Laser spot welding connection method and system for dissimilar materials
Through spiral scanning laser spot welding technology, specific formulas are used to calculate the spiral pitch and laser energy, which solves the problems of unstable molten pool and uneven material mixing in the welding of dissimilar materials, forming a uniform IMC layer, improving welding quality and efficiency, and reducing Eliminate welding defects and improve the performance of welded parts.
Patent Information
- Application Number
- CN202411185240.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-22
AI Technical Summary
During the welding process of dissimilar materials such as aluminum alloys and high-strength steel, problems such as molten pool instability, liquid metal evaporation, uneven material mixing, and weld segregation are prone to occur, leading to welding defects such as pores, cracks, slag inclusions, and lack of fusion, which affect the welding performance and applications of the software.
The spiral scanning laser spot welding method is used to scan laser welding through spiral lines with different spacing and radii. It is combined with the gap adjustment block and positioning clamping mechanism to reduce the material positioning adjustment time. A specific formula is used to calculate the spiral spacing and laser energy to form a uniform Intermetallic compound (IMC) layer ensures uniform force in all directions and improves welding quality.
It achieves high-efficiency and high-quality welding of dissimilar materials, reduces welding defects, and improves the performance and application value of welded parts.
Smart Images

Figure CN118808912A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of dissimilar material welding, and in particular to a dissimilar material laser spot welding connection method and system. Background Art
[0002] In modern engineering practice, the joining of dissimilar materials has attracted much attention because a single material is difficult to meet the needs of complex working environments. Among them, aluminum alloys and high-strength steels are widely used in the automotive, aerospace and other industries due to their respective characteristics. However, the significant differences in the physical and chemical properties of aluminum / steel make the welding process difficult, and it is easy to form hard and brittle intermetallic compounds, which deteriorates the quality of the joint. These challenges include problems such as unstable molten pool, evaporation of liquid metal, uneven material mixing and weld segregation, which may lead to welding defects such as pores, cracks, slag inclusions, and lack of fusion, which have a serious impact on the performance and application of welded parts. Therefore, there is an urgent need to develop a high-quality dissimilar material welding technology.
[0003] In the progress of contemporary industrial technology, galvanometer scanning laser welding technology has demonstrated excellent performance in the field of precision welding of heterogeneous metal materials with its excellent energy concentration, fine operation control and efficient processing rate, and is widely used in high-end industrial fields such as aerospace and automobile manufacturing. This technology provides a solution for the combination of dissimilar materials such as aluminum alloy and high-strength steel.
[0004] In addition, precise gap adjustment and stable positioning between dissimilar materials are also key factors in optimizing the welding process. Therefore, developing an efficient and precise laser welding control technology for dissimilar materials is an important topic for current scientific research and industrial applications. Summary of the invention
[0005] The purpose of the present invention is to solve the above problems and propose a control method for spiral scanning laser spot welding of dissimilar materials, using spiral lines with different spacing and radius for scanning laser spot welding. The positioning adjustment time of the dissimilar material welding plate is reduced by using a gap adjustment block and a positioning clamping mechanism. During welding, the spiral point is used to make the force in all directions uniform, and the bearing and bonding area is increased in a limited space. Through the precise control of the laser energy with different numbers of turns, a continuous and uniform IMC layer is formed, and the dissimilar material welding process is completed with high efficiency and high quality.
[0006] A method for laser spot welding of dissimilar materials, the laser spot welding connection comprising the following steps: Superimpose two or more workpieces to form a workpiece to be welded; Laser spiral welding is performed using a scanning galvanometer; Setting welding parameters, wherein the welding parameters include at least laser power, welding speed, and defocus; Laser spiral welding is performed according to welding parameters, and a spiral weld is finally formed; The spiral pitch of the laser spiral welding Δr>W, W is calculated by the following formula: Among them, η is the heat input efficiency, P is the laser power, v is the welding speed, D is the spot diameter, n is the index of the spot diameter affecting the melt width, a and b are empirical coefficients, and k is the thermal conductivity of the material.
[0007] As a preferred technical solution, a and b are empirical coefficients, the value range of a is 0.2~1.2, and the value range of b is 0.5~1.5.
