Novel rare earth butadiene rubber as well as preparation method and application thereof
By using disulfide dichloride and aluminum trichloride complexes as branching agents, the problems of gelation and molecular distribution in the preparation of rare earth butadiene rubber were solved, and a new type of rare earth butadiene rubber with excellent properties was prepared, which is suitable for many applications. kind of industrial application.
Patent Information
- Application Number
- CN202411312712.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-09-20
AI Technical Summary
In the prior art, rare earth butadiene rubber has problems such as severe gelation, poor cold flow properties, wide molecular weight distribution, or the branching agent disulfide dichloride and butadiene form cyclic small molecule products during the preparation process.
A carbon tetrachloride solution including disulfide dichloride and aluminum trichloride complexes is used as a branching agent, and through polymerization and branching reactions, new rare earth cisterns with narrow molecular weight distribution width and long-chain branched structure are prepared. Butadiene rubber to avoid gelation and the formation of cyclic small molecule products.
The obtained new type of rare earth butadiene rubber has cold flow resistance, low gel content, and excellent comprehensive properties, and is suitable for use in tires, conveyor belts, and shoemaking fields.
Smart Images

Figure CN118812759A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of rubber synthesis, and in particular to a novel rare earth butadiene rubber and a preparation method and application thereof. Background Art
[0002] Since butadiene is affected by factors such as catalysts and polymerization conditions during the polymerization process, in addition to generating linear macromolecular chains, branched chains of different structural forms are also generated. The branched structure of the polymer molecular chain has a great influence on the performance of the polymer, and its branched structure is mainly closely related to the fluidity and viscoelasticity of the polymer. In addition, different types of branched chains have different effects on physical and mechanical properties. For example, polymers with linear and narrow relative molecular weight distribution are beneficial to the injection molding process, but not conducive to the mixing process. However, a high degree of branching has an adverse effect on the physical properties of the polymer. Therefore, a suitable degree of branching is the key to preparing branched cis-1,1-butadiene rubber. Existing studies have shown that cis-1,1-butadiene rubber synthesized using rare earth catalysts has basically no branched chains and has the characteristics of easy cold flow. However, narrow distribution rare earth cis-1,1-butadiene rubber also requires appropriate long-chain branching to improve processing performance and cold flow. Research on the development of rare earth cis-1,4-butadiene rubber production process shows that when using a neodymium carboxylate catalytic system, polymers with high or low cold flow properties, and adjustable Mooney viscosity and molecular weight distribution can be prepared, depending on the composition of the catalytic system and process conditions. However, when the molecular weight distribution of neodymium-based cis-1,4-butadiene rubber is narrow, it generally has high cold flow properties. In order to reduce the cold flow properties of rare earth cis-1,4-butadiene rubber, researchers in the industry have conducted relevant research on adding modifiers to rare earth cis-1,4-butadiene rubber.
[0003] In the prior art, the invention patent publication number: EP0386808A1 (1990) shows that Enichem uses phosphorus trichloride as a modifier. When the polymerization reaction is carried out to a conversion rate greater than 95%, the sample is taken and the Mooney viscosity is measured to be 28Pa·s; then 0.1% of the modifier phosphorus trichloride is added to the polymer, and the reaction is continued at 110°C for 15 minutes, and then the antioxidant and terminator are added, the solvent is removed and dried, and the Mooney viscosity is measured to be 40Pa·s. The data shows that phosphorus trichloride is an effective modifier, which not only reduces the cold flow property, but also shortens the bonding time between the rubber and carbon black, and also has the effect of increasing the Mooney viscosity. In the invention patent publication (announcement) number: US3374191A (1968), Bayer discovered as early as the 1960s that oxygen-free sulfur chloride can effectively improve the cold flow performance of diene rubber without damaging its processing performance and having no adverse effect on the physical and mechanical properties of the vulcanized rubber. In the invention patent publication (announcement) number: US5567784A (1996), Bayer used this bifunctional sulfur derivative as a branching additive for rare earth cis-1,1-butadiene rubber to improve cold flow and prepare new branched rare earth cis-1,1-butadiene rubber. In the embodiment, the