Hot isostatic pressure additive manufacturing composite preparation method of titanium alloy component

Through the additive manufacturing and hot isostatic pressing composite preparation method of titanium alloy homogeneous cladding, the problems of high cladding processing costs and environmental pollution during the molding process of titanium alloy components are solved, and an efficient and low-cost preparation process is achieved. Improved mechanical properties of titanium alloy components.

CN118808670APending Publication Date: 2024-10-22TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411114109.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing hot isostatic pressing method of titanium alloy components has problems such as high packaging processing costs, inability to reuse, complicated processes, and environmental pollution. In addition, additive manufacturing has low printing efficiency, long preparation cycle, and expensive costs.

Method used

The titanium alloy homogeneous cladding is prepared through additive manufacturing, and the excess structure is removed after hot isostatic pressing, which significantly shortens the preparation cycle, improves the mechanical properties, and enables the recycling of the homogeneous cladding.

Benefits of technology

It significantly shortens the preparation cycle of titanium alloy components, improves mechanical properties, reduces production costs, is environmentally friendly, and achieves the closure of additive manufacturing pore defects and improvement of mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808670A_ABST
    Figure CN118808670A_ABST
Patent Text Reader

Abstract

The invention discloses a hot isostatic pressure additive manufacturing composite preparation method of a titanium alloy component, and belongs to the technical field of titanium alloy manufacturing, the titanium alloy component is prepared by adopting a method of firstly carrying out additive manufacturing and then carrying out hot isostatic pressure, the preparation period of additive manufacturing is remarkably shortened, and the smaller the volume percent of a homogeneous sheath in a solid part is, the smaller the volume percent of the homogeneous sheath in the solid part is. Meanwhile, compared with a homogeneous sheath prepared by purely adopting additive manufacturing, the mechanical property of the homogeneous sheath can be remarkably improved by adopting the method disclosed by the invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy manufacturing, and in particular relates to a hot isostatic pressing additive manufacturing composite preparation method for a titanium alloy component. Background Art

[0002] The manufacture of large key load-bearing components is the basis for the manufacture of major equipment such as large aircraft, launch vehicles and nuclear power plants. With the rapid development of the aerospace and defense industries, metal components have been developing towards high complexity, high precision and integrated forming. The "China Materials Science Development Strategy 2035" clearly points out that powder hot isostatic pressing and additive manufacturing technology are typical metal near-net forming technologies.

[0003] Powder hot isostatic pressing technology is to fill powder into a metal sleeve (usually a steel sleeve), sinter and form under high temperature and high pressure, which can achieve near-net shape, the density of the alloy is close to 100%, the mechanical properties are close to forgings, the dimensional accuracy is equivalent to that of precision castings, and it can be produced in batches. Similar to the reaction between the alloy melt and the ceramic mold shell in precision casting, the heterogeneous sleeve and the powder body will undergo obvious interfacial diffusion under high temperature and high pressure, which may affect the mechanical properties of powder metallurgy components. On the other hand, the complex sleeve required for hot isostatic pressing has high processing costs and cannot be reused; at the same time, after hot isostatic pressing, the complex sleeve still needs to be removed through mechanical processing and chemical milling, which is complicated and pollutes the environment. These factors limit the large-scale application of this forming method. Metal additive manufacturing is a forming process that uses laser beams, electron beams, and arcs to melt and stack powder layer by layer to form a three-dimensional entity and quickly solidify it. Additive manufacturing is recognized as an effective technical means to solve the problem of overall forming of personalized and complex metal components. However, in order to ensure the density and dimensional accuracy of printed components, the printing efficiency of additive manufacturing is still low, the preparation cycle of large-sized complex components is long, and the cost is expensive. For example, patent application CN110539000 A discloses a titanium alloy component and its preparation method. Although the patent adopts additive manufacturing to prepare the sheath, followed by hot isostatic pressing, the sheath preparation method in the patent adopts a heterogeneous sheath (low carbon steel). After forming, the sheath needs to be removed by machining and chemical milling, which is costly and chemical milling pollutes the environment; patent application CN 108971495 A discloses a hot isostatic pressing method for a titanium alloy gas cylinder hemisphere. The patent still uses a conventional steel sheath, which has the problems of high processing cost and cannot be reused. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a hot isostatic pressing additive manufacturing composite preparation method for titanium alloy components.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A hot isostatic pressing additive manufacturing composite preparation method for a titanium alloy component comprises the following steps:

[0007] (1) According to the shape and size of the target part, the wall thickness of the additively manufactured titanium alloy homogeneous sheath is fixed, and finite element simulation is performed. Through inverse compensation and iterative calculation, a three-dimensional model of the titanium alloy homogeneous sheath is determined, and the titanium alloy homogeneous sheath is reserved with a powder injection port;

[0008] (2) Slicing the three-dimensional model of the titanium alloy homogeneous sheath using 3D printing slicing software and outputting an STL file to determine a printing path for additive manufacturing;

[0009] (3) importing the STL file into a 3D printer, fixing the printing layer thickness and scanning spacing, regulating the printing power and scanning rate of additive manufacturing, and preparing the titanium alloy homogeneous sheath;

[0010] (4) filling the titanium alloy powder into the titanium alloy homogeneous sheath through a reserved powder injection port, and performing degassing and sealing welding to obtain a titanium alloy homogeneous sheath powder body;

[0011] (5) hot isostatic pressing the titanium alloy homogeneous sheathed powder body, and then cooling and releasing the pressure after the pressing to obtain a titanium alloy homogeneous sheathed powder body;

[0012] (6) removing redundant structures of the titanium alloy homogeneous sheathed powder blank to obtain the titanium alloy component.

[0013] The present invention adopts a method of first additive manufacturing and then hot isostatic pressing to prepare titanium alloy components, which significantly shortens the preparation cycle of additive manufacturing. The smaller the volume percentage of the homogeneous sheath in the solid part is, the shorter the preparation cycle is. At the same time, compared with the homogeneous sheath prepared by simply additive manufacturing, the method of the present invention can significantly improve the mechanical properties of the homogeneous sheath.

[0014] Furthermore, in step (1), in order to ensure airtightness, the wall thickness of the homogeneous sheath is greater than 1.5 mm, preferably greater than 2 mm; the number of reverse compensation and iterative calculation is not less than 3 times, preferably not less than 5 times. The homogeneous sheath will shrink and deform during the hot isostatic pressing step. If the wall thickness is too thin, it is easy to tear and damage, and the densification of the powder body cannot be guaranteed. On the other hand, since the homogeneous sheath is prepared by additive manufacturing technology, there may be pore defects, and too thin wall thickness will increase the risk of hot isostatic pressing failure. Iterative calculation is to reverse design the shape and size of the sheath. Since the purpose of the hot isostatic pressing step is to sinter discrete powders into a dense body, there is a volume shrinkage of more than about 30%. The more iterative calculations are performed, the more optimized the shape and size of the sheath can be obtained, and the higher the dimensional accuracy of the final molded part.

[0015] Furthermore, in step (1), the titanium alloy includes α-type titanium alloy, (α+β)-type titanium alloy and β-type titanium alloy.

[0016] Furthermore, in step (3), the printing layer thickness is 20-120 μm, the scanning spacing is 50-250 μm; the printing power is 280-370 W, and the scanning rate is 1200-1600 mm / s; preferably, the printing layer thickness is 100-120 μm, the scanning spacing is 100-250 μm, the printing power is 300-350 W, and the scanning rate is 1400-1600 mm / s. By regulating the printing power and the scanning rate, a homogeneous titanium alloy sheath with almost no holes can be prepared. In order to ensure that the homogeneous sheath does not fail in the hot isostatic pressing step, it is generally required that the homogeneous sheath has the lowest possible porosity. By adjusting the printing power and the scanning power (orthogonal test), the printing process with the highest density can be obtained. Generally speaking, the density of the homogeneous titanium alloy sheath is the highest at a higher printing power and a higher printing rate.