[0008] As a preferred technical solution, the spiral pitch Δr is as small as possible while satisfying Δr>W.
[0009] As a preferred technical solution, the heat input efficiency is set in the range of 0.7-0.8.
[0010] As a preferred technical solution, the spot diameter D is calculated by the following formula: Among them, M 2 is the beam quality factor, D0 is the minimum spot diameter at the beam waist, λ is the wavelength, and z is the defocus.
[0011] As a preferred technical solution, the laser power of the laser welding is 1000-1200W.
[0012] As a preferred technical solution, the defocusing amount of the laser welding is -5-5mm.
[0013] As a preferred technical solution, the scanning speed of the laser welding is 140-180 mm / s.
[0014] A welding device is provided, which performs the aforementioned spiral scanning laser spot welding method for dissimilar materials.
[0015] The welding device comprises a collimating aperture, a scanning galvanometer lens, an X-direction scanning galvanometer, an optical path, a focusing lens, a Y-direction scanning galvanometer, and a reflecting mirror; The collimating aperture is used to control the size and direction of the light to ensure the stability and collimation of the light; The scanning galvanometer lens is used to achieve precise control of the laser beam on a two-dimensional plane; The X-direction scanning galvanometer and the Y-direction scanning galvanometer are used to control the scanning of the laser beam in the X direction and the Y direction respectively; The focusing lens is used to focus the laser beam to a small spot; The reflector is used to change the direction and angle of light propagation; The optical path starts from the laser, passes through the collimating aperture, the reflector, the X-direction scanning galvanometer, the Y-direction scanning galvanometer, the reflector, the scanning galvanometer lens, and finally reaches the welding area.
[0016] The present invention has the following beneficial effects: During welding, the invention adopts spiral points with specific spacing calculated by specific formulas to make the force in all directions uniform and increase the bearing and bonding area in a limited space. Through the precise control of laser energy with different numbers of turns, a continuous and uniform IMC layer is formed, and the welding process of dissimilar materials is completed with high efficiency and high quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the structure of the galvanometer scanning laser welding equipment; Figure 2 Macroscopic morphology of weld surface under different spiral pitch Δr Figure 3 The cross-sectional morphology of the weld at different spiral pitches Δr Figure 4 Mechanical properties of welded joints at different spiral pitches Δr Figure 5 The fracture morphology of the welded joint under the optimal process parameters The reference numerals are as follows: 1-collimating aperture, 2-scanning galvanometer lens, 3-X-direction scanning galvanometer, 4-optical path, 5-focusing lens, 6-Y-direction scanning galvanometer, 7-reflecting mirror, 8-steel plate, 9-aluminum plate. DETAILED DESCRIPTION
[0018] The present invention relates to the field of welding of dissimilar materials, and discloses a method for laser spot welding of dissimilar materials, the method comprising: superimposing two or more workpieces to form a workpiece to be welded; using a scanning galvanometer for laser spiral welding; setting welding parameters, the welding parameters at least including laser power, welding speed, and defocus; performing laser spiral welding according to the welding parameters, and finally forming a spiral weld; the spiral pitch Δr>W of the laser spiral welding. During welding, the present invention uses spiral points of a specific pitch calculated by a specific formula, so that the force in each direction is uniform, and the bearing and bonding area is increased in a limited space. Through the precise control of the laser energy of different numbers of turns, a continuous and uniform IMC layer is formed, and the welding process of dissimilar materials is completed efficiently and with high quality.
[0019] The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" or "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0020] Galvanometer scanning laser welding technology: The galvanometer scanning laser welding machine uses galvanometer technology to control the direction and focal length of the laser beam by adjusting the galvanometer. The galvanometer can achieve rapid adjustment and high-frequency scanning, so that the laser beam can be accurately focused in the welding area. By finely adjusting the focal length and scanning speed, the galvanometer laser welding machine can achieve high-speed and fine welding. This technology is not only suitable for plane welding, but also can be applied to the welding of three-dimensional complex configurations to improve welding quality and efficiency.
