High-temperature thermal insulation material and preparation method thereof
By using a combination of nanosol and inorganic high-temperature fiber materials in high-temperature insulation materials, forming them by vacuum suction filtration, and adding silica fume and α-alumina powder, the problem of uneven pores in traditional insulation materials is solved and the strength of the material is improved. and thermal insulation properties, suitable for lining high temperature equipment.
Patent Information
- Application Number
- CN202410835511.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-22
AI Technical Summary
The pores of traditional high-temperature insulation materials are large and unevenly distributed, resulting in poor structural strength and thermal insulation uniformity of the material, limiting its use in structures with high strength requirements.
Nano-sol is used as a binding agent, and inorganic high-temperature fiber materials are formed through vacuum suction filtration. Silica fume and α-alumina powder are added to form a high-temperature thermal insulation material with small pores and even distribution, improving the flexural strength and thermal insulation performance of the material.
It achieves high strength and good insulation performance of high-temperature insulation materials, reduces high-temperature re-burning shrinkage, expands the use scenarios of the material, and can be used as a lining for high-temperature equipment.
Smart Images

Figure BDA0004913061380000071 
Figure HDA0004913061390000011
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of thermal insulation materials, and in particular to a high-temperature thermal insulation material and a preparation method thereof. Background Art
[0002] Thermal insulation materials refer to materials that can block the transfer of heat flow, also known as thermal insulation materials. Traditional thermal insulation materials include glass fiber, asbestos, rock wool, silicate, etc., and new thermal insulation materials include aerogel felt, vacuum panels, etc. They are used for building enclosures or thermal equipment, materials or material composites that resist heat flow transfer, including both thermal insulation materials and cold insulation materials. On the one hand, thermal insulation materials meet the thermal environment of building space or thermal equipment, and on the other hand, they also save energy.
[0003] There are generally two commonly used methods for making high-temperature thermal insulation materials. One is the burn-out method, in which combustible materials are added to the material. During the firing process, the combustibles are burned away, leaving pores, which reduces the density of the material and thus improves the thermal insulation of the material. The other is the foaming method, in which a foaming agent is added to the material. During the preparation process, the foaming agent produces gas and bubbles, leaving pores in the material. The remaining pores reduce the density of the material, thereby improving the thermal insulation of the material. However, the thermal insulation materials produced by these two methods have large pores and uneven distribution, which greatly reduces the structural strength of the material and the uniformity of thermal insulation. The material cannot be used in structures with high strength requirements, limiting its scope of use. Summary of the invention
[0004] In order to improve the strength and thermal insulation performance of the prepared thermal insulation material, the present application provides a high-temperature thermal insulation material and a preparation method thereof.
[0005] In the first aspect, the present application provides a high-temperature thermal insulation material, which adopts the following technical solution: A high-temperature thermal insulation material, the raw materials of which include the following components in parts by weight: 150-200 parts of nanosol, 10-30 parts of inorganic high-temperature fiber material, 3-5 parts of silica fume, 70-80 parts of α-alumina powder, and 3-5 parts of sintering agent.
[0006] By adopting the above technical solution, using nanosol as a binder, and then combining with inorganic high-temperature fiber materials, the high-temperature insulation material formed by vacuum filtration has small pores and uniform distribution, so that the high-temperature insulation material has good insulation performance. Due to the addition of inorganic high-temperature fibers, the flexural strength of the material is several times higher than that of the high-temperature insulation material of the same density; at the same time, the high-temperature reburning shrinkage rate of the material is also small, which greatly improves the use scenario of the material and can be directly used as the lining of high-temperature equipment; Silica fume has excellent flow properties and extremely high activity. It can fill the gaps and defects in refractory materials and improve the density and hardness of the materials. At the same time, silica fume can generate a high-strength silicate phase through reaction, which greatly enhances the compressive strength and wear resistance of the materials. The radiation effect and thermal conductivity coefficient of silica fume are very low, so it can effectively improve the thermal insulation performance of refractory materials. α-alumina powder has the characteristics of high temperature resistance, high strength, high hardness and oxidation resistance, so it can further improve the strength and thermal insulation performance of the obtained insulation material.