[0017] Further, in step (4), the filling density of the titanium alloy powder is greater than 0.62, and the vacuum degree of the titanium alloy homogeneous sheathed powder body is less than 0.5Pa, preferably the filling density is greater than 0.66, and the vacuum degree is less than 0.05Pa. A leak detector is used to test the homogeneous sheathed powder body for tightness. When the filling density is low, the deformation of the sheath and the powder body is relatively large, the forming accuracy of the powder metallurgy component will decrease, and there is even a risk of failure. As for the vacuum degree, it is mainly because the titanium alloy will dissolve elements such as oxygen, nitrogen, and hydrogen in the environment, which will have a certain effect on the chemical composition of the alloy and the mechanical properties of the powder metallurgy titanium alloy. The reason for the tightness test is that hot isostatic pressing is the coupling of high temperature and high pressure to complete the densification of the powder. Specifically, the gas pressure acts on the surface of the sheath and is further transmitted to the powder. If the sheath leaks, it is equivalent to putting the powder in a high-pressure gas. The gas pressure has no positive effect on the densification of the powder, but will reduce the density of the powder body.

[0018] Furthermore, in step (4), the titanium alloy powder is vibrated and filled into the titanium alloy homogeneous sheath through a reserved powder injection port, and subjected to vacuum degassing and sealing treatment to obtain a titanium alloy homogeneous sheath powder body.

[0019] Further, in step (5), during the hot isostatic pressing process: the heating rate is 5-10°C / min, the temperature is 800-1250°C, the pressure is greater than or equal to 120MPa, preferably the pressure is greater than 150MPa, and the heat preservation and pressure holding time is 0.5-4 hours. Hot isostatic pressing can be carried out in a hot isostatic pressing furnace. Preferably, before heating, an inert gas such as argon is filled into the furnace body. When the temperature reaches the preset temperature, the inert gas pressure is ensured to be greater than or equal to 120MPa; heat preservation and pressure holding for 0.5-4 hours; then the temperature is reduced and the pressure is released at a cooling rate of 1-2000°C / min until the titanium alloy powder component reaches the furnace discharge temperature. Generally speaking, the higher the temperature, the greater the pressure, and the longer the time, the higher the degree of densification of the powder. However, if the hot isostatic pressing temperature is too high and the heat preservation time is too long, the microstructure of the powdered titanium alloy will be significantly coarsened, thereby reducing the strength and plasticity of the powdered titanium alloy. Therefore, for different titanium alloy powders, the hot isostatic pressing parameters are not the same. Here, in order to broaden the scope of patent protection, the process parameters here are all a range.

[0020] Furthermore, in step (5), the pressure during the hot isostatic pressing process is 120-200 MPa.

[0021] Furthermore, in step (5), the cooling rate during the cooling and pressure relief process is 1-2000°C / min. The cooling rate can be equivalent to the cooling rate of heat treatment. The faster the cooling rate, the higher the strength of the material and the worse the plasticity. With an appropriate cooling rate, the strength and plasticity of the material are both good. With a slower cooling rate, due to the coarsening of the microstructure, the strength and plasticity of the material are not very good, but the fracture toughness of the material is the best. Therefore, the present invention selects a cooling rate of 1-2000°C / min.

[0022] Furthermore, in step (6), redundant structures such as the powder injection riser of the titanium alloy homogeneous sheathed powder blank after hot isostatic pressing are removed by mechanical processing or the like to obtain a titanium alloy component.

[0023] Compared with the prior art, the present invention has the following advantages and technical effects:

[0024] (1) Compared with the additive manufacturing process for directly preparing solid parts, the composite preparation process designed in the present invention only prepares a homogeneous sheath (part outer shell) in the additive manufacturing step, which significantly shortens the preparation cycle of additive manufacturing. The smaller the volume percentage of the homogeneous sheath in the solid part is, the shorter the preparation cycle is.

[0025] (2) The traditional hot isostatic pressing process requires the production of a sleeve and a mold. After hot isostatic pressing, the sleeve and the mold need to be removed by mechanical processing and chemical milling. The composite preparation process designed in the present invention adopts additive manufacturing to prepare a titanium alloy homogeneous sleeve. After hot isostatic pressing, the additively manufactured homogeneous sleeve becomes a part of the part. There is no need to produce a sleeve and a mold, which is environmentally friendly.

