Grouting material based on magnetic particle tracing as well as preparation method and application of grouting material
By using grouting materials traced by magnetic particles in coal mine tunnels, the problem of difficulty in determining the diffusion pattern of grouting liquid within the surrounding rock of the tunnel is solved, and the dynamic detection of cracks and slurry diffusion in the surrounding rock of the tunnel is realized, as well as the grouting reinforcement effect. improvement.
Patent Information
- Application Number
- CN202410940455.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-12
AI Technical Summary
In the control of surrounding rock in coal mine tunnels, it is difficult to accurately obtain the flow and diffusion rules of grouting fluid in the internal cracks of surrounding rock in coal mines with existing technology, which makes it difficult to judge the grouting reinforcement effect and lacks real-time and detailed visual representation methods.
Using grouting materials based on magnetic particle tracers, polypolyol-modified magnetic nanoparticles are prepared by polymerizing magnetic particles with active hydroxyl sites on the surface and a polyol mixture, and are added to the gelling material to form Tracers that can diffuse and flow in the cracks in the surrounding rock of the roadway are monitored and tracked using detection equipment.
It achieves dynamic detection of cracks in the surrounding rock of the tunnel and slurry diffusion, improves the fluidity and interface bonding strength of the grouting material, improves the grouting reinforcement effect, and provides a simple and low-cost tracing function.
Smart Images

Figure CN118812221A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of mining engineering technology, and in particular to a grouting material based on magnetic particle tracing, a preparation method and application thereof. Background Art
[0002] The technology of "support-modification-pressure relief" coordinated control has gradually been formed in the field of coal mine roadway surrounding rock control. Grouting reinforcement, as an effective means of roadway surrounding rock control, has been widely used in the field of coal mine roadway surrounding rock control. Due to the concealment of grouting slurry penetrating into the internal cracks of the roadway surrounding rock, coupled with the complex characteristics of the coal mine roadway itself such as anisotropy, it is difficult to accurately know the flow and diffusion law of slurry in the internal cracks of the coal mine roadway surrounding rock, resulting in the difficulty in judging the effect of grouting reinforcement of coal mine roadway surrounding rock. At present, the flow distribution state of slurry during grouting is still concentrated on model simulation, lacking real-time and detailed intuitive characterization methods, and it is difficult to reveal the penetration and diffusion mechanism of slurry in the cracked rock mass of coal mine roadway surrounding rock. Summary of the invention
[0003] The present application aims to solve at least one of the technical problems in the related art to a certain extent. The present application provides a grouting material based on magnetic particle tracing, a preparation method and its application, wherein the grouting material includes polyol-modified magnetic nanoparticles, which can be used as magnetic particle tracing components, and when the grouting material is injected into the cracks in the surrounding rock of the tunnel, the polyol-modified magnetic nanoparticles diffuse and flow along the cracks in the surrounding rock of the tunnel, and can be monitored and tracked by detection equipment, thereby completing dynamic detection of the cracks in the surrounding rock of the tunnel and the diffusion of the grouting material.
[0004] To achieve the above-mentioned object, according to the first aspect of the present application, a method for preparing a grouting material based on magnetic particle tracing is proposed, comprising the following steps:
[0005] Adding magnetic particles with active hydroxyl sites on the surface into a polyol mixture, and performing polymerization reaction under the catalytic action of a composite catalyst and a protective atmosphere to obtain polyol-modified magnetic nanoparticles;
[0006] Add 12-15 parts by weight of the polyol-modified magnetic nanoparticles and 5-13 parts by weight of an auxiliary agent into 100-120 parts by weight of a gelling material, and stir to obtain a dry powder.
[0007] In some embodiments, based on weight percentage, the magnetic particles are 20 parts; the polyol mixture is 70-80 parts; and the composite catalyst is 5-8 parts.
[0008] In some embodiments, the magnetic particles are obtained by plasma treating iron oxide nanoparticles, iron silicate nanoparticles and aluminum nickel cobalt nanoparticles, and the mass ratio of the iron oxide nanoparticles, the iron silicate nanoparticles and the aluminum nickel cobalt nanoparticles is (2-5): (1-2): (2-4).
[0009] In some embodiments, the parameters of the plasma treatment are power 5-6 kW, frequency 2450-2500 MHz, density 25-28 W / cm 2 , time 15-18 minutes.