neodymium neodecanoate ternary system and butadiene were polymerized in an adiabatic polymerization manner, the polymerization temperature reached 110°C, the pressure was about 5 to 7 bar, the conversion rate was greater than 99%, and stearic acid and antioxidant were added to terminate the polymerization; then the pressure was reduced to 1.5 bar, the low boiling point components and part of the solvent volatilized, the concentration of the rubber solution increased from 17% to 18%, and S2Cl2 solution was added under stirring, and the reaction was stirred at 110°C for 30 minutes, and then dried according to the usual method. The Mooney viscosity was measured to be 44Pa·s, and the cold flow value was 10mg / min. In the invention patent publication (announcement) number: US8586678B2 (2013), Sullivan et al. described the jump reaction of adding sulfide as follows: the sulfur atom reacts with the double bonds of two macromolecular chains to form a long-chain branched macromolecule, the molecular weight increases, and the Mooney viscosity jumps. However, as a low-temperature vulcanizing agent for rubber, disulfur dichloride has a high chemical reactivity and can react chemically with many inorganic and organic compounds. It is easy to react with hydrocarbons, alcohols, aldehydes, ethers, carboxylic acids, esters, amines, alkenes, etc. It can react violently with unsaturated double bonds, and sulfur and chlorine are respectively connected to the unsaturated bonds. Therefore, when using disulfur dichloride to prepare branched rare earth butadiene rubber, it has a particularly strong gelation tendency, especially in the dispersion process of high-viscosity butadiene rubber, it is very easy to form local gel groups. In the invention patent publication (announcement) number: US3374191A, the amount of disulfur dichloride added is 0.5% of polybutadiene, while in the invention patent publication (announcement) number: US5567784A, 0.05 to 0.5% of polybutadiene needs to be added. As the amount is too high, gelation is easily aggravated. In addition, disulfur dichloride is very easy to form a cyclic small molecule product with the butadiene remaining in the glue.
[0004] Based on this, faced with the technical problems that the rare earth butadiene rubber in the prior art has serious gelation during the preparation process, or has cold flow properties, or has a wide molecular weight distribution, or the branching agent disulfur dichloride is very easy to form cyclic small molecule products with the butadiene residual in the rubber solution, it is urgently needed to provide a new rare earth butadiene rubber and its preparation method to improve the above problems. Summary of the invention
[0005] The main purpose of the present invention is to provide a novel rare earth butadiene rubber and a preparation method and application thereof, so as to solve the technical problems in the prior art that the rare earth butadiene rubber has serious gelation, cold flow, wide molecular weight distribution, or the branching agent disulfur dichloride easily forms cyclic small molecule products with residual butadiene in the rubber solution during the preparation process.
[0006] In order to achieve the above-mentioned object, according to one aspect of the present invention, a method for preparing a novel rare earth butadiene rubber is provided, and the method comprises the following steps: step S1, taking butadiene, an organic solvent and a rare earth catalyst for polymerization reaction to obtain a rubber polymer; step S2, taking a branching agent and carrying out a branching reaction in the rubber polymer, and then adding a terminator to obtain a novel rare earth butadiene rubber; wherein the branching agent comprises a carbon tetrachloride solution of a disulfur dichloride and an aluminum trichloride complex.
[0007] Furthermore, in step S2, in the branching agent, the molar ratio of disulfur dichloride to aluminum chloride is (0.2-1.5):1; in terms of weight percentage, preferably, the weight of carbon tetrachloride accounts for 40-98wt% of the branching agent.
[0008] Furthermore, in step S2, the branching reaction temperature is 20-100°C, and the reaction time is 10-120 min.
[0009] Furthermore, in step S1, the organic solvent is hexane; and the polymerization reaction is preferably carried out under a nitrogen atmosphere.
[0010] Furthermore, in step S1, the rare earth catalyst includes a rare earth compound and an alkyl aluminum, the molar ratio of the rare earth compound to the alkyl aluminum is (0.02-0.25):1, the rare earth compound is selected from one or more of neodymium neodecanoate, neodymium isooctanoate or neodymium phosphate; the alkyl aluminum is a mixture of diisobutylaluminum hydride and diisobutylaluminum chloride, and the molar ratio of diisobutylaluminum hydride to diisobutylaluminum chloride is (4-15):1.
[0011] Furthermore, in step S1, the weight ratio of butadiene to the organic solvent is (0.12-0.30):1 in weight percentage.
[0012] Furthermore, in step S1, the reaction temperature of the polymerization reaction is 20-90° C., and the reaction time is 1-10 h.