[0026] (3) The composite preparation process designed by the present invention, the hot isostatic pressing step can not only densify the powder body, but also further close the metallurgical defects such as pores in the additively manufactured homogeneous sheath, thereby improving the mechanical properties of the additively manufactured homogeneous sheath. The mechanical properties of the titanium alloy component are isotropic.

[0027] (4) The composite preparation process designed in the present invention can realize the recycling of the powder returned from additive manufacturing, further reducing the production cost of large-sized titanium alloy components. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0029] Figure 1 Schematic diagram of the TA15 titanium alloy homogeneous sheath prepared by the laser selective melting process of Comparative Example 2 (unit: mm).

[0030] Figure 2 This is a scanning electron microscope photograph of the microstructure of the longitudinal sample of TA15 titanium alloy prepared in Example 1.

[0031] Figure 3 This is a scanning electron microscope photograph of the transverse microstructure of the TA15 titanium alloy sample prepared in Example 1. DETAILED DESCRIPTION

[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0033] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0037] Unless otherwise specified, the room temperature in the embodiments of the present invention is 25±2°C.

[0038] In the present invention, the purpose of printing transverse samples and longitudinal samples is mainly to cut samples for mechanical property testing, wherein the sampling direction of the transverse samples is parallel to the printing plane, and the sampling direction of the longitudinal samples is perpendicular to the printing plane.

[0039] All raw materials used in the examples of the present invention are commercially available.

[0040] The technical solution of the present invention is further illustrated by the following embodiments.

[0041] Example 1 (Hot isostatic pressing additive manufacturing composite preparation method of the present invention)

[0042] This embodiment uses TA15 titanium alloy powder, and its alloy components, measured by mass percentage, are: Al 6.55%, Zr 1.8%, Mo 1.26%, V 1.65%, Si 0.05%, Fe 0.03%, O 0.098%, and the balance is Ti.

[0043] The titanium alloy homogeneous sheath is prepared by the laser selective melting process in the additive manufacturing process. The particle size composition of the selected TA15 titanium alloy powder is 5-53μm, and the average particle size is 33.9μm. The particle size composition of the powder for filling the cavity of the titanium alloy homogeneous sheath is 5-250μm, and the average particle size is 95μm.

[0044] Laser selective melting technology was used to print two different titanium alloy homogeneous sheaths. Pure titanium substrate was used for printing. The printing layer thickness was 100μm, the scanning interval was 150μm, the printing power was 350W, the scanning rate was 1400mm / s, and the scanning strategy was 90° scanning.

[0045] Size Figure 1 The outer dimensions of the homogeneous package of the longitudinal sample are 12mm long, 12mm wide, and 26mm high, and the cavity dimensions are 9mm long, 9mm wide, and 6mm high; the outer dimensions of the homogeneous package of the transverse sample are 26mm long, 12mm wide, and 12mm high, and the cavity dimensions are 6mm long, 9mm wide, and 9mm high.

[0046] TA15 titanium alloy powder with a size of 5-250 μm was vibrated and filled into a titanium alloy homogeneous package, and the filling density of the powder was 0.64.

[0047] After the powder is filled, the powder injection port is welded to the stainless steel pipe for degassing by argon arc welding.

[0048] The titanium alloy homogeneous encapsulated powder body is subjected to vacuum degassing pretreatment. The degassing pretreatment system is: 400℃, 8h, vacuum degree less than 10 -2 Pa.

[0049] After vacuum degassing treatment, the degassed stainless steel pipe is first pressure welded and then argon arc welded, and finally the degassing pipe protective sleeve is welded to prevent vacuum leakage before hot isostatic pressing.

[0050] The TA15 titanium alloy homogeneous sheathed powder was placed in a hot isostatic pressing furnace, and the sheath was heated from room temperature to 930°C at a heating rate of 10°C / min, with a pressure of 150MPa, and maintained at this temperature for 3 hours; then the temperature was lowered and the pressure was released.

[0051] The powder injection structure was removed by machining to obtain TA15 titanium alloy.