[0010] In some embodiments, the polyol mixture includes ethylene glycol, glycerol, and caprylyl glycol in a mass ratio of 2:1:1.
[0011] In some embodiments, the composite catalyst includes nickel octadienediyl, nickel cobalt sulfide, and nickel acetylacetonate in a mass ratio of 1:1:3.
[0012] In some embodiments, the protective atmosphere is an inert gas, including nitrogen, helium or neon.
[0013] In some embodiments, the polymerization reaction parameters are 190-200° C. and reaction time of 50 min.
[0014] In some embodiments, the additives include, by weight, 1-2 parts of a dispersant, 1-3 parts of a coagulant, 1 part of a toughening agent, 1-5 parts of a reinforcing agent, and 1-2 parts of a fluid loss reducer.
[0015] In some embodiments, the cementitious material includes sulphoaluminate clinker, ferroaluminate clinker and aluminate clinker mixed in a mass ratio of 1:1:2.
[0016] According to another purpose of the present application, a grouting material based on magnetic particle tracing is proposed, which includes a mixture A and a cementitious material; in terms of mass parts, the mixture A includes 12-15 parts of polyol-modified magnetic nanoparticles and 5-13 parts of additives; the cementitious material has a mass fraction of 100-120 parts and includes sulphoaluminate clinker, ferroaluminate clinker and aluminate clinker mixed in a mass ratio of 1:1:2.
[0017] In some embodiments, the additives include, by weight, 1-2 parts of a dispersant, 1-3 parts of a coagulant, 1 part of a toughening agent, 1-5 parts of a reinforcing agent, and 1-2 parts of a fluid loss reducer.
[0018] In some embodiments, the polyol-modified magnetic nanoparticles are obtained by adding magnetic particles having active hydroxyl sites on the surface into a polyol mixture and performing a polymerization reaction under the catalytic action of a composite catalyst and a protective atmosphere.
[0019] According to another object of the present application, it is proposed that the grouting material described in any of the above embodiments is used in magnetic particle tracer grouting in large deformation tunnels in coal mines, and the grouting material described in any of the above embodiments is also used as a tracer in large deformation tunnels.
[0020] Compared with the prior art, this application has the following advantages:
[0021] In the present application, the magnetic particles with active hydroxyl sites on the surface are modified by a polyol mixture, which can reduce the interfacial tension of the polyol-modified magnetic nanoparticles, prevent the agglomeration of the polyol-modified magnetic nanoparticles, and improve the uniform dispersion of the polyol-modified magnetic nanoparticles in the gelling material; at the same time, the polyol-modified magnetic nanoparticles present a spherical shape, and the ball effect can reduce the flow friction resistance of the grouting material and improve the fluidity of the grouting material.
[0022] After the grouting material is injected into the cracks of the tunnel surrounding rock, the polyol-modified magnetic nanoparticles in the grouting material diffuse and flow along the cracks, and are monitored and tracked by detection equipment to achieve dynamic detection of the cracks in the tunnel surrounding rock and the diffusion of slurry; in addition, the surface of the polyol-modified magnetic nanoparticles has a variety of hydroxyl functional groups, which form hydrogen bonds with the hydroxyl groups on the surface of the coal rock mass, thereby improving the interface bonding strength between the grouting stone body formed by the grouting material and the coal rock mass, thereby improving the grouting reinforcement effect.
[0023] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0025] Figure 1 This is a flow chart of a method for preparing a grouting material based on magnetic particle tracing in one embodiment of the present application.
[0026] Figure 2 yes Figure 1 Detailed flow chart. DETAILED DESCRIPTION
[0027] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be construed as limiting the present application. On the contrary, the embodiments of the present application include all changes, modifications and equivalents that fall within the spirit and connotation of the appended claims.
[0028] like Figure 1 As shown, in order to achieve the above-mentioned purpose, according to the first aspect of the present application, a preparation method of a grouting material based on magnetic particle tracing is proposed, comprising the following steps;
[0029] S1: adding magnetic particles having active hydroxyl sites on the surface into a polyol mixture, and performing a polymerization reaction under the catalytic action of a composite catalyst and a protective atmosphere to obtain polyol-modified magnetic nanoparticles;
[0030] S2: Add 12-15 parts by weight of polyol-modified magnetic nanoparticles and 5-13 parts by weight of an auxiliary agent into 100-120 parts by weight of a gelling material, and stir to obtain a dry powder.