[0013] In order to achieve the above object, according to one aspect of the present invention, a new type of rare earth cis-1,4-butadiene rubber is provided. The new type of rare earth cis-1,4-butadiene rubber is obtained by the preparation method of the new type of rare earth cis-1,4-butadiene rubber.
[0014] Furthermore, the content of cis-1,4 structured cis-1,4-butadiene rubber in the new rare earth cis-1,4-butadiene rubber is 95-98%, the Mooney viscosity of the new rare earth cis-1,4-butadiene rubber is 35-80, and the molecular weight distribution width coefficient PDI is 2-3.
[0015] According to another aspect of the present invention, there is provided a novel rare earth butadiene rubber for use in the fields of tires, conveyor belts or shoemaking. The novel rare earth butadiene rubber is the novel rare earth butadiene rubber described above.
[0016] The rare earth butadiene rubber obtained by applying the technical solution of the present invention has the advantages of narrow molecular weight distribution width, long-chain branched structure, cold flow resistance, and low gel content, and has better comprehensive performance and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings herein are incorporated into and constitute a part of the specification, illustrate embodiments consistent with the present application, and together with the specification are used to explain the principles of the present application. In the drawings: Figure 1 The infrared spectrum of rare earth butadiene rubber prepared according to Example 1 of the present invention is shown; Figure 2 The gel permeation chromatogram of the rare earth butadiene rubber prepared according to Example 1 of the present invention is shown; Figure 3 The graph showing the relationship between the intrinsic viscosity and the molecular weight of the rare earth butadiene rubber prepared according to Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0019] According to the background technology of the present invention, the rare earth cis-1,1-butadiene rubber in the prior art has serious gelation, cold flow, wide molecular weight distribution, or the branching agent disulfur dichloride easily forms cyclic small molecule products with the residual butadiene in the rubber solution. Based on this, the present invention provides a method for preparing a novel rare earth cis-1,1-butadiene, an organic solvent, and a rare earth catalyst for polymerization reaction to obtain a rubber polymer; step S2, after a branching agent is taken in the rubber polymer for branching reaction, a terminator is added to obtain a novel rare earth cis-1,1-butadiene rubber; wherein the branching agent includes a carbon tetrachloride solution of disulfur dichloride and an aluminum trichloride complex.
[0020] Based on the technical problems that rare earth cis-1,1-butadiene rubber in the prior art has serious gelation, cold flow, wide molecular weight distribution, or wide molecular weight distribution, or branching agent disulfur dichloride is very easy to form cyclic small molecule products with residual butadiene in the rubber solution due to inappropriate branching degree, wide molecular weight distribution, or inappropriate Mooney viscosity. The present invention provides a method for preparing a novel rare earth cis-1,1-butadiene, an organic solvent, and a rare earth catalyst for polymerization to obtain a rubber polymer; step S2, after taking a branching agent in a rubber polymer for branching reaction, adding a terminator to obtain a novel rare earth cis-1,1-butadiene rubber. In particular, the branching agent provided in the present invention is a carbon tetrachloride solution including disulfur dichloride and an aluminum trichloride complex. On the one hand, it can avoid the problem that disulfur dichloride with high chemical reactivity is used alone as a branching agent in the preparation step of conventional rare earth cis-1,1-butadiene rubber, thereby causing the formation of gel and affecting the reaction process. On the other hand, it can also inhibit the disulfur dichloride from reacting with the residual butadiene in the rubber solution to produce cyclic small molecules, thereby increasing the polymerization reaction conversion rate and optimizing the reaction process. Moreover, the rare earth butadiene rubber prepared by this method has the advantages of narrow molecular weight distribution width, long chain branching structure, cold flow resistance and low gel content, and has better comprehensive performance and broad industrial application prospects.
[0021] In a preferred embodiment, in step S2, in the branching agent, the molar ratio of disulfur dichloride to aluminum chloride is (0.2-1.5):1; in terms of weight percentage, it is further preferred that the amount of carbon tetrachloride added accounts for 40-98wt% of the branching agent; so as to further exert the characteristics of the branching agent and obtain a new rare earth butadiene rubber having a narrow molecular weight distribution width and a long-chain branched structure.
[0022] In order to further prepare a new type of rare earth butadiene rubber with better performance, so that it has the advantages of anti-cold flow properties and low gel content, it is preferred that in step S2, the temperature of the branching reaction is 20~100°C and the reaction time is 10~120min; so that the branching reaction can be fully carried out, the performance of the branched product is improved, and a new type of rare earth butadiene rubber with a narrow molecular weight distribution width and a long-chain branched structure is obtained.
