages and performance characteristics. The service life can reach 3 to 10 times that of traditional products. The overall application ratio has reached more than 90%.

[0003] PDC products are made by synthesizing two materials under high temperature and high pressure. During the cooling process, there is a huge difference in thermal expansion coefficient between diamond and cemented carbide, especially between diamond and metal cobalt in the alloy, which leads to large residual stress inside the product after it is made. In actual use, the residual stress will affect the mechanical properties of the product on the one hand, greatly reducing the service life of the product; on the other hand, it will reduce the heat resistance of the product, causing the product to fail quickly after being heated during the drilling process, affecting normal use.

[0004] Domestic and foreign industries generally use two methods to solve the above-mentioned residual stress problem. One method is to reduce the residual stress through heat treatment, vibration and other methods after synthesis, but the execution conditions of this method are relatively harsh and the effect is often poor; the other method is to reduce the stress by gradient distribution of metal cobalt in the diamond layer before synthesis. However, under high temperature and high pressure, due to the wetting of metal cobalt and diamond, the designed gradient distribution cobalt element will automatically achieve uniform sweep in the diamond layer. The actual synthesized metal cobalt element cannot achieve the designed target distribution and cannot achieve the effect of reducing stress. Summary of the invention

[0005] The technical problem to be solved by the present invention is: in view of the fact that the residual stress of the current composite sheet is too large and cannot be effectively eliminated, the present invention provides a gradient diamond composite sheet and also provides a method for preparing the above diamond composite sheet.

[0006] To achieve the above object, the present invention is achieved through the following technical solutions: A gradient diamond composite sheet comprises a cemented carbide layer at the bottom and a polycrystalline diamond composite layer at the top along the cylindrical axial direction, wherein the cobalt element in the polycrystalline diamond composite layer is distributed in a gradient manner along the axial direction.

[0007] The components of the polycrystalline diamond composite layer are 75-90wt.% of 15-40μm diamond powder, 8-20wt.% of 3-10μm diamond powder, and 2-5wt.% of 1-3μm Co powder.

[0008] The thickness of the polycrystalline diamond composite layer along the axial direction is 1.2~3.5mm.

[0009] The bonding surface between the cemented carbide layer and the polycrystalline diamond composite layer includes but is not limited to a flat surface, a curved surface or a step surface.

[0010] A method for preparing the diamond composite sheet comprises the following steps: 1) Mix 15-40 μm diamond powder, 3-10 μm diamond powder and 1-3 μm Co powder evenly to obtain a premixed powder; 2) The premixed powder is divided into 3 to 6 layers and placed into the metal mold layer by layer. After each layer is added, the powder is first flattened, and then the cobalt wire is placed in the radial direction, and then the next layer of powder is added. This cycle is repeated until the powder is added. The amount of cobalt wire added decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire is added; 3) Place the cemented carbide layer into a metal mold and press it, then place the metal mold, cemented carbide layer, premixed powder and Co powder into a synthesis cavity for high temperature and high pressure synthesis to form a blank product; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond composite layer is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device to deposit and repair the holes formed by decobaltization in the polycrystalline diamond composite layer; 6) The deposited product undergoes secondary post-processing and heat treatment to obtain a finished diamond composite sheet.

[0011] The number of premixed powder layers is 3 to 6, and the thickness of each layer is 1 / 6 to 1 / 3 of the total thickness of the powder layer.

[0012] The diameter of the cobalt wire is ≤0.2mm. The number of cobalt wires placed in each layer is 3 to 12. The length of each wire is 1 / 6 to 1 times the radius of the metal mold. All cobalt wires are evenly distributed in the same layer, and one end of the cobalt wire is in contact with the inner wall of the metal mold.

[0013] The number and total length of cobalt wires in each layer decreases layer by layer from the diamond layer to the cemented carbide layer, with a decreasing range of 10~75%.

[0014] During the synthesis process, the pressure inside the cavity is 5~7GPa; the heat treatment atmosphere is a vacuum environment and the temperature is 500~750℃.

[0015] The deposition method is atomic layer deposition or vapor phase deposition, and the deposit is SiC.

[0016] Compared with the prior art, the present invention has the following beneficial effects: after synthesis, the cobalt element in the diamond layer is non-uniformly removed, and then the decobalted pores are filled by atomic vapor deposition, thereby achieving a true gradient distribution of metallic cobalt in the diamond layer and avoiding the influence of the pores formed by traditional decobalting on the performance.