[0031] Among them Figure 2 As shown, in S1, iron oxide nanoparticles, iron silicate nanoparticles and aluminum nickel cobalt nanoparticles are mixed in a mass ratio of (2-5): (1-2): (2-4), and plasma treatment is performed to obtain magnetic particles having active hydroxyl sites on the surface, wherein the parameters of the plasma treatment are power 5-6kW, frequency 2450-2500MHz, density 25-28W / cm 2 , time 15-18 minutes.
[0032] According to the weight percentage, 20 parts of magnetic particles are added to 70-80 parts of a polyol mixture, wherein the polyol mixture includes ethylene glycol, propylene glycol and octanediol in a weight ratio of 2:1:1, and 5-8 parts of a composite catalyst are added, wherein the composite catalyst includes octadienediyl nickel, cobalt nickel sulfide and acetylacetone nickel in a weight ratio of 1:1:3; auxiliary heating is performed in a microwave reaction tube to promote the polymerization reaction, an inert gas protection such as nitrogen, helium or neon is introduced, and the reaction is carried out at 190-200°C in the microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0033] Wherein this embodiment forms active hydroxyl sites on the surface of iron oxide nanoparticles, iron silicate nanoparticles, and aluminum nickel cobalt nanoparticles through plasma treatment, adds them to ethylene glycol, glycerol, and octanediol mixed monomers, adds octadiene diyl nickel, cobalt nickel sulfide, and acetylacetone nickel composite catalysts, and auxiliary heating promotes polymerization reaction, passes through inert gas protection, and prepares polyol-modified magnetic nanoparticles through polymerization reaction in a microwave reaction tube. The polyol-modified magnetic nanoparticles obtained in this application are modified by polyols on their surfaces, which can reduce the interfacial tension of the polyol-modified magnetic nanoparticles, prevent the polyol-modified magnetic nanoparticles from agglomerating, and improve the uniform dispersibility of the polyol-modified magnetic nanoparticles in the substrate. And the polyol-modified magnetic nanoparticles present a spherical shape, and when used as a part of the grouting material, the ball effect can reduce the flow friction resistance of the grouting material slurry, thereby improving the fluidity of the grouting material.
[0034] like Figure 2 In S2, 12-15 parts of the polyol-modified magnetic nanoparticles obtained in S1 and 5-13 parts of the auxiliary agent are added to 100-120 parts of the gelling material by mass, and the dry powder is stirred and mixed in a dry powder mixer for 30 minutes. The auxiliary agents include 1-2 parts of dispersant, 1-3 parts of coagulant, 1 part of toughening agent, 1-5 parts of reinforcing agent and 1-2 parts of fluid loss reducer; the dispersant includes ethylene bis stearamide, monoglyceride of stearic acid, copper stearate and magnesium stearate, and their mass ratios are 2:2:1:1 respectively; the coagulant includes magnesium oxide, magnesium chloride, magnesium sulfate and disodium magnesium ethylenediaminetetraacetate, and their mass ratios are 1:4:1:2 respectively; the toughening agent includes polyacrylamide, polyethyleneimine and polyethylene oxide, and their mass ratios are 1:1:7 respectively; the reinforcing agent includes tetraammine copper sulfate, potassium trichloro(ethylene)platinate(II) and monochloropentamminecobalt(III) sulfate, and their mass ratios are 2:1:9 respectively; the fluid loss reducer includes sodium humate and sulfomethylphenolic resin in a mass ratio of 1:5. In this embodiment, the cementitious material includes sulphoaluminate clinker, ferroaluminate clinker and aluminate clinker mixed in a mass ratio of 1:1:2, for example, 30 parts of sulphoaluminate clinker, 30 parts of ferroaluminate clinker and 60 parts of aluminate clinker.