[0023] In a preferred embodiment, in step S1, the organic solvent is hexane, so that the reaction raw materials are fully dissolved in the solvent to obtain a uniform and stable reaction solution, thereby making the polymerization reaction more complete; preferably, the polymerization reaction is carried out under a nitrogen atmosphere to avoid impurities in the air from having an adverse effect on the polymerization reaction product, thereby improving the performance of the new rare earth butadiene rubber.
[0024] In order to further prepare rare earth butadiene rubber having a narrow molecular weight distribution width, a long-chain branched structure, anti-cold flow properties and a low gel content, the rare earth catalyst preferably includes a rare earth compound and an alkyl aluminum, and the molar ratio of the rare earth compound to the alkyl aluminum is preferably (0.02~0.25):1; further preferably, the rare earth compound is selected from one or more of neodymium neodecanoate, neodymium isooctanoate or neodymium phosphate; more preferably, the alkyl aluminum is a mixture of diisobutylaluminum hydride and diisobutylaluminum chloride, and the molar ratio of diisobutylaluminum hydride to diisobutylaluminum chloride is (4~15):1.
[0025] In a preferred embodiment, in step S1, the weight ratio of butadiene to the organic solvent is (0.12-0.30):1, in order to prepare a new type of rare earth butadiene rubber with excellent performance.
[0026] In order to prepare a rubber polymer with excellent performance, and to further prepare a new rare earth butadiene rubber with a narrow molecular weight distribution width and a long-chain branched structure, it is preferred that in step S1, the reaction temperature of the polymerization reaction is 20-90° C., and the reaction time is 1-10 h.
[0027] On the other hand, the present invention also provides a novel rare earth cis-1,4-dione rubber, which is obtained by the preparation method of the novel rare earth cis-1,4-dione rubber. The rare earth cis-1,4-dione rubber has the advantages of narrow molecular weight distribution width, long chain branching structure, cold flow resistance and low gel content, and has excellent comprehensive performance and broad application prospects.
[0028] In a preferred embodiment, the content of cis-1,4 structured cis-1,4-butadiene rubber in the novel rare earth cis-1,4-butadiene rubber is 95-98%; preferably, the Mooney viscosity of the novel rare earth cis-1,4-butadiene rubber is 35-80, and the molecular weight distribution width coefficient PDI thereof is 2-3.
[0029] On the other hand, the present invention also provides a new type of rare earth butadiene rubber for use in the fields of tires, conveyor belts or shoemaking. The new type of rare earth butadiene rubber is the new type of rare earth butadiene rubber mentioned above.
[0030] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0031] Example 1 Under nitrogen protection, 1700g of hexane, 300g of butadiene, 0.56mmol of neodymium neodecanoate, 8.33mmol of diisobutylaluminum hydride, and 1.67mmol of diisobutylaluminum chloride were added to a 5L reactor in sequence, and the polymerization reaction was carried out at 50°C for 4h. A carbon tetrachloride solution of a complex of disulfur dichloride and aluminum trichloride (wherein, disulfur dichloride was 0.060g, aluminum trichloride was 0.059g, and carbon tetrachloride was 2.4g) was added, and the branching reaction was carried out at 50°C for 0.5h. After the branched product was taken out from the polymerization reactor, an ethanol solution of 2,6-di-tert-butyl-p-methylphenol was added to terminate the reaction, and a new rare earth cis-1,4 rubber was obtained. The conversion rate was 98.0%, the polymer cis-1,4 structure content was 98.0%, the Mooney viscosity was 48, the molecular weight distribution width coefficient PDI was 2.06, and the gel content was 0. Figure 1 Its infrared spectrum shows that the cis-structured polymer was successfully synthesized. Figure 2 The GPC spectrum shows that the molecular weight distribution range is relatively narrow. Figure 3 As shown in the relationship diagram between its characteristic viscosity and molecular weight, the viscosity of the new rare earth butadiene rubber increases with the increase of molecular weight. Specifically, the small molecular weight part of the rare earth butadiene rubber with a molecular weight below 100,000 is a linear structure; when the molecular weight is greater than 100,000, a branched structure appears in the molecular chain, and its viscosity is lower than the theoretical viscosity of the linear structure. In addition, the degree of branching increases with the increase of the molecular weight of the polymer chain. This shows that the prepared rare earth butadiene rubber has a branched structure.