[0017] 1. The present invention utilizes cobalt wire to form a cobalt removal channel, and realizes a gradient distribution of metallic cobalt elements in the diamond layer based on the cobalt removal process, thereby reducing the internal residual stress caused by the different thermal expansion coefficients of the two materials, and significantly improving the mechanical properties of the product.

[0018] 2. The present invention reduces the metal content in the diamond layer by removing cobalt, thereby avoiding internal defects caused by uneven expansion of the product after being heated during use.

[0019] 3. The present invention uses atomic layer deposition technology to fill the cobalt removal holes, reducing the damage to the mechanical properties of the diamond layer caused by the formation of cobalt removal holes in the traditional cobalt removal process.

[0020] 4. The present invention uses SiC as the filling material, which, on the one hand, facilitates the filling density of the holes. On the other hand, since the thermal expansion coefficient of SiC is between cobalt and diamond, it can effectively balance the internal stress of the diamond layer when heated, further improving the impact resistance of the product.

[0021] 5. The present invention performs heat treatment after filling SiC, which can better balance the stress between the components in the diamond layer, thereby effectively reducing the internal stress of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a top view of the distribution of the cobalt wires in each layer of the present invention; Figure 2 This is another top view of the cobalt filament distribution; Figure 3 yes Figure 1 Schematic diagram of the spatial distribution of cobalt filaments after assembly; Figure 4 yes Figure 3 Schematic diagram of the product after synthesis and decobalting; Figure 5 yes Figure 4 Schematic diagram of the product after the meteorological filling hole; Figure 6 It is another product diagram after the weather fills the hole. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0025] like Figure 1 As shown, a gradient diamond composite sheet includes a cemented carbide layer 2 at the bottom and a polycrystalline diamond composite layer 1 at the top along the cylindrical axial direction, wherein the cobalt element in the polycrystalline diamond composite layer 1 is distributed in a gradient manner along the axial direction.

[0026] Furthermore, the components of the polycrystalline diamond composite layer 1 are 75-90 wt.% of 15-40 μm diamond powder, 8-20 wt.% of 3-10 μm diamond powder, and 2-5 wt.% of 1-3 μm Co powder.

[0027] Furthermore, the thickness of the polycrystalline diamond composite layer 1 along the axial direction is 1.2-3.5 mm.

[0028] Furthermore, the bonding surface between the cemented carbide layer 2 and the polycrystalline diamond composite layer 1 includes but is not limited to a flat surface, a curved surface, and a stepped surface.

[0029] The present invention also provides a method for preparing a diamond composite sheet, comprising the following steps: 1) Mix 15~40μm diamond powder, 3~10μm diamond powder and 1~3μm Co powder evenly to obtain a premixed powder; 2) The premixed powder is divided into 3 to 6 layers and placed into the metal mold layer by layer. After each layer is added, the powder is first flattened, and then the cobalt wire 3 is placed in the radial direction, and then the next layer of powder is added. This cycle is repeated until the powder is added. The amount of cobalt wire 3 added decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire 3 is added; 3) placing the cemented carbide layer 2 into a metal mold and pressing it, and then placing the metal mold, the cemented carbide layer 2, the premixed powder and the Co powder into a synthesis cavity for high temperature and high pressure synthesis to form a blank product; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond composite layer 1 is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device to deposit and repair the holes 101 formed by decobalting in the polycrystalline diamond composite layer 1; 6) The deposited product undergoes secondary post-processing and heat treatment to obtain a finished diamond composite sheet.

[0030] Furthermore, the number of premixed powder layers is 3 to 6, and the thickness of each layer is 1 / 6 to 1 / 3 of the total thickness of the powder layers.

[0031] Furthermore, the wire diameter of the cobalt wire 3 is ≤0.2 mm, the number of cobalt wires 3 placed in each layer is 3 to 12, the length of each wire is 1 / 6 to 1 times the radius of the metal mold, all cobalt wires are evenly distributed in the same layer, and one end of the cobalt wire is in contact with the inner wall of the metal mold.

[0032] Furthermore, the number and total length of the cobalt wires 3 in each layer decreases layer by layer from the diamond layer to the cemented carbide layer, and the decreasing range is 10-75%.

[0033] Furthermore, the pressure inside the cavity during the synthesis process is 5~7GPa.

[0034] Furthermore, the deposition method is atomic layer deposition or vapor phase deposition, and the deposit is SiC.

