Automatic laying forming method and automatic laying forming equipment for composite material

In the automatic lay-up molding technology, the fiber yarn and the resin film are compounded and heated and compacted in the lamination mechanism. Combined with ultrasonic treatment and appropriate molding parameters, the problem of poor bonding force between fiber and resin is solved and the composite material is realized. Efficient and low-cost preparation and improvement of mechanical properties.

CN118810071AActive Publication Date: 2024-10-22上海晋飞碳纤科技股份有限公司

Patent Information

Application Number
CN202411129250.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-22
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

In the existing automatic lay-up and molding technology, the interface adhesion and affinity between the continuous fiber and the matrix resin are low, resulting in poor mechanical properties of the composite material.

Method used

By compounding the fiber yarn and the resin film, the prepreg is formed, and is heated and compacted in the lamination mechanism. The appropriate mold temperature, laying temperature, pressure roller pressure and laying speed are set to improve the relationship between the fiber and the resin. The bonding force uses ultrasonic treatment and appropriate molding parameters, combined with automatic lay-up and molding equipment, to achieve efficient and low-cost preparation of composite materials.

Benefits of technology

It significantly improves the mechanical properties of composite materials, reduces preparation costs, improves production efficiency, and reduces dependence on expensive prepreg products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118810071A_ABST
    Figure CN118810071A_ABST
Patent Text Reader

Abstract

The invention discloses an automatic laying forming method and automatic laying forming equipment of a composite material, and the method comprises the following steps: compounding fiber yarns and a resin film to obtain a prepreg; the prepreg is input into a pressing mechanism, the prepreg is heated through a heating mechanism, the temperature of a mold is set to be 20-150 DEG C, the laying temperature is set to be 130-420 DEG C, the pressure intensity of a pressing roller is set to be 1-20 MPa, the laying speed is set to be 10-500 mm / s, and composite material laying forming is conducted on the prepreg. According to the method, use of expensive materials such as prepreg tapes or prepreg filaments can be avoided, the quality of formed parts is good, and technical reference is provided for industrial production of low-cost, high-quality and high-efficiency composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite material forming, and in particular to an automatic laying and forming method and automatic laying and forming equipment for composite materials. Background Art

[0002] In recent years, the automatic placement technology of continuous fiber reinforced composite materials has attracted widespread attention, especially in the field of civil aviation, where the use of automatic placement technology to manufacture large structural components has become a trend. The quality of structural components depends largely on raw materials, processes, equipment, etc., among which raw materials, as the starting point, play a vital role in component quality.

[0003] At present, the raw materials used in automatic placement molding are prepreg tapes or prepreg filaments of continuous fiber reinforced thermoplastic or thermosetting resins. However, in the prior art, the interfacial adhesion and affinity between continuous reinforcing fibers such as glass fibers, carbon fibers, etc. and the matrix resin are very low. Therefore, there are many void defects in the interface area between the fibers and the resin, resulting in poor mechanical properties of the composite material. Summary of the invention

[0004] The purpose of the present application is to propose an automatic placement and molding method of composite materials and an automatic placement and molding device, aiming to solve the problem of poor mechanical properties of composite materials molded by traditional methods.

[0005] In a first aspect, an embodiment of the present application provides a method for laying out and molding a composite material, the method comprising:

[0006] Compounding the fiber yarn with the resin film to obtain a prepreg;

[0007] The prepreg is input into the pressing mechanism and heated by the heating mechanism. The mold temperature is set to 20-150°C, the laying temperature is set to 130-420°C, the pressure of the pressure roller is set to 1-20MPa, and the laying speed is set to 10-500mm / s to lay and form the prepreg into a composite material.

[0008] Preferably, the step of compounding the fiber yarn with the resin film to obtain the prepreg comprises:

[0009] The yarn reel of the continuous fiber material is fixed on the yarn rack mechanism, and the yarns of the yarn reel are respectively passed through the yarn collecting mechanism at the same level, and then passed through the yarn spreading mechanism to obtain a fiber thin layer;

[0010] The upper resin film and the lower resin film are transported, and are compounded with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain a prepreg.

