A lightweight and low-carbon tile adhesive building material and its preparation method and application
By adding light sand, modified polyvinyl alcohol and modified cellulose ether to the ceramic tile paste, the problems of low bond strength and high water absorption are solved, and the weather resistance and permeability of ceramic tile paste paste paste paste are improved. Performance, suitable for green building materials field.
Patent Information
- Application Number
- CN202411311817.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The existing lightweight and low-carbon ceramic tiles have low bond strength, poor aging resistance and high water absorption, which leads to the unstable sticking of the ceramic tiles and is prone to fall off due to changes in temperature differences.
Add light sand coated with lightweight sand, modified polyvinyl alcohol and modified cellulose ether to the formula of ceramic tile adhesion clay to enhance the binding force between components through silane coupling agent, and modify polyvinyl alcohol and epoxy resin to improve bonding Performance, nanoclay enhances mechanical properties and optimizes construction performance with early strength agents and lubricants.
It significantly improves the bonding strength, weather resistance, impermeability and low water absorption rate of ceramic tile adhesion clay, extends its service life, and is suitable for green building materials.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of building materials, and relates to a lightweight and low-carbon tile adhesive mortar building material, a preparation method and an application thereof, and specifically to a lightweight and low-carbon tile adhesive mortar building material with high bonding strength and strong environmental resistance, a preparation method thereof and an application thereof in the preparation of green building materials. Background Art
[0002] There are many materials for pasting tiles, among which cement-based tile adhesive is the largest in usage as a tile pasting adhesive. Cement-based tile adhesive, concrete and tiles are three materials with different components. Due to their different thermal expansion coefficients, the thermal expansion and contraction of the three materials are not synchronized under different temperature changes, which leads to interfacial stress at the bonding interface. The continuous thermal expansion and contraction in the cycle of the four seasons and day and night causes a significant decrease in the bonding strength of the interface, which eventually causes the tiles to fall off. And because the temperature difference in room temperature is generally greater than that indoors, the problem of tile falling off on the exterior wall is more obvious.
[0003] In addition, in order to improve environmental protection and respond to the needs of sustainable development, lightweight and low-carbon tile adhesives have received widespread attention. In order to reduce the weight of tile adhesives, some low-quality substances are usually added during the preparation of the adhesives. Due to their large pores, they can usually also play a role in sound insulation and heat preservation, improve indoor acoustic environment and thermal comfort. However, due to the addition of these lightweight substances, the adhesives will be phase separated after being placed for a long time. This is mainly because most lightweight substances use inorganic substances and have poor interfacial compatibility with other substances. At the same time, the prepared lightweight and low-carbon tile adhesives have a high water absorption rate, resulting in low adhesive strength of the adhesive. This is mainly because most lightweight substances have a structure with more pores, which leads to the absorption of water vapor in the environment after long-term use, affecting the bonding strength of the adhesive.
[0004] Therefore, there is an urgent need for a lightweight, low-carbon tile pasting mortar building material with high bonding strength, good aging resistance and low water absorption rate. Summary of the invention
[0005] The purpose of the present application is to provide a lightweight low-carbon tile adhesive building material and a preparation method thereof and its application in the preparation of green building materials, so as to solve the problems of low bonding strength, poor aging resistance and high water absorption of the above-mentioned lightweight low-carbon tile adhesive. The three substances of coated lightweight sand, modified polyvinyl alcohol and modified cellulose ether added in the formula of the present application have a synergistic effect, which improves the weather resistance, cold and hot alternation resistance, impermeability and bonding strength of the lightweight low-carbon tile adhesive. The comprehensive performance of the tile adhesive is improved and can be applied to the field of green building materials.
[0006] The present application provides a lightweight and low-carbon tile adhesive building material, which includes the following raw materials in parts by weight:
[0007] Coated light sand 15~40 parts
[0008] 15~30 parts of cement
[0009] Modified polyvinyl alcohol 5~10 parts
[0010] Modified cellulose ether 2~5 parts
[0011] Redispersible latex powder 3~25 parts
[0012] Density regulator 10~20 parts
[0013] Early strength agent 0.1~1 part
[0014] Lubricant 0.05~0.5 parts
[0015] 10-20 parts water;
[0016] The modified polyvinyl alcohol comprises polyvinyl alcohol and epoxy resin, and the mass ratio of polyvinyl alcohol to epoxy resin is 8-10:2-5;
[0017] The modified cellulose ether includes nano clay and cellulose ether, and the mass ratio of the nano clay to the cellulose ether is 1-3:10-15.
[0018] As a relatively new material, lightweight and low-carbon tile adhesive has some advantages, such as light weight, low carbon and environmental protection. However, the performance of lightweight and low-carbon tile adhesive after use still has some disadvantages, such as low bonding strength and poor weather resistance. Therefore, this application addresses the above-mentioned problems of tile adhesive and redesigns the formula of tile adhesive to improve its weather resistance and bonding strength.