[0035] Furthermore, the heat treatment atmosphere condition is a vacuum environment, and the temperature is 500~750℃.

[0036] Embodiment 1: The diamond composite sheet of this embodiment is prepared by the following steps: 1) Mix 15-40 μm diamond powder, 3-10 μm diamond powder and 1-3 μm Co powder in a ratio of 75 wt.%, 20 wt.%, and 5 wt.% to obtain a premixed powder; 2) The premixed powder is divided into 4 layers and placed into a metal mold layer by layer, with the thickness of each layer being 1 / 4 of the total layer thickness. After the powder is placed, the powder is first flattened, and then the cobalt wire 3 is placed in the radial direction, and then the next layer of powder is placed. This cycle is repeated until the powder is placed. The amount of cobalt wire 3 placed decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire 3 is placed. The thickness of the final product diamond layer is 2.8 mm; the diameter of the cobalt wire 3 is 0.1 mm, and the number and length of the three layers of cobalt wire 3 from the diamond layer to the alloy direction are 8×r+4×1 / 4r, 4×r, and 3×2 / 3r, respectively, where r is the radius of the metal mold; 3) Place the flat cemented carbide layer 2 into a metal mold and press it, then place the metal mold, cemented carbide layer 2, premixed powder and Co powder into a synthesis cavity for high temperature and high pressure synthesis, with the synthesis cavity pressure being 6.5 GPa; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond layer is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device, and the holes 101 formed by decobalting in the diamond layer are repaired by SiC deposition using an atomic layer deposition method to form a silicon carbide filling phase 4; 6) The deposited product is subjected to secondary post-processing and heat treatment to obtain a finished diamond composite sheet. The heat treatment environment is a vacuum environment and the temperature is 650°C.

[0037] A batch of diamond composite sheets were made by this method, and 5 were randomly selected for performance testing. The impact toughness of the diamond composite sheets was tested by an impact tester. The diamond composite sheets were compared with the diamond composite sheets made by the current traditional assembly process under the same conditions. The comparison results are as follows: Embodiment 2: The diamond composite sheet of this embodiment is prepared by the following steps: 1) Mix 15-40 μm diamond powder, 3-10 μm diamond powder and 1-3 μm Co powder in a ratio of 80 wt.%, 15 wt.%, and 5 wt.% to obtain a premixed powder; 2) The premixed powder is divided into 3 layers and placed into the metal mold layer by layer, with each layer thickness being 1 / 3 of the total layer thickness. After the powder is placed, the powder is first flattened, and then the cobalt wire 3 is placed in the radial direction, and then the next layer of powder is placed. This cycle is repeated until the powder is placed. The amount of cobalt wire 3 placed decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire 3 is placed. The thickness of the final product diamond layer is 1.5 mm; the diameter of the cobalt wire 3 is 0.1 mm, and the number and length of the two layers of cobalt wire 3 from the diamond layer to the alloy direction are 4×r and 3×r respectively, where r is the radius of the metal mold; 3) Place the flat cemented carbide into a metal mold and press it, then place the metal mold, alloy, premixed powder and Co powder into a synthesis cavity for high temperature and high pressure synthesis, with the synthesis cavity pressure being 7.0 GPa; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond layer is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device, and SiC deposition is performed to repair the holes 101 formed by decobalting in the diamond layer by a vapor deposition method to form a silicon carbide filling phase 4; 6) The deposited product is subjected to secondary post-processing and heat treatment to obtain a finished diamond composite sheet. The heat treatment environment is a vacuum environment and the temperature is 550°C.