[0011] Preferably, in the step of fixing the yarn reel of continuous fiber material on the creel mechanism:

[0012] The continuous fiber material is at least one of carbon fiber, glass fiber, aramid fiber, polyimide fiber, boron fiber, ultra-high molecular weight polyethylene fiber, polypropylene fiber, polyamide fiber, hemp fiber, alumina fiber, and silicon carbide fiber;

[0013] The thickness of the fiber thin layer is 0.01-0.5 mm.

[0014] Preferably, in the step of conveying the upper resin film and the lower resin film and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain the prepreg:

[0015] The upper resin film and the lower resin film are both thermoplastic resin films or thermosetting resin films. The thermoplastic resin film is one of polyethylene, polypropylene, polyamide, polycarbonate, thermoplastic polyurethane, thermoplastic polyimide, polyphenylene sulfide, and polyaryletherketone. The weight of the thermoplastic resin film is 9 to 70 g / m 2 ;

[0016] Preferably, in the step of conveying the upper resin film and the lower resin film and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain the prepreg:

[0017] The thermosetting resin film is one of epoxy resin, phenolic resin, bismaleimide resin, benzoxazine resin, polyurethane resin and polyimide resin, and the weight of the thermosetting resin film is 10-65 g / m 2 .

[0018] Preferably, in the step of conveying the upper resin film and the lower resin film and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain the prepreg:

[0019] The temperature of the dipping mechanism is 70-450°C, the pressure of the dipping mechanism is 1-20MPa, and the gap of the dipping mechanism is 0.05-0.3mm;

[0020] The resin content in the prepreg is 20wt% to 50wt%.

[0021] Preferably, the step of conveying the upper resin film and the lower resin film and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer in the impregnation mechanism to obtain the prepreg further includes:

[0022] During the prepreg process, the bonding area between the resin film and the fiber thin layer is subjected to ultrasonic treatment at a frequency of 5 to 40 KHz.

[0023] Preferably, in the step of inputting the prepreg into the pressing mechanism and heating the prepreg by a heating mechanism:

[0024] The heating mechanism is any one of a hot air heater, an infrared heater, and a laser heater, and the heating temperature of the heating mechanism is 70 to 450°C.

[0025] In summary, this application proposes a composite material placement and molding method, and adapts the designed automatic placement and molding equipment to achieve efficient and low-cost preparation of composite materials while ensuring the excellent mechanical properties of the composite materials.

[0026] In a second aspect, an embodiment of the present application further provides an automatic placement and molding device for realizing the above-mentioned placement and molding method of composite materials, which includes a creel mechanism, a wire collecting mechanism, a yarn spreading mechanism, a prepreg mechanism, and a pressing mechanism;

[0027] The creel mechanism is used to place the yarn roll, the yarn spreading mechanism includes a support and a yarn spreading roller arranged on the support, the prepreg mechanism includes a film placing roller and a dip roller located on the upper and lower sides of the yarn, and the film placing roller is used to place the resin film roll;

[0028] The yarns in at least two of the yarn rolls are transported to the wire collecting mechanism via the yarn frame mechanism, and are transported to the yarn spreading mechanism along the same horizontal plane. The two resin film rolls are respectively transported to the two sides of the unfolded yarn via the film placing rollers, and are pre-impregnated together via the two dipping rollers. The pressing mechanism is used to press the prepreg.

[0029] Preferably, it also includes a heating mechanism, an ultrasonic mechanism and a prepreg trimming mechanism, wherein the heating mechanism is used to heat the prepreg during pressing, the ultrasonic mechanism is used to ultrasonically treat the yarn and resin film during the prepreg process, and the prepreg trimming mechanism is used to cut off excess resin on both sides of the prepreg.

[0030] In summary, the new automatic placement and molding equipment proposed in this application can realize the rapid prepreg of resin film and continuous fiber, and directly input the obtained prepreg into the pressing mechanism of the placement equipment, thereby realizing the molding and preparation of composite materials. There is no need to purchase expensive prepreg products. Composite materials can be efficiently prepared by low-cost raw materials resin film and continuous fiber, which greatly reduces the preparation cost of composite materials and improves the preparation efficiency of composite materials.