[0019] The formula in this application contains coated light sand, cement, modified polyvinyl alcohol, modified cellulose ether, redispersible latex powder, density regulator, early strength agent, lubricant and water, wherein the coated light sand provides light properties, improves the density of the overall material, and enhances the bonding force with other components through silane coupling agent; cement, as the main cementitious material, gives the adhesive glue sufficient bonding strength and stability after hardening; modified polyvinyl alcohol improves bonding performance, increases the flexibility and crack resistance of the adhesive glue, and the combination of polyvinyl alcohol and epoxy resin can further improve bonding strength and durability; modified cellulose ether improves water retention, improves construction performance, and improves the mechanical properties and water resistance of the material through the addition of nanoclay; density regulator is used to reduce the overall density of the adhesive glue while maintaining good physical properties; early strength agent accelerates the hydration process of cement, so that the adhesive glue can reach the initial strength faster and shorten the construction period. Lubricant improves the smearing performance during construction, makes the adhesive glue easier to spread, and reduces the occurrence of shrinkage cracks. These components of this application cooperate with each other, not only improving the performance of the adhesive glue, but also making it more environmentally friendly and sustainable. Such lightweight and low-carbon tile adhesive is very suitable for use in the field of green building materials.
[0020] The present application also continues to limit the mass ratio of the composition in the coated lightweight sand, the molecular weight of polyvinyl alcohol, the type of epoxy resin, the type of cellulose ether, the type of dispersible latex powder, etc., to further improve the weather resistance, resistance to alternating cold and heat, impermeability, low absorption rate and bonding strength of the tile adhesive.
[0021] In some embodiments of the present application, the coated lightweight sand includes a silane coupling agent and a lightweight sand composition, the mass ratio of the silane coupling agent to the lightweight sand composition is 1~5:100~300, the lightweight sand composition includes lightweight sand aggregate, fly ash and pumice, and the mass ratio of the lightweight sand aggregate, fly ash and pumice is 1~1.5:0.1~0.3:0.2~0.4.
[0022] In some embodiments of the present application, the particle size of the lightweight sand aggregate is 0.1-0.3 mm, the particle size of the fly ash is 1-5 μm, and the particle size of the pumice is 10-20 μm.
[0023] The role of the coated light sand in the light low-carbon tile adhesive of the present application is mainly to provide good bonding performance, while ensuring that the material has a lower density and better weather resistance, resistance to alternating cold and heat, impermeability, low water absorption and bonding strength. Among them, the silane coupling agent can form an organic-inorganic composite layer on the surface of the light sand to enhance the interfacial bonding between the light sand and the cement paste. The silane coupling agent can also improve the water resistance and chemical corrosion resistance of the material, thereby improving its weather resistance; at the same time, because it can improve the bonding strength between the interfaces, it also helps to improve the ability of the material to resist stress cracking caused by temperature changes. Among them, the light sand aggregate, fly ash and pumice are all lightweight materials, and their use can significantly reduce the density of the final product and reduce the structural load. The porosity of the light sand composition is relatively high, but after being treated with the silane coupling agent, its pore surface is partially closed, reducing the channel for water penetration, thereby improving the impermeability. Similarly, due to the closure of the pore surface, the water absorption rate of the light sand composition will also be reduced, which helps to improve the long-term durability of the material.
[0024] The application sets a reasonable ratio between lightweight sand aggregate, fly ash and pumice to form a relatively stable skeleton structure, which helps to improve the overall bonding strength. Among them, the lightweight sand aggregate provides lightweight characteristics and is the main filling material for adhesive mortar. Fly ash, as an active filler, can undergo secondary hydration reaction with cement to further improve the bonding strength and durability. Pumice, as a natural lightweight filler, helps to reduce the density of the material while providing a certain mechanical strength.
[0025] Therefore, the use of coated light sand in this application can not only significantly reduce the density of light low-carbon tile adhesive, but also improve its bonding performance, weather resistance, cold and hot alternation resistance, impermeability and reduce water absorption through the treatment of silane coupling agent. This improved material can better adapt to various environmental conditions in practical applications and extend its service life.
[0026] The present application has limitations on the mass ratio between the silane coupling agent and the light sand composition and the ratio between the light sand aggregate, fly ash and pumice. If the ratio of the silane coupling agent is too low, the surface of the light sand may not be fully covered, resulting in insufficient bonding strength between the light sand and the cement paste, thereby affecting the overall bonding performance. If the ratio of the silane coupling agent is too high, overreaction or waste may occur, which not only increases the cost, but also may affect other properties of the material, such as increasing water absorption and reducing impermeability. If the ratio of light sand aggregate is too low, the density of the overall material may increase, the light characteristics may be lost, and the impermeability and cold and hot alternation resistance of the material may also be affected. If the ratio of fly ash is too low, the possibility of secondary hydration reaction with cement is reduced, resulting in lower bonding strength and durability. If the ratio of pumice is too low, pumice, as a lightweight filler, helps to reduce the density of the material and provide a certain mechanical strength. If its ratio is too low, these effects may not be fully exerted. If the ratio of any one component is too high, the ratio of other components may be relatively reduced, thereby affecting the overall performance. For example, too much lightweight sand aggregate may lead to reduced bonding strength, and too much fly ash or pumice may affect the fluidity and construction performance of the material. Therefore, the present application needs to define the mass ratio of the silane coupling agent and the lightweight sand composition, as well as the mass ratio of the lightweight sand aggregate, fly ash and pumice.