[0052] Comparative Example 1 (Traditional Powder Hot Isostatic Pressing Process)

[0053] This comparative example uses TA15 titanium alloy powder, whose alloy composition is: Al 6.55%, Zr 1.8%, Mo 1.26%, V

[0054] 1.65%, Si 0.05%, Fe 0.03%, O 0.098%, and the balance is Ti.

[0055] TA15 titanium alloy powder (powder particle size is 5-250μm) is filled into a low carbon steel cylindrical sleeve. The outer diameter of the sleeve is 150mm, the height is 110mm, and the wall thickness is 4mm. Through vibration filling and volume deduction method, the filling relative density of TA15 titanium alloy powder is obtained to be 0.66.

[0056] After the powder is filled, the powder injection port is welded to the stainless steel pipe for degassing by argon arc welding.

[0057] The package is subjected to vacuum degassing pretreatment. The degassing pretreatment system is: 400℃, 8h, vacuum degree less than 10 -2 Pa.

[0058] After vacuum degassing treatment, the sheathed degassing stainless steel pipe is first pressure welded and then argon arc welded, and finally the degassing pipe protection sleeve is welded to prevent vacuum leakage before hot isostatic pressing.

[0059] The package powder is placed in a hot isostatic pressing furnace, and the temperature of the package is increased from room temperature to 930°C at a heating rate of 10°C / min, with a pressure of 150MPa, and the temperature and pressure are maintained for 3 hours; the temperature is reduced and the pressure is released.

[0060] Finally, the low-carbon steel sheath was removed by mechanical processing to obtain powder metallurgy TA15 titanium alloy.

[0061] Comparative Example 2 (Additive Manufacturing Process)

[0062] This comparative example uses TA15 titanium alloy powder, whose alloy composition is: Al 6.55%, Zr 1.8%, Mo 1.26%, V

[0063] 1.65%, Si 0.05%, Fe 0.03%, O 0.098%, and the balance is Ti.

[0064] The powder particle size is 5-53μm, and the average particle size is 33.9μm.

[0065] The TA15 titanium alloy block sample was prepared by the laser selective melting process in the additive manufacturing process. A pure titanium substrate was used for printing, the printing layer thickness was 30μm, the scanning spacing was 120μm, the printing power was 280W, the scanning rate was 700mm / s, and the scanning strategy was 90° scanning.

[0066] Block samples are divided into two categories, longitudinal samples and transverse samples. The longitudinal sample size is 12mm long, 12mm wide, and 26mm high, while the transverse sample size is 26mm long, 12mm wide, and 12mm high.

[0067] After printing, the substrate was removed by wire cutting to obtain the additively manufactured TA15 titanium alloy.

[0068] According to GB / T 228.1-2021, the mechanical properties of the TA15 titanium alloy obtained in Example 1 and Comparative Examples 1-2 were tested, and the results are shown in Table 1, where the TA15 titanium alloy forging data was selected from "GB / T 2965-2007 Titanium and Titanium Alloy Bars".

[0069] Table 1 Comparison of mechanical properties of TA15 titanium alloy obtained in Example 1 and Comparative Examples 1-2

[0070] state Yield strength / MPa Tensile strength / MPa Elongation / % Comparative Example 1 866 952 15.0 Comparative Example 2 Horizontal 1275 1350 2.4 Comparative Example 2 Vertical 996 1124 10.0 Example 1 Horizontal 833 930 9.4 Example 1: Vertical 881 954 10.2 TA15 Titanium Alloy Forgings 825 885 8

[0071] After testing, the powder metallurgy TA15 titanium alloy laser additive manufacturing homogeneous sheath and powder blank prepared by the hot isostatic pressing additive manufacturing composite preparation method of the present invention (hereinafter referred to as the composite process of the present invention) have good interface bonding. Since the strength of the laser additive manufacturing homogeneous sheath area is high, and the plasticity of the powder blank is good, and since the interface of the two parts is well bonded, the TA15 titanium alloy designed and prepared by the present invention has good strength and plasticity matching, as shown in Table 1. The mechanical properties of the titanium alloy prepared by the composite preparation method of the present invention can reach the TA15 forging titanium alloy standard (GB / T 2965-2007).