[0032] Example 2 The only difference from Example 1 is: 5.56 mmol of diisobutylaluminum hydride and 1.39 mmol of diisobutylaluminum chloride. A new rare earth butadiene rubber was obtained with a conversion rate of 98.0%, a polymer cis-1,4 structure content of 98.0%, a Mooney viscosity of 65, a molecular weight distribution of 2.6, and a gel content of 0.
[0033] Example 3 The only difference from Example 1 is that a carbon tetrachloride solution of a complex of disulfur dichloride and aluminum trichloride (wherein, 0.012 g of disulfur dichloride, 0.060 g of aluminum trichloride, and 1.44 g of carbon tetrachloride) is added to obtain a new rare earth butadiene rubber with a conversion rate of 97.5%, a polymer cis-1,4 structure content of 96.9%, a Mooney viscosity of 53, a molecular weight distribution of 2.6, and a gel content of 0.
[0034] Example 4 The only difference from Example 1 is that a carbon tetrachloride solution of a complex of disulfur dichloride and aluminum trichloride (wherein, 0.024 g of disulfur dichloride, 0.024 g of aluminum trichloride, and 0.24 g of carbon tetrachloride) is added to obtain a new rare earth butadiene rubber with a conversion rate of 96.7%, a polymer cis-1,4 structure content of 97.3%, a Mooney viscosity of 56, a molecular weight distribution of 2.7, and a gel content of 0.
[0035] Example 5 The only difference from Example 1 is that a carbon tetrachloride solution of a complex of disulfur dichloride and aluminum trichloride (wherein, 0.048 g of disulfur dichloride, 0.024 g of aluminum trichloride, and 0.18 g of carbon tetrachloride) is added to obtain a new rare earth butadiene rubber with a conversion rate of 97.5%, a polymer cis-1,4 structure content of 97.7%, a Mooney viscosity of 61, a molecular weight distribution of 2.8, and a gel content of 0.
[0036] Example 6 The only difference from Example 1 is that a carbon tetrachloride solution of a complex of disulfur dichloride and aluminum trichloride (wherein, 0.096 g of disulfur dichloride, 0.048 g of aluminum trichloride, and 0.36 g of carbon tetrachloride) is added to obtain a new rare earth butadiene rubber with a conversion rate of 98.2%, a polymer cis-1,4 structure content of 97.1%, a Mooney viscosity of 72, a molecular weight distribution of 2.9, and a trace amount of gel content.
[0037] Example 7 The only difference from Example 1 is that the branching reaction temperature is 20° C., a new rare earth butadiene rubber is obtained, the conversion rate is 96.5%, the polymer cis-1,4 structure content is 96.3%, the Mooney viscosity is 51, the molecular weight distribution is 2.6, and the gel content is 0.
[0038] Example 8 The only difference from Example 1 is that the branching reaction temperature is 35° C., a new rare earth butadiene rubber is obtained, the conversion rate is 96.4%, the polymer cis-1,4 structure content is 95.8%, the Mooney viscosity is 56, the molecular weight distribution is 2.8, and the gel content is 0.
[0039] Example 9 The only difference from Example 1 is that the branching reaction temperature is 75°C, a new rare earth butadiene rubber is obtained, the conversion rate is 97.1%, the polymer cis-1,4 structure content is 97.5%, the Mooney viscosity is 69, the molecular weight distribution is 2.9, and the gel content is 0.
[0040] Example 10 The only difference from Example 1 is that the branching reaction temperature is 20° C., a new rare earth butadiene rubber is obtained, the conversion rate is 96.5%, the polymer cis-1,4 structure content is 97.9%, the Mooney viscosity is 75, the molecular weight distribution is 3.0, and the gel content is 0.
[0041] Embodiment 11 The only difference from Example 1 is that: 5.00 mmol of diisobutylaluminum hydride and 1.39 mmol of diisobutylaluminum chloride are used to obtain a new rare earth butadiene rubber with a conversion rate of 96.3%, a polymer cis-1,4 structure content of 98.0%, a Mooney viscosity of 85, a molecular weight distribution of 2.9, and a gel content of 0.