[0007] In a specific embodiment, the nanosol comprises nanosilica sol.
[0008] By adopting the above technical solution, nano-silica sol has higher bonding strength and high temperature resistance, which can improve the strength of the thermal insulation material. Nano-silica sol is used as a binder and baked at low temperature. The material can reach the strength required for use without high-temperature firing, which is energy-saving and environmentally friendly and reduces production costs.
[0009] In a specific embodiment, the inorganic high temperature fiber material includes alumina fiber, aluminum silicate fiber, or a mixture of the two.
[0010] By adopting the above technical solution and adding alumina fibers and aluminum silicate fibers, the thermal insulation material can be prepared by the suction filtration method, and it also has higher strength and thermal insulation performance.
[0011] In a specific embodiment, the weight ratio of the inorganic high temperature fiber material to the nanosol is 1:(5-10).
[0012] By adopting the above technical solution, the ratio of the inorganic high-temperature fiber material to the nanosol is further limited, so that the inorganic high-temperature fiber material can be better dissolved in the nanosol, thereby improving the performance of the obtained insulation material.
[0013] In a specific embodiment, the silica fume is zirconium-containing silica fume.
[0014] By adopting the above technical solution, components such as silicon dioxide and zirconium oxide in the zirconium-containing silica ash can fully react with other compounds to generate a gel that fills the pores of the thermal insulation material, thereby improving the strength of the thermal insulation material; in addition, the zirconium-containing silica ash has good fluidity and can be fully dispersed.
[0015] In a specific embodiment, the sintering agent includes clay.
[0016] In a specific embodiment, the raw material of the high-temperature thermal insulation material further includes 5 to 10 parts by weight of a phase change material, and the phase change material includes a mixture of fatty acids and hydrated salts.
[0017] By adopting the above technical solution, the composite phase change material composed of fatty acid and hydrated salt can further improve the thermal insulation performance of the thermal insulation material.
[0018] In a second aspect, the present application provides a method for preparing a high-temperature thermal insulation material, which adopts the following technical solution: A method for preparing a high-temperature thermal insulation material comprises the following steps: First, add the inorganic high temperature fiber material into the nanosol, stir until it is completely dissolved, then add silica fume, α-alumina powder, sintering agent and other raw materials, continue to stir until it is completely dissolved, and obtain the material; The material is pumped into the mold, and then the vacuum degree is pumped to -0.07-0.08MPa until the material is completely solidified to obtain a green body, which is then dried and machined to obtain a high-temperature thermal insulation material.
[0019] By adopting the above technical solution, the inorganic high-temperature fiber material is first added to the sol, and then silica ash, α-alumina powder, sintering agent and other raw materials are added, stirred to dissolve, and then added to the mold, evacuated to solidify the material, and finally dried to obtain an insulating material with high strength and good thermal insulation performance.
[0020] In a specific embodiment, the drying temperature of the green body is 110-120°C.
[0021] By adopting the above technical solution, the drying temperature of the blank is further limited, so that the thermal insulation material can be better formed.
[0022] In a third aspect, the present application provides a molding device for high-temperature insulation materials, which adopts the following technical solution: A molding device for high-temperature insulation materials comprises a mixing bin, a mold, a filtrate bin, a drying kiln car, and a drying and drying room. The mixing bin is connected with a feed pipe, a water pump is installed on the feed pipe, one end of the feed pipe away from the mixing bin is located in the mold, a filter screen is provided on the filtrate bin, the mold is arranged on the filter screen, a vacuum pump is installed on the filtrate bin, a conveyor belt is provided between the filtrate bin and the drying kiln car, and a bottom plate is provided on the conveyor belt.
[0023] By adopting the above technical scheme, the nano sol is first added into the mixing bin and stirred. During the stirring process, the inorganic high temperature fiber material is added and stirred to dissolve. Then, silica fume, α-alumina powder, sintering agent and other raw materials are added and stirred to dissolve to obtain the material. The water pump is turned on to pump the material in the mixing bin into the mold, the vacuum pump is turned on to vacuumize the material to solidify the material to obtain the green body, and then the mold is removed, the green body is pushed onto the bottom plate, and the green body is transported to the drying kiln car by a conveyor belt. Finally, the green body is transported to the drying and drying room by the drying kiln car, and dried at 110-120°C to obtain the high temperature insulation material.