[0072] Comparison of the efficiency of the additive manufacturing process represented by the laser selective melting process and the composite process of the present invention (taking the TA15 titanium alloy in Example 1 as an example):

[0073] The solid cube of the model part with a length of 200 mm, a width of 200 mm, and a height of 290 mm was prepared by using the laser selective melting printing process in Comparative Example 2, and the estimated printing time was about 581 hours. Taking the production of 10 model parts as a batch, the laser selective melting process was used alone, and the printer was required for a total of about 5810 hours. The composite process of the present invention was used to prepare a hollow cube (homogeneous package) with a thickness of 2 mm, and the estimated printing time was about 41 hours. Using the composite process of the present invention, the first step is to print the homogeneous package, which takes about 410 hours to print; the second step is hot isostatic pressing process, which involves four links: powder filling, vacuum degassing, hot isostatic pressing and mechanical processing: powder filling, each model part requires 0.5 hours, a total of 5 hours; vacuum degassing, 5 parts blanks are treated as a group, a total of two groups, and the estimated time is 24 hours; hot isostatic pressing, 5 parts blanks are a group, including heating and cooling time, the estimated time is 48 hours; mechanical processing to remove the powder injection structure, it is estimated to take 10 hours, a total of 497 hours, and the production cycle of a single part is about 50 hours. The comparison of the preparation efficiency of the above two processes is shown in Table 2. By comparing the laser selective melting process and the composite process of the present invention, it can be seen that for large-sized parts, the present invention can significantly shorten the processing and preparation cycle, and the smaller the volume of the titanium alloy homogeneous package occupies the actual part, the higher the production efficiency of the present invention.

[0074] Table 2 Comparison of preparation process and production efficiency of laser selective melting process and composite process of the present invention

[0075]

[0076] Figure 1 Schematic diagram of the TA15 titanium alloy homogeneous sheath prepared by the laser selective melting process of Comparative Example 2 (unit: mm).

[0077] Figure 2 This is a scanning electron microscope photo of the microstructure of the longitudinal sample of TA15 titanium alloy prepared in Example 1. It can be seen that the microstructure of TA15 titanium alloy consists of two parts, namely the laser additive manufacturing homogeneous jacket area and the powder blank area. The microstructure of the laser additive manufacturing area is composed of vertical columnar crystals (original β grain structure), and the columnar crystals are composed of α laths (gray) and a small amount of lamellar β phase (white), without obvious hole defects; the microstructure of the powder blank area is composed of equiaxed and strip-shaped α phase (gray) and a small amount of lamellar β phase (white), and there are a small number of micropores with a size of less than 1μm in the organization.

[0078] Figure 3 This is a scanning electron microscope photo of the transverse microstructure of the TA15 titanium alloy sample prepared in Example 1. It can be seen that the microstructure of the TA15 titanium alloy consists of two parts, namely the laser additive manufacturing homogeneous jacket area and the powder blank area. The laser additive manufacturing area microstructure is composed of equiaxed original β grains, and the equiaxed grains are composed of α laths (gray) and a small amount of lamellar β phase (white), without obvious hole defects; the powder blank area microstructure is composed of equiaxed and strip α phase (gray) and a small amount of lamellar β phase (white), and there are a small number of micropores with a size of less than 1μm in the organization.

[0079] Example 2

[0080] This embodiment uses TC4 titanium alloy powder, and its alloy components, measured by mass percentage, are: Al 6.05%, V 3.95%, Si 0.04%, Fe 0.02%, O 0.15%, and the balance is Ti.

[0081] The titanium alloy homogeneous sheath is prepared by the laser selective melting process in the additive manufacturing process. The particle size composition of the selected TC4 titanium alloy powder is 5-53μm, and the average particle size is 35μm. The particle size composition of the powder for filling the cavity of the titanium alloy homogeneous sheath is 15-250μm, and the average particle size is 92μm.

[0082] Two different titanium alloy cylindrical homogeneous sheaths were prepared by laser selective melting process, with dimensions of 10 mm in diameter, 60 mm in height and 1.5 mm in wall thickness.