[0031] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become apparent from the following description, or will be understood through the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram showing a process of a composite material placement and molding method according to an embodiment of the present application is shown;

[0033] Figure 2 A detailed diagram of step S101 in an embodiment of the present application is shown;

[0034] Figure 3 A flow chart of automatic composite material placement and molding according to an embodiment of the present application is shown;

[0035] Figure 4 A schematic structural diagram of an automatic placement and forming device according to an embodiment of the present application is shown.

[0036] Explanation of symbols: 11-fixed plate, 12-yarn shaft, 2-yarn, 3-yarn collecting mechanism, 41-support, 42-yarn spreading roller, 51-upper film roller, 52-lower film roller, 53-upper glue dipping roller, 54-lower glue dipping roller, 55-upper PE film collecting roller, 56-lower PE film collecting roller, 6-ultrasonic mechanism, 8-pressing mechanism, 9-resin film, 7-edge cutting mechanism, 10-heating mechanism. DETAILED DESCRIPTION

[0037] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Several embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0039] In this document, unless otherwise specified, the term "°C" means "degrees Celsius"; the term "MPa" means: megapascal; the term "mm / s" means: millimeter per second; the term "mm" means: millimeter; the term "g / m 2 " means: grams per square meter; the term "wt%" means: mass percentage; the term "KHz" means: kilohertz.

[0040] In this article, all defined ranges are meant to include each specific range within a given range and a combination of sub-ranges between given ranges. For example, a range of 1 to 5 specifically includes 1, 2, 3, 4 and 5, and also includes sub-ranges such as 2 to 5, 3 to 5, 2 to 3, 2 to 4, 1 to 4, etc.

[0041] <First aspect>

[0042] like Figure 1 As shown, the first aspect of the embodiment of the present application provides a method for laying and molding a composite material, comprising the following steps S101-S102:

[0043] S101: Compounding the fiber yarn and the resin film to obtain a prepreg;

[0044] S102: input the prepreg into the pressing mechanism, and heat the prepreg by the heating mechanism, set the mold temperature to 20-150°C, the laying temperature to 130-420°C, the pressure of the pressure roller to 1-20MPa, and the laying speed to 10-500mm / s, so as to lay and shape the prepreg into a composite material.

[0045] In some embodiments, the heating mechanism is any one of a hot air heater, an infrared heater, and a laser heater. The heating temperature of the heating mechanism is 70 to 450°C. The prepreg effect of the prepreg is maintained by setting the heating mechanism. Exemplarily, the heating temperature of the heating mechanism can be 70°C, 165°C, 260°C, 355°C, 450°C, and the like.

[0046] In some embodiments, in order to improve the interlayer adhesion of the composite material during the molding process and reduce the gap between the continuous fiber and the resin in the bonding area, the present application sets molding parameters such as mold temperature, laying temperature, pressure roller pressure and laying speed. The mold temperature refers to the temperature of the mold or base plate used for prepreg laying, the laying temperature refers to the temperature set by the heater, and the laying speed refers to the moving speed of the laying head, that is, the feeding speed (conveyance speed) of the yarn and resin film. For example, the mold temperature can be 20°C, 85°C, or 170°C. If the mold temperature is too low, it will cause the first layer of prepreg to be difficult to bond to the mold. If the mold temperature is too high, the first layer of prepreg may be Risk of thermal degradation; the laying temperature can be 130℃, 215℃, 300℃, 400℃, etc. If the laying temperature is too low, the prepreg will be difficult to cure or consolidate, and there will be serious interlayer bonding problems. If it is too high, the thermosetting prepreg will cure prematurely and lose its adhesion, or the thermoplastic prepreg will undergo thermal degradation. The roller pressure can be 1MPa, 10MPa, 20MPa, etc. If it is too low, the prepreg layers will be difficult to bond with each other, and if it is too high, glue overflow and fiber breakage will occur. The laying speed can be 10mm / s, 100mm / s, 200mm / s, 300mm / s, 400mm / s, 500mm / s. If it is too low, the production efficiency will be low, and if it is too high, the product quality will be unstable.