[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. In this application, nanosol is used as a binder, and inorganic high-temperature fiber materials are combined to form a high-temperature insulation material by vacuum filtration. The pores are small and evenly distributed, so that the high-temperature insulation material has good insulation performance. Due to the addition of inorganic high-temperature fibers, the flexural strength of the material is several times higher than that of the high-temperature insulation material of the same density; at the same time, the high-temperature reburning shrinkage rate of the material is also small, which greatly improves the use scenario of the material and can be directly used as the lining of high-temperature equipment; 2. The method of the present application first adds the inorganic high temperature fiber material to the sol, then adds silica fume, α-alumina powder, sintering agent and other raw materials, stirs and dissolves, then adds to the mold, evacuates to solidify the material, and finally dries to obtain a thermal insulation material with high strength and good thermal insulation performance; 3. The equipment in the present application first adds the nanosol into the mixing bin and stirs it. During the stirring process, the inorganic high-temperature fiber material is added and stirred to dissolve. Then, silica fume, α-alumina powder, sintering agent and other raw materials are added and stirred to dissolve to obtain the material. The water pump is turned on to draw the material in the mixing bin into the mold, and the vacuum pump is turned on to vacuumize the material to solidify the material to obtain a green body. The mold is then removed and the green body is pushed onto the bottom plate. The green body is transported to the drying kiln car by a conveyor belt and finally transported to the drying and drying room by the drying kiln car, and dried at 110-120°C to obtain a high-temperature insulating material. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a structural schematic diagram used to reflect the high-temperature insulation material molding equipment in Example 1 of the present application.
[0026] Explanation of the reference numerals: 1. Mixing bin; 11. Feed pipe; 12. Water pump; 2. Mould; 3. Filtrate bin; 31. Filter screen; 32. Vacuum pump; 4. Drying kiln car; 5. Drying and drying room; 6. Conveyor belt; 7. Bottom plate. DETAILED DESCRIPTION
[0027] The present application is further described in detail below with reference to the embodiments.
[0028] All raw materials in the examples can be obtained from commercial sources, including nano silica sol CAS No.: 14808-60-7; α-alumina powder CAS No.: 1344-28-1. Example
[0029] Example 1 Embodiment 1 provides a molding device for high temperature insulation materials, comprising the following steps: Reference Figure 1 A molding device for high-temperature insulation materials includes a mixing bin 1, a mold 2, a filtrate bin 3, a drying kiln car 4, and a drying and drying room 5. The mixing bin 1 is connected with a feed pipe 11, and a water pump 12 is installed on the feed pipe 11. The end of the feed pipe 11 away from the mixing bin 1 is located in the mold 2. A filter screen 31 is installed on the top wall of the filtrate bin 3, and the filter screen 31 is arranged horizontally. The mold 2 is installed on the top wall of the filter screen 31. A vacuum pump 32 is installed on the side wall of the filtrate bin 3. A conveyor belt 6 is installed between the filtrate bin 3 and the drying kiln car 4, and a bottom plate 7 is placed on the conveyor belt 6.
[0030] Embodiment 1 also provides a method for preparing a high-temperature thermal insulation material, comprising the following steps: A method for preparing a high-temperature thermal insulation material comprises the following steps: First, 150 kg of nano sol is added to the mixing bin 1 and stirred. During the stirring process, 10 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then, 3 kg of silica ash, 70 kg of α-alumina powder and 3 kg of sintering agent are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on to pump the vacuum to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying kiln car 4 by the drying kiln car 4. The green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 110°C, and mechanically processed to obtain a high-temperature insulation material. The nano sol is nano silica sol; the inorganic high-temperature fiber material is alumina fiber; the silica ash is zirconium-containing silica ash; and the sintering agent is clay.
[0031] Example 2 The difference between Example 2 and Example 1 is that 200 kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 20 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then 4 kg of silica ash, 75 kg of α-alumina powder and 4 kg of sintering agent are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on to pump the vacuum to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 110°C, and machined to obtain a high-temperature insulating material. The remaining steps are consistent with Example 1.