[0083] A pure titanium substrate was used for printing, with a printing layer thickness of 50 μm, a scanning spacing of 140 μm, a printing power of 280 W, a scanning rate of 1200 mm / s, and a scanning strategy of 67° scanning.

[0084] TC4 titanium alloy powder with a size of 5-250 μm was vibrated and filled into a titanium alloy homogeneous package, and the filling density of the powder was 0.65.

[0085] After the powder is filled, the powder injection port is welded to the stainless steel pipe for degassing by argon arc welding.

[0086] The titanium alloy homogeneous encapsulated powder body is subjected to vacuum degassing pretreatment. The degassing pretreatment system is: 220℃, 4h, vacuum degree less than 10 -2 Pa.

[0087] After vacuum degassing treatment, the degassed stainless steel pipe is first pressure welded and then argon arc welded, and finally the degassing pipe protective sleeve is welded to prevent vacuum leakage before hot isostatic pressing.

[0088] The TA15 titanium alloy homogeneous sheathed powder was placed in a hot isostatic pressing furnace, and the sheath was heated from room temperature to 920°C at a heating rate of 10°C / min, with a pressure of 150MPa, and maintained at this temperature for 3h; then the temperature was lowered and the pressure was released, with a cooling rate of 50°C / min.

[0089] The powder injection structure was removed by machining to obtain TC4 titanium alloy.

[0090] Comparative Example 3 (Traditional Powder Hot Isostatic Pressing Process)

[0091] This embodiment uses TC4 titanium alloy powder, and its alloy components, measured by mass percentage, are: Al 6.05%, V 3.95%, Si 0.04%, Fe 0.02%, O 0.15%, and the balance is Ti.

[0092] TC4 titanium alloy powder (powder size 5-250μm) was filled into a low carbon steel cylindrical sleeve. The outer diameter of the sleeve was 40mm, the height was 110mm, and the wall thickness was 2mm. Through vibration filling and volume deduction method, the filling relative density of TC4 titanium alloy powder was obtained to be 0.66.

[0093] After the powder is filled, the powder injection port is welded to the stainless steel pipe for degassing by argon arc welding.

[0094] The package is pre-treated by vacuum degassing. The degassing pre-treatment system is: 220℃, 4h, vacuum degree less than 10 -2 Pa.

[0095] After vacuum degassing treatment, the sheathed degassing stainless steel pipe is first pressure welded and then argon arc welded, and finally the degassing pipe protection sleeve is welded to prevent vacuum leakage before hot isostatic pressing.

[0096] The package powder was placed in a hot isostatic pressing furnace, and the temperature of the package was increased from room temperature to 920°C at a heating rate of 10°C / min, with a pressure of 150MPa, and the temperature and pressure were maintained for 3 hours; the temperature was reduced and the pressure was released, with a cooling rate of 50°C / min.

[0097] Finally, the low-carbon steel sheath is removed by mechanical processing to obtain powder metallurgy TC4 titanium alloy.

[0098] Comparative Example 4 (Additive Manufacturing Process)

[0099] TC4 titanium alloy powder is used, and its alloy composition is as follows, in terms of mass percentage: Al 6.05%, V 3.95%, Si 0.04%, Fe 0.02%, O 0.15%, and the balance is Ti.

[0100] The powder particle size is 5-53μm, and the average particle size is 35μm.

[0101] The TC4 titanium alloy cylinder was prepared by laser selective melting process in additive manufacturing. The sample size is 10 mm in diameter and 60 mm in height.

[0102] A pure titanium substrate was used for printing, with a printing layer thickness of 50 μm, a scanning spacing of 140 μm, a printing power of 280 W, a scanning rate of 1200 mm / s, and a scanning strategy of 67° scanning.

[0103] After printing, the substrate was removed by wire cutting to obtain the additively manufactured TC4 titanium alloy.

[0104] The tensile properties and high cycle fatigue properties (four-point bending) of the TC4 titanium alloy obtained in Example 2 and Comparative Examples 3-4 were tested. The results are shown in Table 3, where the TC4 titanium alloy forging data was selected from GB / T 2965-2007 Titanium and Titanium Alloy Bars.