[0035] In this embodiment, the prepared polyol-modified magnetic nanoparticles, dispersants, coagulants, toughening agents, reinforcing agents, and fluid loss reducers are added to sulphoaluminate, ferroaluminate, and aluminate clinker gelling materials to prepare grouting materials based on magnetic particle tracing suitable for large deformation lanes in coal mines and their preparation methods. In the grouting material of this embodiment, the polyol-modified magnetic nanoparticles are injected into the cracks of the surrounding rock of the lane along with the grouting material. The polyol-modified magnetic nanoparticles diffuse and flow along the cracks, and are monitored and tracked by detection equipment to achieve dynamic detection of the cracks of the surrounding rock of the lane and the diffusion of slurry; in addition, the surface of the polyol-modified magnetic nanoparticles has a variety of hydroxyl functional groups, which form hydrogen bonding forces with the hydroxyl groups on the surface of the coal rock mass, thereby improving the interfacial bonding strength between the grouting stone body formed by the grouting material and the coal rock mass, and improving the grouting reinforcement effect. Finally, the grouting material of this application realizes a simple, low-cost, and tracing function-based preparation method of the grouting material for large deformation lanes in coal mines based on magnetic particle tracing.
[0036] According to another purpose of the present application, a grouting material based on magnetic particle tracing is proposed, which includes a mixture A and a cementitious material; in terms of mass parts, the mixture A includes 12-15 parts of polyol-modified magnetic nanoparticles and 5-13 parts of additives; the cementitious material has a mass fraction of 100-120 parts and includes sulphoaluminate clinker, ferroaluminate clinker and aluminate clinker mixed in a mass ratio of 1:1:2.
[0037] Among them, this embodiment proposes a grouting material based on magnetic particle tracing, which includes A mixture and cementitious material, wherein A mixture includes 12-15 parts of polyol-modified magnetic nanoparticles and 5-13 parts of additives; polyol-modified magnetic nanoparticles are obtained according to the method in the above embodiment and will not be repeated; according to the mass parts, the additives include 1-2 parts of dispersant, 1-3 parts of accelerator, 1 part of toughening agent, 1-5 parts of reinforcing agent and 1-2 parts of fluid loss reducer. The cementitious material includes 30-35 parts of sulphoaluminate clinker, 30-40 parts of ferroaluminate clinker and 40-45 parts of aluminate clinker.
[0038] According to another object of the present application, it is proposed that the grouting material in any of the above embodiments is used in magnetic particle tracing grouting in large deformation tunnels in coal mines, and the grouting material in any of the above embodiments is also used as a tracer in large deformation tunnels.
[0039] The following is a specific example of the preparation method of the magnetic particle tracer grouting material.
[0040] Example 1
[0041] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 6 kW, a plasma frequency of 2500 MHz and a plasma density of 28 W / cm 2 , the time is 18 minutes plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 200°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0042] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0043] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0044] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the auxiliary agent in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0045] Dispersion coefficient of magnetic nanoparticles: 1.27;
[0046] Magnetic nanoparticle size: 47nm;
[0047] Magnetic field strength of magnetic nanoparticles: 79emu / g.
[0048] Compressive strength of grouting material: 47MPa.
[0049] Example 2
[0050] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 15 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 5 kW, a plasma frequency of 2450 MHz and a plasma density of 25 W / cm 2, the time is 15 minutes of plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 190°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0051] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0052] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0053] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the auxiliary agent in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0054] Dispersion coefficient of magnetic nanoparticles: 1.24;
[0055] Magnetic nanoparticle size: 42nm;
[0056] Magnetic field strength of magnetic nanoparticles: 86emu / g.
[0057] Compressive strength of grouting material: 49MPa.
[0058] Example 3
[0059] 10 kg of iron oxide nanoparticles, 10 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 6 kW, a plasma frequency of 2500 MHz and a plasma density of 28 W / cm 2 , the time is 18 minutes plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 200°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0060] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0061] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0062] Take 15 kg of the polyol-modified magnetic nanoparticles and 10 kg of the additives in this embodiment and add them to 100 kg of the gelling material, stir and mix the dry powder in a dry powder mixer for 30 minutes to obtain a grouting material, and test the product quality indicators;
[0063] Dispersion coefficient of magnetic nanoparticles: 1.22;
[0064] Magnetic nanoparticle size: 40nm;
[0065] Magnetic field strength of magnetic nanoparticles: 94emu / g.
[0066] Compressive strength of grouting material: 50MPa.