[0027] In some embodiments of the present application, the molecular weight of the polyvinyl alcohol is 170,000 to 220,000, and the epoxy resin is bisphenol A epoxy resin.
[0028] The molecular weight of polyvinyl alcohol is limited in this application. The molecular weight of polyvinyl alcohol is relatively high. High molecular weight PVA (170,000 to 220,000) usually has better film-forming and bonding properties, which can effectively improve the bonding strength of tile adhesive. High molecular weight PVA has better weather resistance and can enhance the material's ability to resist environmental factors such as ultraviolet rays and temperature changes. The high molecular weight of PVA helps to form a dense film structure and reduce the chance of water penetration. The high molecular weight of PVA can reduce the porosity of the material and reduce water absorption, thereby improving durability.
[0029] If the molecular weight of the polyvinyl alcohol in this application is too low, the low molecular weight PVA may lead to poor film-forming properties, reduced bonding strength, and weakened weather resistance. If the molecular weight of PVA is too high, although a high molecular weight generally means better performance, if the molecular weight is too high, it may cause the solubility of PVA in water to decrease, affecting its uniform distribution in the formula, and thus affecting the bonding performance.
[0030] The type of epoxy resin is limited in this application. The epoxy resin is bisphenol A epoxy resin. Bisphenol A epoxy resin has excellent bonding properties due to its high cross-linking density, which can improve the bonding strength of tile adhesive. Bisphenol A epoxy resin has good weather resistance and can improve the durability of materials under harsh environmental conditions. The cross-linked network formed by epoxy resin can improve the density of the material and reduce moisture penetration. Epoxy resin can reduce the porosity inside the material, thereby reducing water absorption.
[0031] If the epoxy resin type in this application is changed, different epoxy resin types have different chemical properties and performance characteristics. For example, some epoxy resins may not have as high crosslink density and weather resistance as bisphenol A epoxy resin, which may result in reduced bonding strength, reduced weather resistance, and poor impermeability and low water absorption properties of the tile adhesive.
[0032] In some embodiments of the present application, the cellulose ether is one or more of carboxymethyl cellulose ether, hydroxypropyl methyl cellulose ether, and hydroxyethyl cellulose ether.
[0033] In some embodiments of the present application, the redispersible latex powder is one or more of vinyl acetate-ethylene copolymer, vinyl acetate-ethylene-vinyl ester polymer, styrene-acrylate copolymer, vinyl acetate-vinyl ester-acrylic acid-ethylene copolymer, and vinyl chloride-ethylene-vinyl laurate copolymer.
[0034] In some embodiments of the present application, the density regulator is one or more of vitrified microspheres, expanded vermiculite, expanded perlite, sepiolite, walnut shells, and volcanic rock particles.
[0035] In some embodiments of the present application, the early strength agent is one or more of calcium formate, calcium chloride and sodium sulfate.
[0036] In some embodiments of the present application, the lubricant is one or more of bentonite, methyl cellulose and polyacrylamide.
[0037] The present application provides a method for preparing a lightweight and low-carbon tile adhesive mortar building material, comprising the following steps:
[0038] (1) Preparation of coated lightweight sand
[0039] The lightweight sand aggregate, fly ash and pumice are mixed in proportion to obtain a lightweight sand composition;
[0040] Add the silane coupling agent to ethanol and mix well to obtain a 0.05-0.1% coating solution;
[0041] The coating solution is uniformly sprayed on the light sand composition, and stirred at room temperature for 20 to 30 minutes using a stirrer to obtain a mixture;
[0042] The mixture is transferred to an oven and dried at 100-120°C to obtain coated light sand;
[0043] (2) Preparation of modified polyvinyl alcohol
[0044] Add polyvinyl alcohol to water, heat and stir at 55-65°C for 2-4 hours until the polyvinyl alcohol is completely dissolved to obtain a polyvinyl alcohol solution with a mass percentage of 5-10%;
[0045] Add epoxy resin to the polyvinyl alcohol solution, heat and stir at 70-80°C for 2-5 hours, and after the reaction is completed, filter, wash and dry to obtain modified polyvinyl alcohol;
[0046] (3) Preparation of modified cellulose ether
[0047] The nanoclay is added to an aqueous solution of hexadecyltrimethylammonium bromide with a concentration of 0.1-0.2 M, and ultrasonically stirred for 30-40 minutes to obtain a nanoclay dispersion with a mass percentage of 1-5%.