[0021] IMC layer: IMC layer is Intermetallic compound layer, which means interfacial alloy co-compound. In a broad sense, IMC refers to the formation of a layer of alloy-like compound when certain metals are in close contact with each other, resulting in atomic migration interaction between their interfaces, and the molecular formula of this layer of compound can be given. In a narrow sense in the field of welding, IMC specifically refers to the co-compounds between copper-tin, gold-tin, nickel-tin and silver-tin.
[0022] Defocus Defocus refers to the distance between the laser beam focus and the workpiece surface during welding. In laser welding, the selection of defocus has an important impact on the welding quality. The appropriate defocus can ensure that the laser beam energy is evenly distributed on the workpiece, achieving high-quality welding.
[0023] When the defocus is 0mm, it means that the focus of the laser beam is exactly on the surface of the workpiece. In this case, the laser energy density is the highest and the welding speed may be faster, but it may also cause the heat affected zone of the weld to increase, increasing the risk of welding deformation.
[0024] If the defocus is positive, that is, the laser beam focus is above the workpiece, the energy distribution of the laser beam is more uniform, the heat affected zone of welding will be reduced, and the risk of welding deformation will be reduced. However, too large a positive defocus may slow down the welding speed and affect production efficiency.
[0025] On the contrary, if the defocus is negative, that is, the focus of the laser beam is below the workpiece, the laser energy is more concentrated, which may lead to an increase in welding speed, but it may also increase the risk of welding deformation and welding defects.
[0026] For ease of understanding, the specific process of the embodiment of the present invention is described below: like Figure 1 , is a common galvanometer scanning laser welding equipment. This equipment is a precision welding equipment. Its core structure and working principle ensure the precise control and high-speed scanning of the laser beam. The following is a structural introduction to the main components of the equipment: Collimation diaphragm 1: The collimation diaphragm is usually located at the output end of the laser to ensure the parallelism and collimation of the laser beam. It can eliminate the divergence angle of the laser beam and make the laser energy more concentrated and stable.
[0027] Scanning galvanometer lens 2: The scanning galvanometer lens is one of the key components of the galvanometer scanning laser welding equipment. It contains the X-direction scanning galvanometer and the Y-direction scanning galvanometer. Through the rapid scanning movement in these two directions, the laser beam can be accurately positioned and moved at high speed on a two-dimensional plane.
[0028] X-direction scanning galvanometer 3: The X-direction scanning galvanometer is responsible for scanning the laser beam in the horizontal direction (X axis). It is usually a high-speed rotating mirror. By precisely controlling its rotation angle and speed, the laser beam can be accurately scanned in the X axis.
[0029] Optical path 4: The optical path refers to the path of the laser beam from the laser, through various optical elements, and finally to the workpiece. In the galvanometer scanning laser welding equipment, the design and optimization of the optical path is crucial to ensure the stability and energy distribution of the laser beam.
[0030] Focusing lens 5: The focusing lens is used to focus the laser beam onto the workpiece surface so that its energy density reaches the level required for welding. By adjusting the position and focal length of the focusing lens, the focal size and position of the laser beam can be controlled to achieve welding of different depths and widths.
[0031] Y-direction scanning galvanometer 6: The Y-direction scanning galvanometer is similar to the X-direction scanning galvanometer, but it is responsible for scanning the laser beam in the vertical direction (Y axis). By precisely controlling the rotation angle and speed of the Y-direction scanning galvanometer, accurate scanning of the laser beam on the Y axis can be achieved.
[0032] Reflector 7: The reflector is used to change the propagation direction of the laser beam and guide it to the scanning galvanometer lens and focusing lens. In the galvanometer scanning laser welding equipment, multiple reflectors may be required to build a suitable optical path.
[0033] Steel plate 8 and aluminum plate 9: As the distance, two materials, steel plate 8 and aluminum plate 9, are used. These two materials usually appear on the workbench of the galvanometer scanning laser welding equipment as welding test pieces or workpieces. During the welding process, the laser beam acts on the joint of the two plates to achieve welding by melting the materials.
[0034] A welding device is provided, and the welding device performs the above-mentioned welding method.