[0067] Example 4
[0068] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 5 kW, a plasma frequency of 2450 MHz and a plasma density of 25 W / cm 2 , the time is 15 minutes of plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 190°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0069] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0070] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0071] 12 kg of the polyol-modified magnetic nanoparticles and 10 kg of the auxiliary agent in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0072] Magnetic nanoparticle dispersion coefficient: 1.20;
[0073] Magnetic nanoparticle size: 36nm;
[0074] Magnetic field strength of magnetic nanoparticles: 96emu / g.
[0075] Compressive strength of grouting material: 54MPa.
[0076] Example 5
[0077] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 5 kW, a plasma frequency of 2450 MHz and a plasma density of 25 W / cm 2 , the time is 15 minutes of plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 190°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0078] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0079] Prepare 13 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 5 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0080] 13 kg of the polyol-modified magnetic nanoparticles and 13 kg of the auxiliary agent in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0081] Dispersion coefficient of magnetic nanoparticles: 1.18;
[0082] Magnetic nanoparticle size: 31nm;
[0083] Magnetic field strength of magnetic nanoparticles: 107emu / g.
[0084] Compressive strength of grouting material: 55MPa.
[0085] Example 6
[0086] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 5 kW, a plasma frequency of 2450 MHz and a plasma density of 25 W / cm 2 , the time is 15 minutes of plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 190°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0087] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0088] Prepare 5 kg of auxiliary agent by mixing 1 kg of dispersant, 1 kg of accelerator, 1 kg of toughening agent, 1 kg of reinforcing agent and 1 kg of fluid loss reducer;
[0089] 13 kg of the polyol-modified magnetic nanoparticles and 5 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0090] Dispersion coefficient of magnetic nanoparticles: 1.15;
[0091] Magnetic nanoparticle size: 27nm;
[0092] Magnetic field strength of magnetic nanoparticles: 105emu / g.
[0093] Compressive strength of grouting material: 50MPa.
[0094] Example 7
[0095] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 5 kW, a plasma frequency of 2450 MHz and a plasma density of 25 W / cm 2, the time is 15 minutes of plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 190°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0096] Component B is a cementitious material. 120 kg of cementitious material is prepared by mixing 30 kg of sulphoaluminate clinker, 30 kg of ferroaluminate clinker and 60 kg of aluminate clinker.
[0097] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0098] 13 kg of the polyol-modified magnetic nanoparticles and 5 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0099] Dispersion coefficient of magnetic nanoparticles: 1.19;
[0100] Magnetic nanoparticle size: 32nm;
[0101] Magnetic field strength of magnetic nanoparticles: 106emu / g.
[0102] Compressive strength of grouting material: 56MPa.
[0103] Example 8
[0104] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 5 kW, a plasma frequency of 2450 MHz and a plasma density of 25 W / cm 2 , the time is 15 minutes of plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and auxiliary heating is used to promote the polymerization reaction. Nitrogen protection is introduced, and the reaction is carried out at 190°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0105] Component B is a cementitious material. To prepare 100 kg of cementitious material, 25 kg of sulphoaluminate clinker, 25 kg of ferroaluminate clinker and 50 kg of aluminate clinker are mixed;
[0106] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0107] 13 kg of the polyol-modified magnetic nanoparticles and 5 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested.
[0108] Dispersion coefficient of magnetic nanoparticles: 1.19;
[0109] Magnetic nanoparticle size: 30nm;
[0110] Magnetic field strength of magnetic nanoparticles: 108emu / g.
[0111] Compressive strength of grouting material: 51MPa.
[0112] Comparative Example 1
[0113] This comparative example is different from Example 1 as follows:
[0114] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 4 kW, a plasma frequency of 2500 MHz and a plasma density of 20 W / cm 2 , time is 18 minutes; polyol-modified magnetic nanoparticles are prepared.
[0115] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0116] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0117] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested;
[0118] Dispersion coefficient of magnetic nanoparticles: 1.50;
[0119] Magnetic nanoparticle size: 113nm;
[0120] Magnetic field strength of magnetic nanoparticles: 77emu / g.
[0121] Compressive strength of grouting material: 34MPa.
[0122] Comparative Example 1
[0123] This comparative example is different from Example 1 as follows:
[0124] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 4 kW, a plasma frequency of 2500 MHz and a plasma density of 20 W / cm 2 , time is 18 minutes; polyol-modified magnetic nanoparticles are prepared.