[0105] Table 3 Comparison of mechanical properties of TA15 titanium alloy obtained in Example 2 and Comparative Examples 3-4

[0106] state Yield strength / MPa Tensile strength / MPa Elongation / % Fatigue strength / MPa Example 2 920 1020 16.4 600 Comparative Example 3 890 930 17.5 500 Comparative Example 4 1190 1230 4.2 300 TC4 Titanium Alloy Forgings 825 895 10 —

[0107] In summary, the titanium alloy components prepared by the hot isostatic pressing additive manufacturing method of the present invention have good interface bonding between the additively manufactured homogeneous sheath and the powder blank, no obvious metallurgical defects in the microstructure, and mechanical properties close to the standards of forgings with the same composition. It is a low-cost and high-performance rapid prototyping technology for preparing large-size titanium alloy components.

[0108] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A hot isostatic pressing additive manufacturing composite preparation method for titanium alloy components, It is characterized in that The following steps are involved: (1) According to the shape and size of the target part, the wall thickness of the additively manufactured titanium alloy homogeneous sheath is fixed, and finite element simulation is performed. Through inverse compensation and iterative calculation, a three-dimensional model of the titanium alloy homogeneous sheath is determined, and the titanium alloy homogeneous sheath is reserved with a powder injection port; (2) Slicing the three-dimensional model of the titanium alloy homogeneous sheath using 3D printing slicing software and outputting an STL file; (3) importing the STL file into a 3D printer, fixing the printing layer thickness and scanning spacing, regulating the printing power and scanning rate of additive manufacturing, and preparing the titanium alloy homogeneous sheath; (4) filling the titanium alloy powder into the titanium alloy homogeneous sheath through a reserved powder injection port, and performing degassing and sealing welding to obtain a titanium alloy homogeneous sheath powder body; (5) hot isostatic pressing the titanium alloy homogeneous sheathed powder body, and then cooling and releasing the pressure after the pressing to obtain a titanium alloy homogeneous sheathed powder body; (6) removing redundant structures of the titanium alloy homogeneous sheathed powder blank to obtain the titanium alloy component.

2. The hot isostatic pressing additive manufacturing composite preparation method of the titanium alloy component according to claim 1, It is characterized in that In step (1), the wall thickness of the homogeneous sheath is greater than 1.5 mm; and the reverse compensation and iterative calculation are performed no less than 3 times.

3. The hot isostatic pressing additive manufacturing composite preparation method of the titanium alloy component according to claim 1, It is characterized in that In step (1), the titanium alloy includes α-type titanium alloy, (α+β)-type titanium alloy and β-type titanium alloy.

4. The hot isostatic pressing additive manufacturing composite preparation method of the titanium alloy component according to claim 1, It is characterized in that In step (3), the printing layer thickness is 20-120 μm, the scanning interval is 50-250 μm; the printing power is 280-370 W, and the scanning rate is 1200-1600 mm / s.

5. The hot isostatic pressing additive manufacturing composite preparation method of the titanium alloy component according to claim 1, It is characterized in that In step (4), the packing density of the titanium alloy powder is greater than 0.62, and the vacuum degree of the titanium alloy homogeneous sheathed powder body is less than 0.5Pa.

6. The hot isostatic pressing additive manufacturing composite preparation method of the titanium alloy component according to claim 1, It is characterized in that In step (5), during the hot isostatic pressing process: the heating rate is 5-10°C / min, the temperature is 800-1250°C, the pressure is greater than or equal to 120MPa, and the heat and pressure holding time is 0.5-4 hours.

7. The hot isostatic pressing additive manufacturing composite preparation method of the titanium alloy component according to claim 6, It is characterized in that In step (5), the pressure during the hot isostatic pressing process is 120-200 MPa.

8. The hot isostatic pressing additive manufacturing composite preparation method of a titanium alloy component according to claim 1, It is characterized in that In step (5), the cooling rate during the cooling and pressure relief process is 1-2000°C / min.

Citation Information

Patent Citations

  • Hot isostatic pressing forming method of titanium alloy gas cylinder hemispheroid

    CN108971495A

  • Titanium alloy component and preparation method thereof

    CN110539000A