[0035] The welding device comprises a collimating aperture, a scanning galvanometer lens, an X-direction scanning galvanometer, an optical path, a focusing lens, a Y-direction scanning galvanometer, and a reflecting mirror; The collimating aperture is used to control the size and direction of the light to ensure the stability and collimation of the light; The scanning galvanometer lens is used to achieve precise control of the laser beam on a two-dimensional plane; The X-direction scanning galvanometer and the Y-direction scanning galvanometer are used to control the scanning of the laser beam in the X direction and the Y direction respectively; The focusing lens is used to focus the laser beam to a small spot; The reflector is used to change the direction and angle of light propagation; The optical path starts from the laser, passes through the collimating aperture, the reflector, the X-direction scanning galvanometer, the Y-direction scanning galvanometer, the reflector, the scanning galvanometer lens, and finally reaches the welding area.
[0036] The laser spot welding connection method of dissimilar materials of the present invention is as follows: Superimpose two or more workpieces to form a workpiece to be welded; Laser spiral welding is performed using a scanning galvanometer; Setting welding parameters, wherein the welding parameters include at least laser power, welding speed, and defocus; Laser spiral welding is performed according to welding parameters, and a spiral weld is finally formed; The spiral pitch of the laser spiral welding Δr>W, W is calculated by the following formula: Wherein, η is the heat input efficiency, P is the laser power, v is the welding speed, D is the spot diameter, n is the index of the spot diameter affecting the melt width, a and b are empirical coefficients, and k is the thermal conductivity of the material. The a and b are empirical coefficients, and the spiral pitch Δr is as small as possible when Δr>W is satisfied. The heat input efficiency setting range is 0.7-0.8.
[0037] The spot diameter D is calculated by the following formula: Among them, M 2is the beam quality factor, D0 is the minimum spot diameter at the beam waist, λ is the wavelength, and z is the defocus.
[0038] The laser power of the laser welding is 1000-1200 W. The defocusing amount of the laser welding is -5-5 mm. The scanning speed of the laser welding is 140-180 mm / s.
[0039] Experimental process and results 1.5mm 6061 aluminum alloy (aluminum for short) and 1.0mm DP980 high-strength steel (steel for short) were used, with the same size of 130mm × 38mm. For lap welding, the steel plate was overlapped on the aluminum plate with an overlap distance of 38mm. Before welding, the specimens were polished to remove the surface oxide film, and then ultrasonically cleaned in acetone for 15min to remove surface oil. The laser welding system mainly consists of a Kuka robot, a TruDisk 8001 disk laser and a 3D PFO galvanometer scanner. The maximum output power is 8 kW, the wavelength is 1030 nm, and the beam quality parameter is 4.0 mm-rad. The laser scanning path is generated by a galvanometer scanning system (3D PFO galvanometer), such as Figure 1 As shown. In order to minimize the influence of the gap on the welding process, the clamping between the aluminum plate and the steel plate is achieved by the pre-tightening force of the clamp bolt. During the laser welding process, nitrogen with a flow rate of 15 L / min is used to protect the joint from oxidation to improve the quality of weld formation. The laser scans along the spiral scanning path. First, the spiral pitch Δr>w of the laser spiral welding is calculated by the following formula: Among them, η is the heat input efficiency, P is the laser power, v is the welding speed, D is the spot diameter, n is the index of the spot diameter affecting the melt width, a and b are empirical coefficients, k is the thermal conductivity of the material, a is 1, and b is 1.
[0040] Calculated by the above formula, the optimal Δr value under the current test conditions is 0.25 mm.