[0125] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0126] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0127] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested;
[0128] Dispersion coefficient of magnetic nanoparticles: 1.53;
[0129] Magnetic nanoparticle size: 97nm;
[0130] Magnetic field strength of magnetic nanoparticles: 41emu / g.
[0131] Compressive strength of grouting material: 30MPa.
[0132] Comparative Example 2
[0133] This comparative example is different from Example 1 as follows:
[0134] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 4 kW, a plasma frequency of 2500 MHz and a plasma density of 20 W / cm 2 , time is 18 minutes; polyol-modified magnetic nanoparticles are prepared.
[0135] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0136] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0137] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested;
[0138] Dispersion coefficient of magnetic nanoparticles: 1.71;
[0139] Magnetic nanoparticle size: 135nm;
[0140] Magnetic field strength of magnetic nanoparticles: 32emu / g.
[0141] Compressive strength of grouting material: 29MPa.
[0142] Comparative Example 3
[0143] This comparative example is different from Example 1 as follows:
[0144] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 6 kW, a plasma frequency of 2500 MHz and a plasma density of 28 W / cm 2 , the time is 18 minutes plasma treatment to form active hydroxyl sites on its surface, and magnetic particles are obtained. The magnetic particles are added to a polyol mixture formed by mixing 40 kg of ethylene glycol, 20 kg of propylene glycol and 20 kg of octanediol, and a composite catalyst formed by mixing 1 kg of octadienediyl nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel, and nitrogen is passed through the mixture for protection. The mixture is stirred at room temperature in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles.
[0145] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0146] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0147] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested;
[0148] Dispersion coefficient of magnetic nanoparticles: 1.73;
[0149] Magnetic nanoparticle size: 122nm;
[0150] Magnetic field strength of magnetic nanoparticles: 79emu / g.
[0151] Compressive strength of grouting material: 27MPa.
[0152] Comparative Example 4
[0153] This comparative example is different from Example 1 as follows:
[0154] 10 kg of iron oxide nanoparticles, 5 kg of iron silicate nanoparticles and 10 kg of aluminum nickel cobalt nanoparticles were mixed and subjected to a plasma power of 6 kW, a plasma frequency of 2500 MHz and a plasma density of 28 W / cm 2 , the time is 18 minutes plasma treatment to form active hydroxyl sites on the surface, and magnetic particles are obtained. The magnetic particles are added to 80 kg of octanediol, 1 kg of octadiene nickel, 1 kg of cobalt nickel sulfide and 3 kg of acetylacetonate nickel to form a composite catalyst, auxiliary heating to promote the polymerization reaction, nitrogen protection is introduced, and the reaction is carried out at 200°C in a microwave reaction tube for 50 minutes to prepare polyol-modified magnetic nanoparticles. .
[0155] Component B is a cementitious material. 110 kg of cementitious material is prepared by mixing 27.5 kg of sulphoaluminate clinker, 27.5 kg of ferroaluminate clinker and 55 kg of aluminate clinker.
[0156] Prepare 10 kg of auxiliary agent by mixing 2 kg of dispersant, 3 kg of accelerator, 1 kg of toughening agent, 2 kg of reinforcing agent and 2 kg of fluid loss reducer;
[0157] 13 kg of the polyol-modified magnetic nanoparticles and 10 kg of the additives in this embodiment were added to 100 kg of the gelling material, and the dry powder was stirred and mixed in a dry powder mixer for 30 minutes to obtain a grouting material, and the product quality indicators were tested;
[0158] Dispersion coefficient of magnetic nanoparticles: 1.69;
[0159] Magnetic nanoparticle size: 143nm;
[0160] Magnetic field strength of magnetic nanoparticles: 48emu / g.
[0161] Compressive strength of grouting material: 30MPa.
[0162] It should be noted that, in the description of this application, the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. In addition, in the description of this application, unless otherwise specified, the meaning of "plurality" is two or more.
[0163] Any process or method description in a flowchart or otherwise described herein may be understood to represent a module, segment or portion of code that includes one or more executable instructions for implementing the steps of a specific logical function or process, and the scope of the preferred embodiments of the present application includes alternative implementations in which functions may not be performed in the order shown or discussed, including performing functions in a substantially simultaneous manner or in the reverse order depending on the functions involved, which should be understood by technicians in the technical field to which the embodiments of the present application belong.