[0042] Example 12 The only difference from Example 1 is that: 0.83 mmol of neodymium neodecanoate, 8.34 mmol of diisobutylaluminum hydride, and 1.67 mmol of diisobutylaluminum chloride are polymerized at 35° C. for 6 hours to obtain a new rare earth butadiene rubber with a conversion rate of 96.3%, a polymer cis-1,4 structure content of 95.4%, a Mooney viscosity of 35, a molecular weight distribution of 2.6, and a gel content of 0.
[0043] Comparative Example 1 The difference from Example 1 is that no branching agent is added. The product conversion rate is 96.8%, the polymer cis-1,4 structure content is 96.4%, the Mooney viscosity is 29, the molecular weight distribution is 2.1, and the gel content is 0.
[0044] Comparative Example 2 The difference from Example 2 is that no branching agent was added. The product conversion rate was 96.8%, the polymer cis-1,4 structure content was 97.9%, the Mooney viscosity was 49, the molecular weight distribution was 2.4, and the gel content was 0.
[0045] Comparative Example 3 The difference from Example 3 is that no branching agent is added. The Mooney viscosity is 48 and the molecular weight distribution is 2.4.
[0046] Comparative Example 4 The difference from Example 4 is that no branching agent is added. The Mooney viscosity is 49 and the molecular weight distribution is 2.5.
[0047] Comparative Example 5 The difference from Example 5 is that no branching agent is added. The Mooney viscosity is 47 and the molecular weight distribution is 2.5.
[0048] Comparative Example 6 The difference from Example 6 is that no branching agent is added. The Mooney viscosity is 49 and the molecular weight distribution is 2.4.
[0049] Comparative Example 7 The difference from Example 7 is that no branching agent is added. The Mooney viscosity is 47 and the molecular weight distribution is 2.4.
[0050] Comparative Example 8 The difference from Example 8 is that no branching agent is added. The Mooney viscosity is 49 and the molecular weight distribution is 2.6.
[0051] Comparative Example 9 The difference from Example 9 is that no branching agent is added. The Mooney viscosity is 49 and the molecular weight distribution is 2.4.
[0052] Comparative Example 10 The difference from Example 10 is that no branching agent is added. The Mooney viscosity is 50 and the molecular weight distribution is 2.6.
[0053] Comparative Example 11 The difference from Example 11 is that no branching agent was added. The product conversion rate was 96.5%, the polymer cis-1,4 structure content was 98.1%, the Mooney viscosity was 55, the molecular weight distribution was 2.3, and the gel content was 0.
[0054] Comparative Example 12 The difference from Example 12 is that no branching agent was added. The product conversion rate was 94.7%, the polymer cis-1,4 structure content was 95.5%, the Mooney viscosity was 29, the molecular weight distribution was 2.1, and the gel content was 0.
[0055] Comparative Example 13 The only difference from Example 1 is that the added branching agent is 0.12 g of disulfur dichloride.
[0056] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: According to the embodiments of the present invention and the comparative examples, the polymer cis-1,4 structure content, Mooney viscosity, molecular weight distribution and gel content are tested. It can be found that the cis-1,4 structure content of the polymer before and after branching does not change much; the gel content does not increase significantly, which avoids the conventional technology using disulfur dichloride to prepare branched rare earth cis-1,4 rubber, which has a strong gelation tendency and is very easy to form local gel groups; the Mooney viscosity has a significant jump, which avoids the operation that the rubber solution of rare earth cis-1,4 rubber needs to remove small molecule volatiles before the branching reaction can be carried out, and also avoids the problem that disulfur dichloride is very easy to form cyclic small molecule products with the residual butadiene in the rubber solution and cannot effectively form branched structures.
[0057] In summary, the rare earth butadiene rubber prepared by this method has a narrow molecular weight distribution width, a long-chain branched structure, anti-cold flow properties, and a low gel content. It has excellent comprehensive performance and broad application prospects.
[0058] Although this specification includes many specific implementation details, these should not be interpreted as limiting the scope of any invention or the scope of protection claimed, but are mainly used to describe the features of the specific embodiments of specific inventions. Certain features described in multiple embodiments in this specification may also be implemented in combination in a single embodiment. On the other hand, the various features described in a single embodiment may also be implemented separately in multiple embodiments or in any suitable sub-combination. In addition, although features may work in certain combinations as described above and even initially claim protection, one or more features from the claimed combination may be removed from the combination in some cases, and the claimed combination may point to a sub-combination or a variation of a sub-combination.