[0038] A batch of diamond composite sheets were made by this method, and 5 were randomly selected for performance testing. The impact toughness of the diamond composite sheets was tested by an impact tester. The diamond composite sheets were compared with the diamond composite sheets made by the current traditional assembly process under the same conditions. The comparison results are as follows: Embodiment 3: The diamond composite sheet of this embodiment is prepared by the following steps: 1) 15~40μm diamond powder, 3~10μm diamond powder and 1~3μm Co powder are uniformly mixed in a ratio of 85wt..%, 12wt.%, and 3wt.% to obtain a premixed powder; 2) The premixed powder is divided into 4 layers and placed into a metal mold layer by layer, with each layer thickness being 1 / 4 of the total layer thickness. After the powder is placed, the powder is first flattened, and then the cobalt wire 3 is placed in the radial direction, and then the next layer of powder is placed. This cycle is repeated until the powder is placed. The amount of cobalt wire 3 placed decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire is placed. The thickness of the final product diamond layer is 2.0 mm; the diameter of the cobalt wire 3 is 0.2 mm, and the number and length of the three layers of cobalt wire 3 from the diamond layer to the alloy direction are 6×r, 4×r, and 3×r, respectively, where r is the radius of the metal mold; 3) Place the curved cemented carbide into a metal mold and press it, then place the metal mold, alloy, premixed powder and Co powder into a synthesis cavity for high temperature and high pressure synthesis, with the synthesis cavity pressure being 5.5 GPa; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond layer is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device, and SiC deposition is performed to repair the holes 101 formed by decobalting in the diamond layer by a vapor deposition method to form a silicon carbide filling phase 4; 6) The deposited product is subjected to secondary post-processing and heat treatment to obtain a finished diamond composite sheet. The heat treatment environment is a vacuum environment and the temperature is 600°C.

[0039] A batch of diamond composite sheets were made by this method, and 5 were randomly selected for performance testing. The impact toughness of the diamond composite sheets was tested by an impact tester. The diamond composite sheets were compared with the diamond composite sheets made by the current traditional assembly process under the same conditions. The comparison results are as follows: Embodiment 4: The diamond composite sheet of this embodiment is prepared by the following steps: 1) 15~40μm diamond powder, 3~10μm diamond powder and 1~3μm Co powder are uniformly mixed in a ratio of 88wt..%, 10wt.%, and 2wt.% to obtain a premixed powder; 2) The premixed powder is divided into 6 layers and placed into a metal mold layer by layer, with the thickness of each layer being 1 / 6 of the total layer thickness. After the powder is placed, the powder is first flattened, and then the cobalt wire 3 is placed in the radial direction, and then the next layer of powder is placed. This cycle is repeated until the powder is placed. The amount of cobalt wire 3 placed decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire 3 is placed. The thickness of the final product diamond layer is 2.4 mm; the diameter of the cobalt wire 3 is 0.15 mm, and the number and length of the five layers of cobalt wire 3 from the diamond layer to the alloy direction are 6×r, 4×r, 3×r, 4×1 / 2r, and 3×1 / 3r, respectively, where r is the radius of the metal mold; 3) Place the step carbide into a metal mold and press it, then place the metal mold, alloy, premixed powder and Co powder into a synthesis cavity for high temperature and high pressure synthesis, with the synthesis cavity pressure being 6.5 GPa; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond layer is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device, and the holes 101 formed by decobalting in the diamond layer are repaired by SiC deposition using an atomic layer deposition method to form a silicon carbide filling phase 4; 6) The deposited product is subjected to secondary post-processing and heat treatment to obtain a finished diamond composite sheet. The heat treatment environment is a vacuum environment and the temperature is 750°C.

[0040] A batch of diamond composite sheets were made by this method, and 5 were randomly selected for performance testing. The impact toughness of the diamond composite sheets was tested by an impact tester. The diamond composite sheets were compared with the diamond composite sheets made by the current traditional assembly process under the same conditions. The comparison results are as follows: Embodiment 5: The diamond composite sheet of this embodiment is prepared by the following steps: 1) 15~40μm diamond powder, 3~10μm diamond powder and 1~3μm Co powder are uniformly mixed in a ratio of 85wt..%, 10wt.%, and 5wt.% to obtain a premixed powder; 2) The premixed powder is divided into 3 layers and placed into a metal mold layer by layer, with the thickness of each layer being 1 / 3 of the total layer thickness. After the powder is placed, the powder is first flattened, and then the cobalt wire 3 is placed in the radial direction, and then the next layer of powder is placed. This cycle is repeated until the powder is placed. The amount of cobalt wire placed decreases layer by layer. After the last layer of powder is placed and flattened, no cobalt wire 3 is placed. The thickness of the final product diamond layer is 2.1 mm; the diameter of the cobalt wire 3 is 0.2 mm, and the number and length of the two layers of cobalt wire 3 from the diamond layer to the alloy direction are 6×2 / 3r and 3×r respectively, where r is the radius of the metal mold; 3) Place the flat cemented carbide into a metal mold and press it, then place the metal mold, alloy, premixed powder and Co powder into a synthesis cavity for high temperature and high pressure synthesis, with the synthesis cavity pressure being 5.0 GPa; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond layer is decobalted to obtain a semi-finished product; 5) The semi-finished product is placed in a deposition device, and SiC deposition is performed to repair the holes 101 formed by decobalting in the diamond layer by a vapor deposition method to form a silicon carbide filling phase 4; 6) The deposited product is subjected to secondary post-processing and heat treatment to obtain a finished diamond composite sheet. The heat treatment environment is a vacuum environment and the temperature is 500°C.