[0032] Example 3 The difference between Example 3 and Example 1 is that 175 kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 20 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then 4 kg of silica ash, 75 kg of α-alumina powder and 4 kg of sintering agent are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on to pump the vacuum to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 110°C, and machined to obtain a high-temperature insulating material. The remaining steps are consistent with Example 1.
[0033] Example 4 The difference between Example 4 and Example 1 is that 200 kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 30 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then 5 kg of silica ash, 80 kg of α-alumina powder and 5 kg of sintering agent are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on to pump the vacuum to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 110°C, and machined to obtain a high-temperature insulating material. The remaining steps are consistent with Example 1.
[0034] Example 5 The difference between Example 5 and Example 1 is that 150 kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 30 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then, 5 kg of silica ash, 80 kg of α-alumina powder and 5 kg of sintering agent are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on to pump the vacuum to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 110°C, and machined to obtain a high-temperature insulating material. The remaining steps are consistent with Example 1.
[0035] Example 6 The difference between Example 6 and Example 3 is that 175kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 20kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then, 4kg of silica ash, 75kg of α-alumina powder, 4kg of sintering agent, and 7.5kg of phase change material are added and stirred to dissolve to obtain the material; the water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2, and the vacuum pump 32 is turned on to pump the vacuum to -0.07--0.08MPa to solidify the material to obtain a green body, and then the mold 2 is removed, the green body is pushed onto the bottom plate 7, and the green body is transported to the drying kiln car 4 by the conveyor belt 6, and finally the drying kiln car 4 is used to send it to the drying and drying room 5, dried at 110°C, and mechanically processed to obtain a high-temperature insulation material; wherein the phase change material includes a mixture of fatty acids and hydrated salts, and the weight ratio of fatty acids to hydrated salts is 1:1; the remaining steps are consistent with Example 3.
[0036] Example 7 The difference between Example 7 and Example 6 is that 175 kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 20 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then 4 kg of silica ash, 75 kg of α-alumina powder, 4 kg of sintering agent, and 7.5 kg of phase change material are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on and the vacuum is pumped to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 115°C, and machined to obtain a high-temperature insulating material. The remaining steps are consistent with Example 6.
[0037] Example 8 The difference between Example 8 and Example 6 is that 175 kg of nanosol is first added to the mixing bin 1 and stirred. During the stirring process, 20 kg of inorganic high-temperature fiber material is added and stirred to dissolve. Then 4 kg of silica ash, 75 kg of α-alumina powder, 4 kg of sintering agent, and 7.5 kg of phase change material are added and stirred to dissolve to obtain the material. The water pump 12 is turned on to pump the material in the mixing bin 1 into the mold 2. The vacuum pump 32 is turned on and the vacuum is pumped to -0.07--0.08 MPa to solidify the material to obtain a green body. The mold 2 is then removed and the green body is pushed onto the bottom plate 7. The green body is transported to the drying kiln car 4 by the conveyor belt 6. Finally, the green body is transported to the drying and drying room 5 by the drying kiln car 4, dried at 120°C, and machined to obtain a high-temperature insulating material. The remaining steps are consistent with Example 6.
[0038] Comparative Example Comparative Example 1 Comparative Example 1 provides an alumina hollow ball brick, which is an 85 brick.
[0039] Comparative Example 2 Comparative Example 2 provides an alumina hollow ball brick, which is a 90 brick.
[0040] Comparative Example 3 Comparative Example 3 provides an alumina hollow ball brick, which is a 95 brick.
[0041] Performance testing 1. Thermal insulation performance: The thermal insulation materials in each embodiment and comparative example were tested according to GB / T37796-2019 "Thermal conductivity test method" at a test temperature of 800°C to obtain the thermal conductivity. The lower the thermal conductivity, the better the thermal insulation performance of the material.
[0042] 2. Strength test: The insulation materials in the embodiments and comparative examples were tested in accordance with GB / T5072-2008 “Test method for compressive strength at room temperature” to obtain the compressive strength at room temperature.