[0047] like Figure 2 As shown, in some embodiments, step S101 further includes:

[0048] Step S1011: fixing a plurality of yarn reels of continuous fiber material on a yarn rack mechanism, and allowing the yarns of the plurality of yarn reels to pass through a yarn collecting mechanism at the same level, and then pass through a yarn spreading mechanism to obtain a fiber thin layer;

[0049] Step S1012: conveying the upper resin film and the lower resin film, and making the upper resin film and the lower resin film pre-impregnated with the upper surface and the lower surface of the fiber thin layer at the pre-impregnation mechanism, respectively, to obtain pre-impregnated material.

[0050] In some embodiments, the continuous fiber material is at least one of carbon fiber, glass fiber, aramid, polyimide fiber, boron fiber, ultra-high molecular weight polyethylene fiber, polypropylene fiber, polyamide fiber, hemp fiber, aluminum oxide fiber, and silicon carbide fiber. Exemplarily, the continuous fiber may be one of carbon fiber, glass fiber, aramid, polyimide fiber, boron fiber, ultra-high molecular weight polyethylene fiber, polypropylene fiber, polyamide fiber, hemp fiber, aluminum oxide fiber, and silicon carbide fiber, or it may be a combination of two or more fiber materials.

[0051] In some embodiments, the thickness of the obtained fiber thin layer is 0.01-0.5 mm. For example, the thickness of the fiber thin layer can be 0.01 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, etc.

[0052] In some embodiments, the upper resin film and the lower resin film are both resin films, and are both thermoplastic resin films or thermosetting resin films. For the thermoplastic resin film, it is at least one of polyethylene, polypropylene, polyamide, polycarbonate, thermoplastic polyurethane, thermoplastic polyimide, polyphenylene sulfide, and polyaryletherketone. The weight of the thermoplastic resin film is 9 to 70 g / m 2 In some embodiments, the weight of the thermoplastic resin film may be 9 g / m 2 , 10g / m 2 , 40g / m 2 , 70g / m 2 For the thermosetting resin film, it is one of unsaturated polyester resin, epoxy resin, phenolic resin, bismaleimide resin, benzoxazine resin, polyurethane resin, and polyimide resin, and the weight of the thermosetting resin film is 10 to 70 g / m 2 For example, the weight of the thermosetting resin film may be 10 g / m 2 , 20g / m 2 42.5g / m 2 , 65g / m 2 , 70g / m 2 etc.

[0053] In some embodiments, the temperature of the dipping mechanism is 70-450°C, the pressure of the dipping mechanism is 1-20MPa, and the gap of the dipping mechanism is 0.05-0.3mm. If the temperature of the dipping mechanism is too high, the resin will solidify, and if it is too low, the resin will not be well impregnated due to poor fluidity. For example, the temperature of the dipping mechanism can be 70°C, 165°C, 260°C, 355°C, 450°C, etc.; if the pressure of the dipping mechanism is too high, the fiber will be broken, and if it is too low, it will be difficult to fully impregnate the fiber with the resin. For example, the pressure of the dipping mechanism can be 1MPa, 10MPa, 20MPa, etc.; the gap of the dipping mechanism is 0.05-0. 3mm, there is a reasonable range for the gap of the dipping mechanism. Too high or too low will cause the resin content in the prepreg to deviate from the design value, affecting the subsequent laying process and product performance. For example, the gap of the dipping mechanism can be 0.05mm, 0.1mm, 0.2mm, 0.3mm, etc.; the resin content in the prepreg is 20wt% to 50wt%. If the resin content in the prepreg is too low, the adhesion between the prepreg layers will deteriorate, and the composite product will be prone to glue-poor defects. If it is too high, the prepreg will overflow during the laying process and be difficult to lay. For example, the resin content in the prepreg can be 20wt%, 30wt%, 40wt%, 50wt%, etc.

[0054] The present application proposes a method for laying and molding composite materials, and adapts the designed automatic laying and molding equipment to achieve efficient and low-cost preparation of composite materials while ensuring excellent mechanical properties of the composite materials.