[0048] Add cellulose ether into water, heat and stir at 60-80°C for 3-5 hours until the cellulose ether is completely dissolved to obtain a cellulose ether solution with a mass percentage of 5-8%;
[0049] Slowly pour the nanoclay dispersion into the cellulose ether solution, heat and stir at 60-100°C for 4-6 hours, and after the reaction is completed, centrifuge, wash, and dry to obtain the modified cellulose ether;
[0050] (4) Preparation of tile adhesive
[0051] The coated light sand, cement, modified polyvinyl alcohol, modified cellulose ether, redispersible latex powder, density regulator, early strength agent, lubricant and water are uniformly mixed in proportion to obtain a light and low-carbon tile adhesive mortar building material.
[0052] In the preparation process, the present application first synthesizes coated light sand, modified polyvinyl alcohol, and modified cellulose ether. The three are used in light and low-carbon tile adhesive mortar to have a synergistic effect, jointly improve the bonding strength, environmental resistance, and reduce the absorption rate of the tile adhesive mortar, so that the comprehensive performance of the tile adhesive mortar is improved. Among them, the weather resistance of the modified PVA, the water retention of the modified cellulose ether, and the low water absorption rate of the coated light sand work together to improve the overall weather resistance of the material. The modified PVA and the modified cellulose ether jointly improve the flexibility and crack resistance of the material, while the low density characteristics of the coated light sand help to reduce the stress caused by temperature changes, and jointly improve the resistance to alternating cold and heat. The dense structure formed by the modified PVA and the modified cellulose ether is combined with the low water absorption rate of the coated light sand, which reduces the chance of water penetration and improves the anti-seepage performance. The use of modified PVA and modified cellulose ether reduces the porosity inside the material, and the low water absorption rate characteristics of the coated light sand further reduce the overall water absorption rate. The modified PVA is combined with the coated lightweight sand through the treatment of silane coupling agent to improve the bonding strength of the material, while the use of modified cellulose ether further improves the cohesion and stability of the material.
[0053] The present application uses epoxy resin to modify polyvinyl alcohol. Epoxy resin can cross-link with the hydroxyl groups on the PVA molecular chain to form a more stable three-dimensional network structure, which helps to improve the cohesion and interfacial bonding properties of the tile adhesive. In addition, the epoxy resin-modified PVA can better chemically bond with the surface of the substrate, thereby enhancing the bonding strength. The epoxy resin-modified PVA has higher chemical stability, can reduce the aging phenomenon caused by environmental factors (such as ultraviolet rays and humidity changes), and the modified PVA can better resist the erosion of chemical substances and improve the durability of the material. The epoxy resin-modified PVA helps to form a more compact structure, reduces the path of water penetration, and improves the anti-seepage performance. The epoxy resin itself has good waterproof performance, and the modified PVA can better exert this characteristic. The epoxy resin-modified PVA helps to reduce the pores inside the material and reduce the possibility of water absorption. The compact structure formed by the modified PVA can effectively block the intrusion of water and reduce the water absorption rate. Epoxy resin modified PVA has higher thermal stability and can better resist changes in physical properties caused by temperature changes. The modified PVA can reduce stress concentration caused by temperature changes and reduce the risk of cracking.
[0054] The present application uses nanoclay to modify cellulose ether. The small size effect of nanoclay enables it to fill the tiny gaps in the cellulose ether solution, improve the density of the material, and enhance the interfacial bonding performance. The addition of nanoclay can also increase the cohesion of the material, thereby improving the overall bonding strength. The addition of nanoclay can improve the chemical stability of the material, reduce the aging phenomenon caused by environmental factors (such as ultraviolet rays and humidity changes), and nanoclay can also improve the corrosion resistance of the material, especially when exposed to an environment containing chemical substances. The composite material formed by the interaction of nanoclay and cellulose ether can form a denser structure, reduce the path of water penetration, and improve the anti-permeability performance. The addition of nanoclay can enhance the waterproof performance of the material and reduce the absorption of water. The addition of nanoclay can improve the thermal stability of the material, so that it can better resist the changes in physical properties caused by temperature changes. The presence of nanoclay can reduce the stress concentration caused by temperature changes. Through the combination of nanoclay and cellulose ether, a more stable network structure can be formed, thereby improving the crack resistance and durability of the material and reducing the risk of cracking.
[0055] The present application provides an application of a lightweight low-carbon tile adhesive mortar building material and an application of a lightweight low-carbon tile adhesive mortar in the preparation of green building materials.
[0056] The green building materials in this application are not limited to lightweight and low-carbon tiles pasted with adhesive putty, but also include wall materials such as green wall materials pasted with adhesive putty, interior decoration materials such as fiber-reinforced gypsum boards, and building insulation materials and high-performance concrete with good fireproof and heat-insulating properties.