[0043] 3. Re-firing line change rate: The insulation materials in the embodiments and comparative examples were tested according to GB / T5988-2007 "Thermal Permanent Line Change Test Method" to obtain the re-firing line change rate at 1600°C × 3H.
[0044] Table 1 Test results of thermal insulation materials In combination with Example 1 and Comparative Examples 1-3, the thermal insulation performance of the thermal insulation material in Example 1 is better and the strength is also higher. It can be seen that by using the preparation method in the present application, nanosol is used as a binder, and inorganic high-temperature fiber material is combined to form a high-temperature thermal insulation material through vacuum filtration. The pores are small and evenly distributed, so that the high-temperature thermal insulation material has better thermal insulation performance. Due to the addition of inorganic high-temperature fibers, the thermal insulation material also has higher strength.
[0045] Combined with Examples 1-5, the thermal insulation performance of the thermal insulation materials in Examples 2-5 is relatively poor. It can be seen that when mixing, when the ratio of inorganic high-temperature fiber material to nanosol in the raw materials is 1: (5-10), the performance of the obtained thermal insulation material is better.
[0046] Combining Example 5 and Example 6, the thermal insulation performance of the thermal insulation material in Example 6 is better. It can be seen that when mixing, adding a phase change material composed of fatty acids and hydrated salts to the raw materials can further improve the thermal insulation performance of the obtained material.
[0047] In combination with Examples 6-8, the thermal insulation material in Example 7 has the best thermal insulation performance and the highest strength. It can be seen that when the green body is dried, the drying temperature of the green body in Example 7 is optimal, thereby obtaining the thermal insulation material with the best thermal insulation performance.
[0048] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high temperature insulation material, characterized in that: The raw materials of the high-temperature insulation material include the following components in parts by weight: 150-200 parts of nanosol, 10-30 parts of inorganic high-temperature fiber material, 3-5 parts of silica fume, 70-80 parts of α-alumina powder, and 3-5 parts of sintering agent.
2. A high temperature insulation material according to claim 1, characterized in that: The nano sol includes nano silica sol.
3. A high temperature insulation material according to claim 1, characterized in that: The inorganic high temperature fiber material includes one of alumina fiber and aluminum silicate fiber or a mixture of the two.
4. A high temperature insulation material according to claim 1, characterized in that: The weight ratio of the inorganic high temperature fiber material to the nano sol is 1:(5-10).
5. A high temperature insulation material according to claim 1, characterized in that: The silica fume is zirconium-containing silica fume.
6. A high temperature insulation material according to claim 1, characterized in that: The sintering agent includes clay.
7. A high temperature insulation material according to claim 1, characterized in that: The raw materials of the high-temperature thermal insulation material also include 5 to 10 parts by weight of a phase change material, and the phase change material includes a mixture of fatty acids and hydrated salts.
8. A method for preparing a high-temperature thermal insulation material according to any one of claims 1 to 7, characterized in that: The following steps are involved: First, add the inorganic high temperature fiber material into the nanosol, stir until it is completely dissolved, then add silica fume, α-alumina powder, sintering agent and other raw materials, continue to stir until it is completely dissolved, and obtain the material; The material is pumped into the mold, and then the vacuum degree is pumped to -0.07-0.08MPa until the material is completely solidified to obtain a green body, which is then dried and machined to obtain a high-temperature thermal insulation material.
9. The method for preparing a high-temperature thermal insulation material according to claim 8, characterized in that: The drying temperature of the green body is 110-120℃.
10. A molding device for a high-temperature insulation material as claimed in any one of claims 1 to 7, characterized in that: The invention comprises a mixing bin (1), a mould (2), a filtrate bin (3), a drying kiln car (4), and a drying and drying room (5); the mixing bin (1) is connected to a feed pipe (11); a water pump (12) is installed on the feed pipe (11); an end of the feed pipe (11) away from the mixing bin (1) is located in the mould (2); a filter screen (31) is provided on the filtrate bin (3); the mould (2) is arranged on the filter screen (31); a vacuum pump (32) is installed on the filtrate bin (3); a conveyor belt (6) is provided between the filtrate bin (3) and the drying kiln car (4); a bottom plate (7) is provided on the conveyor belt (6).