[0055] <Second Aspect>

[0056] like Figure 3 and Figure 4 As shown, the second aspect of the embodiment of the present application provides an automatic placement and forming device, which includes a creel mechanism, a wire collecting mechanism, a yarn spreading mechanism, an impregnation mechanism and a pressing mechanism, wherein:

[0057] The yarn rack mechanism includes a fixed plate 11 and a plurality of yarn shafts 12 arranged on the fixed plate 11, the yarn shafts 12 are used to place the yarn rolls, the yarn unwinding mechanism includes a support member 41 and a plurality of yarn unwinding rollers 42 arranged on the support member 41, the prepreg mechanism includes an upper film-laying roller 51, a lower film-laying roller 52, an upper dipping roller 53 and a lower dipping roller 54, and an upper PE film-collecting roller 55 and a lower PE film-collecting roller 56 located on the upper and lower sides of the yarn, the upper film-laying roller 51 and the lower film-laying roller 52 are both used to place the resin film roll, the upper PE film-collecting roller 55 and the lower PE film-collecting roller 56 are both used to collect the PE film on the surface of the resin film roll, and the yarn 2 in the yarn roll is transported to the wire collecting mechanism 3 through the yarn rack mechanism. , and transported to the yarn spreading mechanism along the same horizontal plane, the two resin film rolls are respectively transported to the two sides of the unfolded yarn 2 through the film release roller, and are compounded together through two dipping rollers, and the pressing mechanism 8 is used to press the prepreg. In this embodiment, the wire collecting mechanism 3 is a wire collecting plate with multiple through holes, and the yarns 2 on the four yarn shafts 12 pass through the through holes in the wire collecting plate respectively. The pressing mechanism 8 is a laying roller. The yarns 2 on the same horizontal plane are spread together after passing through multiple yarn spreading rollers 42 in sequence, and then compounded with the resin films 9 on both sides to obtain prepreg, and then the prepreg is pressed and formed by laying rollers to obtain a composite material.

[0058] In some embodiments, the automatic placement molding equipment further includes an ultrasonic mechanism 6, a trimming mechanism 7, and a heating mechanism 10. The ultrasonic mechanism 6 is an ultrasonic device for ultrasonically treating the yarn 2 and the resin film 9 during the prepreg process. The trimming mechanism 7 is used to cut off the excess resin on both sides of the prepreg. The heating mechanism 10 is a heater for heating the prepreg during the pressing process.

[0059] In summary, the new automatic placement and molding equipment proposed in the embodiment of the present application can realize the rapid prepreg of resin film and continuous fiber, and directly input the obtained prepreg into the pressing mechanism of the placement equipment, thereby realizing the direct molding of composite materials. There is no need to purchase expensive prepreg products. Composite materials can be efficiently prepared through low-cost raw material resin film and continuous limiting, which greatly reduces the preparation cost of composite materials and improves the preparation efficiency of composite materials.

[0060] Example 1

[0061] The carbon fiber (T700-12K, provided by Toray) yarn is fixed on the yarn shaft, passed through the yarn collecting plate, and then spread by the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.05mm. The temperature of the dip roller is kept at 90℃, the pressure is 10MPa, the gap between the dip roller and the platform is 0.08mm, and the weight of 20g / m 2The epoxy resin film is unwound to be pre-impregnated with the above-mentioned thin layer of fiber at the dipping roller. During the pre-impregnation, the ultrasonic frequency is 10KHz. The pre-impregnated prepreg is transported to the pressing mechanism (feeding system) of the laying equipment, and the sheet is heated by a laser heater. The mold temperature is 30°C, the laying temperature is 150°C, the pressure of the pressure roller is 2MPa, and the composite material is laid and formed at a laying speed of 100mm / s. The laid composite material is placed in an autoclave for vacuum curing. After curing at "140°C, 2h", the curing degree of the carbon fiber reinforced epoxy composite material reaches 99%.

[0062] Example 2

[0063] The ultra-high molecular weight polyethylene fiber (SFG 1600, provided by Changshu Xiupo Company) was fixed on the yarn shaft, passed through the yarn collecting plate, and then spread by the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.1mm. The temperature of the dip roller was kept at 90℃, the pressure was 5MPa, the gap between the dip roller and the platform was 0.15mm, and the weight of 30g / m 2 The epoxy resin film is unwound to be pre-impregnated with the above-mentioned thin layer of fiber at the dipping roller. During pre-impregnation, the ultrasonic frequency is 20KHz. The pre-impregnated material is transported to the feeding system of the laying equipment, and the sheet is heated by a laser heater. The mold temperature is 30°C, the laying temperature is 150°C, the pressure of the pressure roller is 5MPa, and the composite material is laid and formed at a laying speed of 200mm / s. The laid composite material is placed in an autoclave for vacuum curing. After curing at "140°C, 2h", the curing degree of the ultra-high molecular weight polyethylene fiber reinforced epoxy composite material reaches 99%.