[0057] Compared with the prior art, the present application at least achieves the following technical effects:
[0058] The present application relates to a lightweight and low-carbon tile adhesive building material and a preparation method and application thereof, which can not only maintain the lightweight property of the tile adhesive, but also improve the bonding strength and environmental resistance of the tile adhesive, and reduce the water absorption rate, and specifically obtain at least the following technical effects:
[0059] (1) In this application, the bonding performance of the mortar is improved by compounding polyvinyl alcohol and epoxy resin. The synergistic effect of epoxy resin and polyvinyl alcohol makes the modified polyvinyl alcohol have better bonding strength, especially the bonding ability to different material surfaces. The addition of epoxy resin also improves the temperature resistance of the mortar, so that the mortar can still maintain good bonding performance in a hot and cold alternating environment, while improving the waterproof performance of the mortar and reducing the water absorption rate.
[0060] (2) The introduction of nanoclay in the present application enhances the dispersibility and stability of cellulose ether, improves the bonding strength and cohesion of the cement, and the presence of nanoclay increases the thermal stability of the cement, which helps to resist damage caused by temperature changes. The addition of nanoclay enhances the aging resistance of cellulose ether and increases the service life of the cement.
[0061] (3) In the present application, the coating of lightweight sand with silane coupling agent enhances the interfacial bonding force between lightweight sand and other components and improves the overall bonding performance. The use of lightweight sand reduces the overall thermal conductivity of the mortar, reduces the stress caused by temperature difference, and improves the ability to resist alternating cold and hot conditions. Lightweight sand itself has the characteristic of low water absorption, and the coating with silane coupling agent further improves the waterproof performance of lightweight sand.
[0062] (4) The lightweight and low-carbon tile adhesive mortar building material of the present application has achieved significant improvements in bonding strength, resistance to alternating cold and heat, resistance to aging, resistance to penetration and low water absorption through a variety of modification technologies and optimization of ingredients. DETAILED DESCRIPTION
[0063] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below. However, it should be understood that the description here is only used to explain the present application and is not used to limit the scope of the present application.
[0064] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present application, and the terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The reagents and instruments used herein are all commercially available, and the characterization means involved can refer to the relevant descriptions in the prior art, which will not be repeated herein.
[0065] Example 1
[0066] A method for preparing a lightweight and low-carbon tile adhesive building material comprises the following steps:
[0067] (1) Preparation of coated lightweight sand
[0068] Lightweight sand aggregate, fly ash and pumice are mixed in proportion to obtain a lightweight sand composition, wherein the mass ratio of lightweight sand aggregate, fly ash and pumice is 1.2:0.2:0.3; the particle size of the lightweight sand aggregate is 0.2 mm, the particle size of the fly ash is 3 μm, and the particle size of the pumice is 15 μm;
[0069] The silane coupling agent is added to ethanol, the mass ratio of the silane coupling agent to the light sand composition is 3:200, and the mixture is evenly mixed to obtain a 0.08% coating solution; the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane;
[0070] The coating solution is uniformly sprayed on the light sand composition, and stirred at room temperature for 25 minutes using a stirrer to obtain a mixture;
[0071] The mixture was transferred to an oven and dried at 110°C to obtain coated light sand;
[0072] (2) Preparation of modified polyvinyl alcohol
[0073] Add polyvinyl alcohol to water, heat and stir at 60°C for 3 hours until the polyvinyl alcohol is completely dissolved to obtain a polyvinyl alcohol solution with a mass percentage of 8%;
[0074] Add epoxy resin to the polyvinyl alcohol solution, heat and stir at 75°C for 3 hours, and after the reaction is completed, filter, wash and dry to obtain modified polyvinyl alcohol;
[0075] (3) Preparation of modified cellulose ether
[0076] The nanoclay was added into a 0.15M aqueous solution of hexadecyltrimethylammonium bromide, and ultrasonically stirred for 35 minutes to obtain a 2% nanoclay dispersion;
[0077] Add cellulose ether into water, heat and stir at 70°C for 4 hours until the cellulose ether is completely dissolved, to obtain a cellulose ether solution with a mass percentage of 6%;
[0078] Slowly pour the nanoclay dispersion into the cellulose ether solution, heat and stir at 80°C for 5 hours, and after the reaction is completed, centrifuge, wash and dry to obtain the modified cellulose ether;
[0079] (4) Preparation of tile adhesive
[0080] The coated light sand, cement, modified polyvinyl alcohol, modified cellulose ether, redispersible latex powder, density regulator, early strength agent, lubricant and water are mixed uniformly in proportion to obtain light and low-carbon tile adhesive mortar.
[0081] Lightweight low-carbon tile adhesive mortar includes the following raw materials in parts by weight:
[0082] 30 parts of coated light sand
[0083] 20 parts cement
[0084] Modified polyvinyl alcohol 8 parts
[0085] 3 parts of modified cellulose ether
[0086] 15 parts of redispersible latex powder
[0087] Density regulator 15 parts
[0088] 0.5 parts of early strength agent
[0089] 0.2 parts of lubricant
[0090] 15 parts water;
[0091] The modified polyvinyl alcohol includes polyvinyl alcohol and epoxy resin, and the mass ratio of polyvinyl alcohol to epoxy resin is 8:3; the molecular weight of polyvinyl alcohol is 170,000-220,000, purchased from Zhengzhou Shengyu Chemical Products Co., Ltd., and the epoxy resin is bisphenol A type epoxy resin with an epoxy equivalent of 238-256 g / mol, purchased from Jiangsu Sanmu Chemical Co., Ltd., model E-39D.