[0059] Similarly, although operations are depicted in a particular order in the accompanying drawings, this should not be understood as requiring that these operations be performed in the particular order shown or performed sequentially, or requiring that all illustrated operations be performed to achieve the desired results. In some cases, multitasking and parallel processing may be advantageous. In addition, the separation of various system modules and components in the above-described embodiments should not be understood as requiring such separation in all embodiments, and it should be understood that the described program components and systems can generally be integrated together in a single software product, or packaged into multiple software products.
[0060] Thus, specific embodiments of the subject matter have been described. Other embodiments are within the scope of the appended claims. In some cases, the actions recited in the claims can be performed in a different order and still achieve the desired results. In addition, the processes depicted in the drawings do not necessarily require the particular order or sequential order shown to achieve the desired results. In some implementations, multitasking and parallel processing may be advantageous.
[0061] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0062] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing a novel rare earth butadiene rubber, characterized in that: The preparation method comprises the following steps: Step S1, taking butadiene, an organic solvent and a rare earth catalyst to perform a polymerization reaction to obtain a rubber polymer; Step S2, taking a branching agent and subjecting the rubber polymer to branching reaction, and then adding a terminator to obtain the novel rare earth butadiene rubber; wherein the branching agent comprises a carbon tetrachloride solution of a complex of disulfur dichloride and aluminum trichloride.
2. The method for preparing the novel rare earth butadiene rubber according to claim 1, characterized in that: In the step S2, in the branching agent, the molar ratio of the disulfur dichloride to the aluminum chloride is 0.2-1.5:1; and / or, In terms of weight percentage, the weight of the carbon tetrachloride accounts for 40-98wt% of the branching agent.
3. The method for preparing the novel rare earth butadiene rubber according to claim 1, characterized in that: In the step S2, the branching reaction temperature is 20-100° C., and the reaction time is 10-120 min.
4. The method for preparing the novel rare earth butadiene rubber according to claim 1, characterized in that: In the step S1, the organic solvent is hexane, and the polymerization reaction is carried out under a nitrogen atmosphere.
5. The method for preparing the novel rare earth butadiene rubber according to claim 1, characterized in that: In step S1, the rare earth catalyst includes a rare earth compound and an alkyl aluminum, the rare earth compound is selected from one or more of neodymium neodecanoate, neodymium isooctanoate or neodymium phosphate, the molar ratio of the rare earth compound to the alkyl aluminum is 0.02-0.25:1, the alkyl aluminum is a mixture of diisobutylaluminum hydride and diisobutylaluminum chloride, and the molar ratio of the diisobutylaluminum hydride to the diisobutylaluminum chloride is 4-15:
1.
6. The method for preparing the novel rare earth butadiene rubber according to claim 1, characterized in that: In the step S1, the weight ratio of the butadiene to the organic solvent is 0.12-0.30:1 in weight percentage.
7. The method for preparing the novel rare earth butadiene rubber according to claim 1, characterized in that: In the step S1, the reaction temperature of the polymerization reaction is 20-90° C., and the reaction time is 1-10 hours.
8. A new type of rare earth butadiene rubber, characterized in that: The novel rare earth cis-1,4-dione rubber is a novel rare earth cis-1,4-dione rubber obtained by the preparation method of the novel rare earth cis-1,4-dione rubber according to any one of claims 1 to 7.
9. The novel rare earth butadiene rubber according to claim 8, characterized in that: The content of cis-1,4 structured cis-1,4-butadiene rubber in the novel rare earth cis-1,4-butadiene rubber is 95-98%, the Mooney viscosity of the novel rare earth cis-1,4-butadiene rubber is 35-80, and the molecular weight distribution width coefficient PDI is 2-3.
10. Application of a new type of rare earth butadiene rubber in the field of tires, conveyor belts or shoemaking, characterized in that: The novel rare earth butadiene rubber is the novel rare earth butadiene rubber described in claim 8 or 9.
Citation Information
Patent Citations
Starlike branched polybutadiene of rare earth catalyst system and preparation method thereof
CN102115509A
High-mooney ndbr having mooney jump
CN104395351A
Reaction type ultraviolet light absorber as well as a preparation method and application thereof
CN105348131A
NdBR with molar mass breakdown
CN105764928A
Rare earth catalyst, preparation method and applications thereof
CN110903423A
Cited By
Rare earth catalyst, preparation method and application of rare earth catalyst in rare earth butadiene rubber
CN122255320A