[0164] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0165] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A method for preparing a grouting material based on magnetic particle tracing, characterized in that: The steps include: Adding magnetic particles with active hydroxyl sites on the surface into a polyol mixture, and performing a polymerization reaction under the catalytic action of a composite catalyst and a protective atmosphere to obtain polyol-modified magnetic nanoparticles; Add 12-15 parts by weight of the polyol-modified magnetic nanoparticles and 5-13 parts by weight of an auxiliary agent into 100-120 parts by weight of a gelling material, and stir to obtain a dry powder.
2. The preparation method according to claim 1, characterized in that: In terms of weight percentage, the magnetic particles account for 20 parts; the polyol mixture accounts for 70-80 parts; and the composite catalyst accounts for 5-8 parts.
3. The preparation method according to claim 2, characterized in that: The magnetic particles are obtained by plasma treatment of iron oxide nanoparticles, iron silicate nanoparticles and aluminum nickel cobalt nanoparticles, and the mass ratio of the iron oxide nanoparticles, the iron silicate nanoparticles and the aluminum nickel cobalt nanoparticles is (2-5): (1-2): (2-4).
4. The preparation method according to claim 3, characterized in that: The parameters of the plasma treatment are power 5-6kW, frequency 2450-2500MHz, density 25-28W / cm 2 , time 15-18min.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The polyol mixture comprises ethylene glycol, propylene glycol and octanediol in a mass ratio of 2:1:
1.
6. The preparation method according to claim 5, characterized in that: The composite catalyst comprises nickel octadiene, nickel cobalt sulfide and nickel acetylacetonate in a mass ratio of 1:1:
3.
7. The preparation method according to claim 5, characterized in that: The protective atmosphere is an inert gas, including nitrogen, helium or neon.
8. The preparation method according to claim 5, characterized in that: The polymerization reaction parameters are 190-200° C. and reaction time of 50 min.
9. The preparation method according to claim 5, characterized in that: Calculated by weight, the additives include 1-2 parts of dispersant, 1-3 parts of accelerator, 1 part of toughening agent, 1-5 parts of reinforcing agent and 1-2 parts of fluid loss reducer.
10. The preparation method according to claim 5, characterized in that: The cementitious material includes sulphoaluminate clinker, ferroaluminate clinker and aluminate clinker mixed in a mass ratio of 1:1:
2.
11. A grouting material based on magnetic particle tracing, characterized in that: It includes a mixture A and a gelling material; in terms of weight, the mixture A includes 12-15 parts of polyol-modified magnetic nanoparticles and 5-13 parts of an auxiliary agent; the gelling material has a weight of 100-120 parts and includes sulphoaluminate clinker, ferroaluminate clinker and aluminate clinker mixed in a weight ratio of 1:1:
2.
12. The grouting material according to claim 11, characterized in that: Calculated by weight, the additives include 1-2 parts of dispersant, 1-3 parts of accelerator, 1 part of toughening agent, 1-5 parts of reinforcing agent and 1-2 parts of fluid loss reducer.
13. The grouting material according to claim 11, characterized in that: The polyol-modified magnetic nanoparticles are obtained by adding magnetic particles with active hydroxyl sites on the surface into a polyol mixture and performing polymerization reaction under the catalytic action of a composite catalyst and a protective atmosphere.
14. The grouting material according to any one of claims 11 to 13 is used in magnetic particle tracer grouting in large deformation tunnels of coal mines, characterized in that: The grouting material described in any one of claims 11-13 is also used as a tracer in large deformation tunnels.
Citation Information
Patent Citations
Method for synthesizing magnetic samarium cobalt nano-particles by using polyalcohol
CN101695758A
Preparation method of manganese-zinc ferrite magnetic nanoparticle
CN102503390A
Preparation method of magnetic nanoparticles, magnetic energy conversion method and application
CN109498806A
Magnetic photonic crystal microsphere material and preparation method thereof
CN110230042A
Grouting track tracing system for fractured rock mass of coal seam roof and slurry selection method
CN115980172A
Cited By
Grouting track tracing system for fractured rock mass of coal seam roof and slurry selection method
CN115980172A
Coal seam roof fissure rock mass grouting trajectory tracing system and slurry selection method
CN115980172B