[0092] The modified cellulose ether includes nanoclay and cellulose ether, the mass ratio of nanoclay to cellulose ether is 1:10; the cellulose ether is carboxymethyl cellulose ether. The nanoclay material is a mixture of one or more of various naturally extracted or artificially synthesized layered silicate materials with a nano-sheet structure, the purity of each component should be higher than 95%, and the particle size of the nanoclay is 200nm, which is purchased from Shaoxing Pu Rui Coating Co., Ltd.
[0093] The redispersible latex powder is vinyl acetate-ethylene copolymer.
[0094] The density regulator is expanded vermiculite and expanded perlite, and the mass ratio of the two is 1:1.
[0095] The early strength agent is calcium formate.
[0096] The lubricant is polyacrylamide.
[0097] Example 2
[0098] The difference from Example 1 is that the formula of the lightweight and low-carbon tile adhesive is different.
[0099] The prescription of the present embodiment is as follows:
[0100] Lightweight low-carbon tile adhesive mortar includes the following raw materials in parts by weight:
[0101] 25 parts of coated light sand
[0102] 15 parts cement
[0103] 5 parts of modified polyvinyl alcohol
[0104] 2 parts of modified cellulose ether
[0105] Redispersible latex powder 10 parts
[0106] Density regulator 10 parts
[0107] 0.3 parts of early strength agent
[0108] Lubricant 0.1 part
[0109] 10 parts water;
[0110] The modified polyvinyl alcohol comprises polyvinyl alcohol and epoxy resin, and the mass ratio of polyvinyl alcohol to epoxy resin is 9:4;
[0111] The modified cellulose ether includes nano clay and cellulose ether, and the mass ratio of the nano clay to the cellulose ether is 2:12.
[0112] Example 3
[0113] The difference from Example 1 is that the formula of the lightweight and low-carbon tile adhesive is different.
[0114] The prescription of the present embodiment is as follows:
[0115] Lightweight low-carbon tile adhesive mortar comprises the following raw materials in parts by weight:
[0116] 35 parts of coated light sand
[0117] 25 parts cement
[0118] Modified polyvinyl alcohol 9 parts
[0119] 5 parts of modified cellulose ether
[0120] 22 parts of redispersible latex powder
[0121] Density regulator 18 parts
[0122] 0.8 parts of early strength agent
[0123] 0.3 parts of lubricant
[0124] 20 parts water;
[0125] The modified polyvinyl alcohol comprises polyvinyl alcohol and epoxy resin, and the mass ratio of polyvinyl alcohol to epoxy resin is 10:4;
[0126] The modified cellulose ether includes nano clay and cellulose ether, and the mass ratio of the nano clay to the cellulose ether is 3:15.
[0127] Comparative Example 1
[0128] The difference from Example 1 is that the coated lightweight sand is replaced by a lightweight sand composition.
[0129] Comparative Example 2
[0130] The difference from Example 1 is that the mass ratio of lightweight sand aggregate, fly ash and pumice is 3:0.2:0.3.
[0131] Comparative Example 3
[0132] The difference from Example 1 is that the modified polyvinyl alcohol is replaced by polyvinyl alcohol.
[0133] Comparative Example 4
[0134] The difference from Example 1 is that the high molecular weight polyvinyl alcohol is replaced by low molecular weight polyvinyl alcohol, and the molecular weight of the low molecular weight polyvinyl alcohol is specifically 25,000 to 35,000.
[0135] Comparative Example 5
[0136] The difference from Example 1 is that the mass ratio of polyvinyl alcohol to epoxy resin is 15:3.
[0137] Comparative Example 6
[0138] The difference from Example 1 is that the bisphenol A epoxy resin is replaced by a water-based epoxy resin with an epoxy equivalent of 450-550 g / mol, purchased from Shanghai Huayi Fine Chemical Co., Ltd., model number STW600.
[0139] Comparative Example 7
[0140] The difference from Example 1 is that the modified cellulose ether is replaced by cellulose ether.
[0141] Comparative Example 8
[0142] The difference from Example 1 is that the mass ratio of nanoclay to cellulose ether is 1:20.
[0143] Comparative Example 9
[0144] The difference from Example 1 is that the particle size of the lightweight sand aggregate is 0.8 mm.
[0145] Comparative Example 10
[0146] The difference from Example 1 is that the particle size of fly ash is 10 μm, and the particle size of pumice is 50 μm.