[0064] Example 3

[0065] The ultra-high molecular weight polyethylene fiber (SFG 1600, provided by Changshu Xiupo Company) was fixed on the yarn shaft, passed through the yarn collecting plate, and then spread by the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.1mm. The temperature of the dip roller was kept at 130℃, the pressure was 20MPa, the gap between the dip roller and the platform was 0.15mm, and the weight of 30g / m 2 The low-density polyethylene resin film is unwound and pre-impregnated with the thin layer of fiber at the dipping roller. During pre-impregnation, the ultrasonic frequency is 10KHz. The pre-impregnated material is transported to the feeding system of the laying equipment, and the sheet is heated by an infrared heater. The mold temperature is 50°C, the laying temperature is 130°C, the pressure of the pressure roller is 5MPa, and the polyethylene self-reinforced composite material is laid and formed at a laying speed of 400mm / s.

[0066] Example 4

[0067] The glass fiber (ER550-1080, provided by Chongqing International Composite Materials Co., Ltd.) was fixed on the yarn shaft, passed through the yarn collecting plate, and then spread through the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.25 mm. The temperature of the dip roller was kept at 90 ° C, the pressure was 20 MPa, the gap between the dip roller and the platform was 0.05 mm, and the weight of 10 g / m 2 The epoxy resin film is unwound to be pre-impregnated with the above-mentioned thin layer of fiber at the dipping roller. During pre-impregnation, the ultrasonic frequency is 5KHz. The pre-impregnated material is transported to the feeding system of the laying equipment, and the sheet is heated by a laser heater. The mold temperature is 20°C, the laying temperature is 160°C, the pressure of the pressure roller is 1MPa, and the composite material is laid and formed at a laying speed of 50mm / s. The laid composite material is placed in an autoclave for vacuum curing. After curing at "140°C, 2h", the curing degree of the glass fiber reinforced epoxy composite material reaches 99%.

[0068] Example 5

[0069] The carbon fiber (T800-12K, provided by Toray) was fixed on the yarn shaft, passed through the yarn collecting plate, and then spread through the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.25 mm. The temperature of the dip roller was kept at 250°C, the pressure was 10 MPa, the gap between the dip roller and the platform was 0.15 mm, and the weight of 40 g / m 2 The bismaleimide resin film is unwound and pre-impregnated with the above-mentioned thin layer of fiber at the dipping roller. During pre-impregnation, the ultrasonic frequency is 25KHz. The pre-impregnated material is transported to the feeding system of the laying equipment, and the sheet is heated by a laser heater. The mold temperature is 85°C, the laying temperature is 240°C, the pressure of the pressure roller is 10MPa, and the composite material is laid and formed at a laying speed of 200mm / s. The laid composite material is placed in an autoclave for vacuum curing. After curing at "240°C, 4h", the curing degree of the carbon fiber reinforced bismaleimide composite material reaches 99%.

[0070] Example 6

[0071] The para-aramid fiber (Kevlar, provided by DuPont) was fixed on the yarn shaft, passed through the yarn collecting plate, and then spread through the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.25 mm. The temperature of the dip roller was kept at 220°C, the pressure was 15 MPa, the gap between the dip roller and the platform was 0.15 mm, and the weight of 40 g / m 2The polypropylene resin film is unwound and pre-impregnated with the thin layer of fiber at the dipping roller. During pre-impregnation, the ultrasonic frequency is 30KHz. The pre-impregnated material is transported to the feeding system of the laying equipment, and the sheet is heated by a hot air heater. The mold temperature is 100℃, the laying temperature is 220℃, the pressure of the pressure roller is 15MPa, and the composite material is laid and formed at a laying speed of 300mm / s.