[0041] A batch of diamond composite sheets were made by this method, and 5 were randomly selected for performance testing. The impact toughness of the diamond composite sheets was tested by an impact tester. The diamond composite sheets were compared with the diamond composite sheets made by the current traditional assembly process under the same conditions. The comparison results are as follows: The above is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, several changes and improvements can be made without departing from the overall concept of the present invention, which should also be regarded as the scope of protection of the present invention.

Claims

1. A gradient diamond composite sheet, characterized in that: Along the axial direction of the cylinder, it comprises a hard alloy layer (2) at the bottom and a polycrystalline diamond composite layer (1) at the top, wherein the cobalt element in the polycrystalline diamond composite layer (1) is distributed in a gradient manner along the axial direction.

2. A gradient diamond composite sheet according to claim 1, characterized in that: The components of the polycrystalline diamond composite layer (1) are 75-90 wt.% of 15-40 μm diamond powder, 8-20 wt.% of 3-10 μm diamond powder, and 2-5 wt.% of 1-3 μm Co powder.

3. The gradient diamond composite sheet according to claim 1, characterized in that: The thickness of the polycrystalline diamond composite layer (1) along the axial direction is 1.2-3.5 mm.

4. The gradient diamond composite sheet according to claim 1, characterized in that: The bonding surface between the cemented carbide layer (2) and the polycrystalline diamond composite layer (1) includes but is not limited to a flat surface, a curved surface or a stepped surface.

5. A method for preparing a diamond composite sheet according to any one of claims 1 to 4, characterized in that: The steps include: 1) Mix 15-40 μm diamond powder, 3-10 μm diamond powder and 1-3 μm Co powder evenly to obtain a premixed powder; 2) The premixed powder is divided into 3 to 6 layers and placed into a metal mold layer by layer. After each layer is added, the powder is first flattened, and then the cobalt wire (3) is placed in a radial direction, and then the next layer of powder is added. This cycle is repeated until the powder is added. The amount of cobalt wire added decreases layer by layer. After the last layer of powder is added and flattened, no cobalt wire (3) is added; 3) placing the cemented carbide layer (2) into a metal mold and pressing it, and then placing the metal mold, the cemented carbide layer (2), the premixed powder and the Co powder into a synthesis cavity, and performing high temperature and high pressure synthesis to form a blank product; 4) The synthesized rough product is machined, and then the synthesized polycrystalline diamond composite layer (1) is decobalted to obtain a semi-finished product; 5) placing the semi-finished product into a deposition device to deposit and repair the holes (101) formed by decobalting in the polycrystalline diamond composite layer (1); 6) The deposited product undergoes secondary post-processing and heat treatment to obtain a finished diamond composite sheet.

6. The method for preparing the diamond composite sheet according to claim 5, characterized in that: The number of premixed powder layers is 3 to 6, and the thickness of each layer is 1 / 6 to 1 / 3 of the total thickness of the powder layer.

7. The method for preparing a diamond composite sheet according to claim 5, characterized in that: The wire diameter of the cobalt wire (3) is ≤0.2 mm. The number of cobalt wires (3) placed in each layer is 3 to 12, and the length of each wire is 1 / 6 to 1 times the radius of the metal mold. All cobalt wires (3) are evenly distributed in the same layer, and one end of the cobalt wire (3) is in contact with the inner wall of the metal mold.

8. The method for preparing a diamond composite sheet according to claim 5, characterized in that: The number and total length of cobalt wires in each layer decreases layer by layer from the diamond layer to the cemented carbide layer, with a decreasing range of 10~75%.

9. The method for preparing a diamond composite sheet according to claim 5, characterized in that: During the synthesis process, the pressure inside the cavity is 5~7GPa; the heat treatment atmosphere is a vacuum environment and the temperature is 500~750℃.

10. The method for preparing a diamond composite sheet according to claim 5, characterized in that: The deposition method is atomic layer deposition or vapor phase deposition, and the deposit is SiC.

Citation Information

Cited By

  • Gradient-structure polycrystalline diamond compact and preparation method thereof

    CN121017552A