[0147] Performance Testing
[0148] The tile adhesive mortar prepared in the embodiment and the comparative example was tested for performance according to the industry standards JC / T547-2017 and JC / T984-2011. The test results are shown in Tables 1 and 2.
[0149] Table 1
[0150]
[0151] Table 2
[0152]
[0153] It can be seen from the above performance test results that the comprehensive performance of Examples 1-3, such as bonding strength and environmental resistance, is relatively excellent, especially the comprehensive performance of Example 1 is the most outstanding. This is mainly because three substances, namely, coated lightweight sand, modified polyvinyl alcohol and modified cellulose ether, are added to the lightweight and low-carbon tile adhesive. The synergistic effect of the three substances improves the comprehensive performance of the tile adhesive, such as bonding strength, acid and alkali resistance, and impermeability.
[0154] The comparative example, because it did not adopt the necessary technical solution, was significantly worse than the embodiment in the corresponding performance test. In comparative example 1, the composition of the coated light sand was changed, and the light sand composition mixed in proportion was directly applied to the preparation process of tile adhesive. It can be seen that the comprehensive effects such as bonding performance and environmental resistance decreased, proving that the light sand composition coated with silane coupling agent has an important influence on the comprehensive effect. In comparative example 2, the proportion of the three raw materials in the light sand composition was changed, which affected the balance relationship constructed by the three raw materials in this application. From the results, it can be seen that the mass ratio of the light sand composition was affected, resulting in a decrease in environmental resistance, indicating that the proportion of the light sand composition has an important influence on the comprehensive performance of the adhesive. In comparative example 3, pure polyvinyl alcohol that was not modified with epoxy resin was used, which affected the generation of the three-dimensional network structure, and then caused the various properties of the prepared tile adhesive to decrease, indicating that the modification of polyvinyl alcohol by epoxy resin has an important influence on the comprehensive performance of the tile adhesive. In Comparative Example 4, the high molecular weight polyvinyl alcohol used in this application is replaced with low molecular weight polyvinyl alcohol. Since the low molecular weight PVA has low bonding strength and weak weather resistance, it cannot form a three-dimensional network structure with epoxy resin, resulting in a decrease in the impermeability and bonding strength of the prepared lightweight low-carbon tile adhesive, indicating that the molecular weight of polyvinyl alcohol has an important influence on the comprehensive performance of the tile adhesive. In Comparative Example 5, the ratio of epoxy resin to polyvinyl alcohol is changed, and the comprehensive performance of the prepared tile adhesive is reduced, indicating that the ratio of the two directly affects the cross-linking reaction between the epoxy resin and the hydroxyl groups on the PVA molecular chain, and the ratio of the two has an important influence on the performance of the tile adhesive. In Comparative Example 6, the type of epoxy resin is changed, which also leads to a decrease in the impermeability, environmental resistance and bonding performance of the prepared tile adhesive, indicating that the type of epoxy resin has an important influence on the performance of the tile adhesive. In Comparative Example 7, pure cellulose ether without nanoclay modification is used. Due to the presence of tiny pores between the molecules of pure cellulose ether, the compactness of the prepared tile adhesive mortar deteriorates, the bonding strength deteriorates, and the impermeability also decreases, indicating that the modification of cellulose ether plays an important role in improving the performance of tile adhesive mortar. In Comparative Example 8, the addition ratio between nanoclay and cellulose ether is changed, and the stability of the formed network structure is insufficient, resulting in a decrease in the comprehensive performance of the prepared tile adhesive mortar, indicating that the ratio of the two plays an important role in improving the comprehensive performance of the tile adhesive mortar. Comparative Examples 9 and 10 change the particle size of the lightweight sand aggregate, fly ash and pumice in the lightweight sand composition. From the results, the compactness of the tile adhesive mortar prepared therefrom deteriorates, the bonding strength deteriorates, and the impermeability decreases, indicating that the particle size of the lightweight sand composition has a certain influence on the comprehensive performance of the tile adhesive mortar. The above experimental results further prove the importance of the technical scheme defined in this application for its technical effect.
[0155] Therefore, the present application adopts the above-mentioned lightweight and low-carbon tile adhesive building material, its preparation method and its application in the preparation of green building materials. The three substances added in the formula, namely, coated lightweight sand, modified polyvinyl alcohol and modified cellulose ether, have a synergistic effect, thereby improving the weather resistance, resistance to alternating hot and cold temperatures, impermeability and bonding strength of the lightweight and low-carbon tile adhesive. The comprehensive performance of the tile adhesive is improved, and it can be applied in the field of green building materials.
[0156] The applicant declares that the present application uses the above-mentioned embodiments to illustrate a lightweight and low-carbon tile adhesive mortar and its preparation method and its application in the preparation of green building materials, but the present application is not limited to the above-mentioned embodiments, that is, it does not mean that the present application must rely on the above-mentioned embodiments to be implemented. The technicians in the relevant technical field should understand that any improvement to the present application, the equivalent replacement of the raw materials of the present application product, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present application.