[0072] Example 7

[0073] The carbon fiber (IM7, provided by Hershey) was fixed on the yarn shaft, passed through the yarn collecting plate, and then spread by the yarn spreading roller to obtain a thin layer of fiber with a thickness of 0.5 mm. The temperature of the dip roller was kept at 450°C, the pressure was 10 MPa, the gap between the dip roller and the platform was 0.3 mm, and the weight of 70 g / m 2 The polyetheretherketone resin film is unwound and pre-impregnated with the above-mentioned thin layer of fiber at the dipping roller. During pre-impregnation, the ultrasonic frequency is 40KHz. The pre-impregnated material is transported to the feeding system of the laying equipment, and the sheet is heated by a laser heater. The mold temperature is 150℃, the laying temperature is 420℃, the pressure of the pressure roller is 20MPa, and the composite material is laid and formed at a laying speed of 500mm / s.

[0074] Comparative Example 1

[0075] This comparative example is basically the same as Example 1, except that: in this comparative example, no ultrasonic treatment is performed during pre-impregnation, and the obtained composite material is placed in an autoclave for vacuum curing. After curing at "140° C., 2 h", the curing degree of the composite material reaches 99%.

[0076] Comparative Example 2

[0077] The carbon fiber (T700-12K, provided by Toray) placed on the fiber rack is opened by the fiber spreading device after the yarn guide roller, and enters the spray system. The spray head sprays the grafting agent (silane coupling agent, the amount is 0.2% of the continuous fiber) placed in the storage box to the surface of the carbon fiber, and then enters the preheating box for preheating. The preheated continuous fiber is compounded with the epoxy resin film in the high temperature box through the hot pressing roller, and then cooled by the cold pressing roller after leaving the high temperature box, and then trimmed by the cutting device and wound by the winding device, and the carbon fiber reinforced epoxy resin prepreg is obtained. The obtained prepreg is laid according to the 0° ply, and then placed in the autoclave for vacuum curing. After curing at "140°C, 2h", the curing degree of the composite material reaches 99%.

[0078] Result analysis:

[0079] The three-point bending strength was used to characterize the mechanical properties of the composite material. Please refer to Table 1 below, which shows the result data of the composite materials prepared in Examples 1-7 and Comparative Examples 1-2, respectively.

[0080] Table 1

[0081]

[0082] As can be seen from Table 1, the method provided by the present invention can realize the molding of composite materials reinforced by various fibers such as carbon fiber, ultra-high molecular weight polyethylene fiber, para-aramid, and glass fiber. The flexural strength of the composite materials in Example 1 and Comparative Example 1 are 1230MPa and 1095MPa respectively, which shows that the ultrasonic assisted impregnation effect proposed by the present invention is significant. At the same time, it can be seen from Comparative Example 2 that the flexural strength of the carbon fiber reinforced epoxy composite material prepared by the chemical treatment method of the graft coupling agent reaches 1200MPa, and the flexural strength of the composite material of the same level prepared by the present invention by adjusting the molding process parameters reaches 1230MPa, that is, the enhancement effect better than the surface grafting method is obtained.

[0083] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A method for laying and molding a composite material, characterized in that: The method comprises: Compounding the fiber yarn with the resin film to obtain a prepreg; The prepreg is input into the pressing mechanism and heated by the heating mechanism. The mold temperature is set to 20-150°C, the laying temperature is set to 130-420°C, the pressure of the pressure roller is set to 1-20MPa, and the laying speed is set to 10-500mm / s to lay and form the prepreg into a composite material.

2. The composite material placement molding method according to claim 1, characterized in that: The step of compounding the yarn and the resin film to obtain the prepreg comprises: Fixing a plurality of yarn reels of continuous fiber materials on a yarn rack mechanism, and allowing the yarns of the plurality of yarn reels to pass through a yarn collecting mechanism at the same level, and then pass through a yarn spreading mechanism, to obtain a fiber thin layer; The upper resin film and the lower resin film are transported, and are compounded with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain a prepreg.