[0041] Then, we conducted experiments to verify the results. We designed experiments with different spiral pitches Δr. First, we conducted experiments with Δr of 0.2mm, 0.25mm, and 0.3mm while keeping the number of turns unchanged. Then, we conducted experiments with Δr of 0.2mm, 0.25mm, and 0.3mm while keeping the diameter of the solder joint unchanged. Finally, we used a Leica S8APO stereo microscope to photograph the macroscopic surface of the sample, as shown in the figure. Figure 2 As shown in the figure, the Leica DM4 M metallographic microscope takes a picture of the sample cross section. Figure 3As shown in Figure 2, the tensile test was carried out on the welding samples obtained under different welding processes using a SUNSUTM5000 electronic universal tensile testing machine. The tensile rate was 1 mm / min. Three samples were taken for tensile testing with the same process parameters. The average value of the maximum tensile shear force of the three samples was taken as the tensile shear force that the sample could ultimately withstand. The results are shown in Figure 2. Figure 4 The fracture surface was analyzed by Tenscan MIRA3 LMH scanning electron microscope. Figure 5 The corresponding welding parameters are defined as follows: laser power: 1050 W, welding speed: 150 mm / s, defocus: -4 mm. Through experimental analysis, it can be known that the Δr value of 0.25 mm is the optimal value. It can be seen that the empirical formula of the present invention can quickly obtain the optimal Δr value.
[0042] Those skilled in the art can clearly understand that, for the convenience and brevity of description, the specific working process of the above-described system, device, or unit can refer to the corresponding process in the aforementioned method embodiment and will not be repeated here.
[0043] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for laser spot welding of dissimilar materials, characterized in that: The laser spot welding connection comprises the following steps: Superimpose two or more workpieces to form a workpiece to be welded; Laser spiral welding is performed using a scanning galvanometer; Setting welding parameters, wherein the welding parameters include at least laser power, welding speed, and defocus; Laser spiral welding is performed according to welding parameters, and a spiral weld is finally formed; The spiral pitch of the laser spiral welding Δr>W, W is calculated by the following formula: Among them, η is the heat input efficiency, P is the laser power, v is the welding speed, D is the spot diameter, n is the index of the spot diameter affecting the melt width, a and b are empirical coefficients, and k is the thermal conductivity of the material.
2. A method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The a and b are empirical coefficients, the value range of a is 0.2~1.2, and the value range of b is 0.5~1.
5.
3. The method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The spiral pitch Δr is preferably as small as possible while satisfying Δr>W.
4. The method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The heat input efficiency is set in the range of 0.7-0.
8.
5. The method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The spot diameter D is calculated by the following formula: Among them, M 2 is the beam quality factor, D0 is the minimum spot diameter at the beam waist, λ is the wavelength, and z is the defocus.
6. The method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The laser power of the laser welding is 1000-1200W.
7. The method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The defocusing amount of the laser welding is -5-5mm.
8. The method for laser spot welding of dissimilar materials according to claim 1, characterized in that: The scanning speed of the laser welding is 140-180 mm / s.
9. A welding device, which performs the spot welding connection method according to any one of claims 1 to 8.
10. A welding device according to claim 1, comprising a collimating aperture, a scanning galvanometer lens, an X-direction scanning galvanometer, an optical path, a focusing lens, a Y-direction scanning galvanometer, and a reflector; The collimating aperture is used to control the size and direction of the light to ensure the stability and collimation of the light; The scanning galvanometer lens is used to achieve precise control of the laser beam on a two-dimensional plane; The X-direction scanning galvanometer and the Y-direction scanning galvanometer are used to control the scanning of the laser beam in the X direction and the Y direction respectively; The focusing lens is used to focus the laser beam to a small spot; The reflector is used to change the direction and angle of light propagation; The optical path starts from the laser, passes through the collimating aperture, the reflector, the X-direction scanning galvanometer, the Y-direction scanning galvanometer, the reflector, the scanning galvanometer lens, and finally reaches the welding area.
Citation Information
Patent Citations
Laser beam welding with a spiral weld path having a first order of continuity
CN106583926A
Laser welding method, laser welding condition determining method, and laser welding system
CN107530831A
Laminated laser spot welding method for high-strength steel
CN114247999A
Laser double-beam double-helix spot welding method
CN115464266A
Steel-aluminum laser galvanometer welding method
CN116652385A
Cited By
Laser flight welding method for vehicle door inner plate
CN119387828A
High-robustness binding surface micro riveting type ultrashort pulse laser welding system and method
CN120362713A
High-robustness binding surface micro riveting type ultrashort pulse laser welding system
CN224182302U