[0157] The preferred embodiments of the present application are described in detail above; however, the present application is not limited to the specific details in the above embodiments. Within the technical concept of the present application, a variety of simple modifications can be made to the technical solution of the present application, and these simple modifications all fall within the protection scope of the present application.
[0158] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not further describe various possible combinations.
Claims
1. A lightweight and low-carbon tile adhesive building material, characterized by: Lightweight low-carbon tile adhesive building materials include the following raw materials by weight: Coated light sand 15~40 parts 15~30 parts of cement Modified polyvinyl alcohol 5~10 parts Modified cellulose ether 2~5 parts Redispersible latex powder 3~25 parts Density regulator 10~20 parts Early strength agent 0.1~1 part Lubricant 0.05~0.5 parts 10-20 parts water; The modified polyvinyl alcohol comprises polyvinyl alcohol and epoxy resin, and the mass ratio of polyvinyl alcohol to epoxy resin is 8-10:2-5; The modified cellulose ether includes nanoclay and cellulose ether, and the mass ratio of nanoclay to cellulose ether is 1-3:10-15; The coated lightweight sand comprises a silane coupling agent and a lightweight sand composition, the mass ratio of the silane coupling agent to the lightweight sand composition is 1-5:100-300, the lightweight sand composition comprises lightweight sand aggregate, fly ash and pumice, the mass ratio of the lightweight sand aggregate, fly ash and pumice is 1-1.5:0.1-0.3:0.2-0.4; The molecular weight of polyvinyl alcohol is 170,000 to 220,000, and the epoxy resin is bisphenol A epoxy resin; The preparation method of the lightweight low-carbon tile adhesive mortar building material comprises the following steps: (1) Preparation of coated lightweight sand The lightweight sand aggregate, fly ash and pumice are mixed in proportion to obtain a lightweight sand composition; Add the silane coupling agent to ethanol and mix well to obtain a 0.05-0.1% coating solution; The coating solution is uniformly sprayed on the light sand composition, and stirred at room temperature for 20 to 30 minutes using a stirrer to obtain a mixture; The mixture is transferred to an oven and dried at 100-120°C to obtain coated light sand; (2) Preparation of modified polyvinyl alcohol Add polyvinyl alcohol to water, heat and stir at 55-65°C for 2-4 hours until the polyvinyl alcohol is completely dissolved to obtain a polyvinyl alcohol solution with a mass percentage of 5-10%; Add epoxy resin to the polyvinyl alcohol solution, heat and stir at 70-80°C for 2-5 hours, and after the reaction is completed, filter, wash and dry to obtain modified polyvinyl alcohol; (3) Preparation of modified cellulose ether The nanoclay is added to an aqueous solution of hexadecyltrimethylammonium bromide with a concentration of 0.1-0.2 M, and ultrasonically stirred for 30-40 minutes to obtain a nanoclay dispersion with a mass percentage of 1-5%. Add cellulose ether into water, heat and stir at 60-80°C for 3-5 hours until the cellulose ether is completely dissolved to obtain a cellulose ether solution with a mass percentage of 5-8%; Slowly pour the nanoclay dispersion into the cellulose ether solution, heat and stir at 60-100°C for 4-6 hours, and after the reaction is completed, centrifuge, wash, and dry to obtain the modified cellulose ether; (4) Preparation of tile adhesive The coated light sand, cement, modified polyvinyl alcohol, modified cellulose ether, redispersible latex powder, density regulator, early strength agent, lubricant and water are uniformly mixed in proportion to obtain a light and low-carbon tile adhesive mortar building material.
2. A lightweight and low-carbon tile adhesive building material according to claim 1, characterized in that: The cellulose ether is one or more of carboxymethyl cellulose ether, hydroxypropyl methyl cellulose ether and hydroxyethyl cellulose ether.
3. A lightweight and low-carbon tile adhesive building material according to claim 1, characterized in that: The redispersible latex powder is one or more of vinyl acetate-ethylene copolymer, vinyl acetate-ethylene-vinyl versatate polymer, styrene-acrylate copolymer, vinyl acetate-vinyl versatate-acrylic acid-ethylene copolymer, and vinyl chloride-ethylene-vinyl laurate copolymer.
4. A lightweight and low-carbon tile adhesive building material according to claim 1, characterized in that: The density regulator is one or more of vitrified microspheres, expanded vermiculite, expanded perlite, sepiolite, walnut shells, and volcanic rock particles.
5. The lightweight and low-carbon tile adhesive building material according to claim 1 is characterized by: The early strength agent is one or more of calcium formate, calcium chloride and sodium sulfate.
6. A lightweight and low-carbon tile adhesive building material according to claim 1, characterized in that: The lubricant is one or more of bentonite, methyl cellulose and polyacrylamide.
7. The use of a lightweight low-carbon tile adhesive building material according to any one of claims 1 to 6, characterized in that: The lightweight and low-carbon tile adhesive mortar building material is used for the preparation of green building materials.