3. The composite material placement molding method according to claim 2, characterized in that: In the step of fixing a plurality of yarn reels of continuous fiber material on a creel mechanism: The continuous fiber material is at least one of carbon fiber, glass fiber, aramid fiber, polyimide fiber, boron fiber, ultra-high molecular weight polyethylene fiber, polypropylene fiber, polyamide fiber, hemp fiber, alumina fiber, and silicon carbide fiber; The thickness of the fiber thin layer is 0.01-0.5 mm.

4. The composite material placement molding method according to claim 2, characterized in that: In the step of conveying the upper resin film and the lower resin film, and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain the prepreg: The upper resin film and the lower resin film are both thermoplastic resin films or thermosetting resin films; The thermoplastic resin film is one of polyethylene, polypropylene, polyamide, polycarbonate, thermoplastic polyurethane, thermoplastic polyimide, polyphenylene sulfide, and polyaryletherketone, and the weight of the thermoplastic resin film is 9 to 70 g / m 2 ; The thermosetting resin film is one of unsaturated polyester resin, epoxy resin, phenolic resin, bismaleimide resin, benzoxazine resin, polyurethane resin and polyimide resin, and the weight of the thermosetting resin film is 10-70 g / m 2 .

5. The composite material placement molding method according to claim 2, characterized in that: In the step of conveying the upper resin film and the lower resin film, and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer at the impregnation mechanism to obtain the prepreg: The temperature of the dipping mechanism is 70-450°C, the pressure of the dipping mechanism is 1-20MPa, and the gap of the dipping mechanism is 0.05-0.3mm; The resin content in the prepreg is 20wt% to 50wt%.

6. The composite material placement molding method according to claim 2, characterized in that: The step of conveying the upper resin film and the lower resin film and compounding the upper resin film and the lower resin film with the upper surface and the lower surface of the fiber thin layer in the impregnation mechanism to obtain the prepreg also includes: During the prepreg process, the bonding area between the resin film and the fiber layer is subjected to ultrasonic treatment at a frequency of 5-40 KHz.

7. The composite material placement molding method according to claim 1, characterized in that: In the step of inputting the prepreg into the pressing mechanism and heating the prepreg by the heating mechanism: The heating mechanism is any one of a hot air heater, an infrared heater, and a laser heater, and the heating temperature of the heating mechanism is 70 to 450°C.

8. An automatic placement and molding device, used to implement the placement and molding method of the composite material according to any one of claims 1 to 7, characterized in that: It includes a yarn rack mechanism, a yarn collecting mechanism, a yarn spreading mechanism, an impregnation mechanism and a pressing mechanism; The yarn rack mechanism is used to place the yarn roll, the yarn spreading mechanism includes a support and a yarn spreading roller arranged on the support, the impregnation mechanism includes a film placing roller and a dipping roller located on the upper and lower sides of the yarn, and the film placing roller is used to place the resin film roll; The yarn in the yarn roll is transported to the wire collecting mechanism via the yarn frame mechanism, and is transported to the yarn spreading mechanism along the same horizontal plane. The two resin film rolls are respectively transported to the two sides of the unfolded yarn via the film placing rollers, and are pre-impregnated together via the two dipping rollers. The pressing mechanism is used to press the prepreg.

9. The automatic placement and forming equipment according to claim 8, characterized in that: The invention also comprises a heating mechanism and an ultrasonic mechanism. The heating mechanism is used to heat the prepreg during pressing, and the ultrasonic mechanism is used to ultrasonically treat the yarn and the resin film during the prepreg process.

10. The automatic placement and forming equipment according to claim 8, characterized in that: It also includes a prepreg trimming mechanism, which is used to cut off excess resin on both sides of the prepreg.

Citation Information

Patent Citations

  • Prepreg for automatic fiber placement process and preparation method of prepreg

    CN112300534A

  • Preparation method for improving transverse strength of continuous fiber / resin-based composite material

    CN117507347A

  • Carbon fiber reinforced thermoplastic epoxy resin prepreg, composite material and recovery method thereof

    CN118027605A

  • Method for producing fiber-reinforced composite material, and prepreg

    JP2023120708A

  • Carbon fiber-reinforced resin sheet and manufacturing method therefor

    JP2024075888A

Cited By

  • Preparation method and forming device of carbon fiber spreading belt for automatic laying-liquid forming

    CN120963076A