Antistatic hard coating film

By coating the triacetyl cellulose film with an antistatic hard coating composition to form a highly permeable mixed layer, the problems of interference fringes and insufficient adhesion of the triacetyl cellulose film base material are solved, and high temperature and high temperature conditions are achieved. Improved dimensional stability and anti-static properties in wet environments.

CN118812903APending Publication Date: 2024-10-22아티엔스가부시키가이샤 +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410462021.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-17
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

When the existing triacetyl cellulose film is used as a hard coat film substrate, there are problems with interference fringes and insufficient adhesion, especially in high temperature and high humidity environments, resulting in dimensional changes and deformation.

Method used

A hard coating composition containing an antistatic copolymer, a compound having a plurality of ethylenically unsaturated groups, a photopolymerization initiator and a solvent is applied on a triacetyl cellulose film to form a mixed layer, Make the mixed layer occupy more than 65% of the total film thickness of the hard coat and mixed layer to improve the permeability of the substrate and reduce interference fringes.

Benefits of technology

It suppresses interference fringes and improves adhesion, ensuring good dimensional stability and anti-static performance in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812903A_ABST
    Figure CN118812903A_ABST
Patent Text Reader

Abstract

Provided is an antistatic hard coating film which suppresses interference fringes and has excellent adhesion. The technical problem of the present invention is solved by an antistatic hard coating film having a triacetyl cellulose film, a mixed layer, and a hard coating layer, the hard coating layer being formed from a composition for forming an antistatic hard coating layer, the composition for forming the antistatic hard coat layer contains a specific antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E), and the mixed layer is formed by dissolving or swelling a triacetyl cellulose film with the composition. When a cross-section in the thickness direction is observed with a scanning electron microscope, the film thickness ratio of the mixed layer in the total film thickness of the hard coat layer and the mixed layer is 65% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an antistatic hard coating film. Background Art

[0002] In various displays such as liquid crystal displays, plasma displays, EL displays, rear projection displays, and CRT displays used as image display devices for televisions, computers, car navigation systems, vehicle-mounted instrument panels, and mobile phones, hard coating films are used for the purpose of protecting the surfaces of displays and the like (for example, International Publication No. 2007 / 046428).

[0003] Among hard coatings, transparent plastics have excellent properties such as mechanical characteristics, dimensional stability, and electrical insulation, and are therefore widely used as substrates for a variety of applications, including packaging materials such as optical display materials, electrical insulation materials, various photographic materials, and art printing materials.

[0004] Among transparent plastics, triacetyl cellulose (TAC) films are often used in optical display materials such as displays in view of transparency, light refractive index, impact resistance, heat resistance, durability, and the like.

[0005] Generally, a hard coating film is produced by forming a hard coating layer on a triacetylcellulose film as a substrate by coating or printing a resin composition. A cured coating film (hard coating layer) formed of a compound having a (meth)acryloyl group in a molecule that is cured by active energy rays such as ultraviolet rays has a high intrinsic surface resistance value and is prone to static electricity, which may cause problems such as dust adsorption and failures caused by static electricity, and significant loss of productivity.

[0006] In order to solve these problems, attempts have been made to study antistatic hard coating films that impart antistatic properties to films (for example, Japanese Patent Application Laid-Open No. 2011-225796).

[0007] Japanese Patent Application Publication No. 2012-102166 discloses an antistatic coating composition comprising an antistatic copolymer having a quaternary ammonium salt group, a compound having three or more ethylenically unsaturated groups, a photopolymerization initiator, and a solvent selected from alcohols, carbonates, or cyclic ethers. An antistatic hard coating film is also described, which is formed by applying the antistatic coating composition to a substrate to form an antistatic layer with excellent durability.

[0008] On the other hand, in the hard coat film, due to the refractive index difference between the hard coat layer and the triacetyl cellulose as the base film, or the discontinuous change of the refractive index with the interface as the boundary, there is a problem that light reflected on the surface of the hard coat layer interferes with light reflected at the interface between the hard coat layer and the base film, causing interference fringes (rainbow fringes), which deteriorates the visibility of the display and also damages the aesthetics of the display.

[0009] In recent years, as displays have become thinner and lighter, film substrates have also become thinner, and along with this, the level of demand for suppressing interference fringes is increasing.

[0010] Furthermore, since the hard coat film using a triacetylcellulose film as a substrate has a high water vapor permeability, there is a problem that the film absorbs moisture in a high temperature / high humidity environment, causing dimensional changes, deformation, and reduced adhesion.

[0011] An antistatic hard coat film using a triacetylcellulose film as a substrate, which suppresses interference fringes and has excellent adhesion, has not yet been developed. Summary of the invention

[0012] Problem that the invention aims to solve

[0013] In view of the above problems, an object of the present invention is to provide an antistatic hard coat film which suppresses interference fringes and has excellent adhesion.

[0014] Solutions for solving problems

[0015] The inventors of the present invention have conducted intensive studies to solve the above-mentioned problems and have completed the present invention as a result.

[0016] [1]: An antistatic hard coating film comprising a triacetyl cellulose film, a mixed layer, and a hard coating layer,

[0017] The hard coat layer is formed from an antistatic hard coat layer-forming composition, wherein the antistatic hard coat layer-forming composition comprises an antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E).

[0018] The mixed layer is a layer formed by dissolving or swelling the triacetyl cellulose film in the antistatic hard coat layer-forming composition.

[0019] When a cross section of the antistatic hard coating film in the thickness direction is observed with a scanning electron microscope, the ratio of the thickness of the mixed layer to the total thickness of the hard coating layer and the mixed layer is 65% or more.

[0020] The antistatic copolymer (A) is a copolymer having structural units derived from a compound (a-1) and a compound (a-2), wherein the compound (a-1) is a monomer having a quaternary ammonium salt group represented by the following general formula (1), and the compound (a-2) is a monomer having an alkylene oxide chain represented by the following general formula (2).

[0021] General formula (1)

[0022] CH2=C(R 1 )COZ(CH2) k N + (R 2 )(R 3 )R 4 ·X -

[0023] (Where R 1 Indicates H or CH3, R 2 ~R 4 represents a hydrocarbon group having 1 to 9 carbon atoms, Z represents an oxygen atom or an NH group, k represents an integer of 1 to 10, and X ― represents a univalent anion);

[0024] General formula (2)

[0025] CH2=C(R 5 )COO(AO) n R 6

[0026] (Where R 5 Indicates H or CH3, R 6 represents hydrogen or a hydrocarbon group having 1 to 22 carbon atoms, n represents an integer of 2 to 200, and A represents an alkylene group having 2 to 4 carbon atoms).

[0027] [2]: The antistatic hard coat film according to [1], wherein the mass ratio of the compound (C) / solvent (E) is 0.03 to 0.30.

[0028] [3]: The antistatic hard coat film according to [1] or [2], characterized in that the solvent (E) is selected from dimethyl carbonate, ethyl acetate, acetone, methyl ethyl ketone and 1,3-dioxolane.

[0029] [4]: An antistatic hard coat film according to any one of [1] to [3], characterized in that it comprises a compound (c1) having an ethylenically unsaturated group, wherein the mass change value between the mass (X1) and the mass (X2) [(X2) / (X1)] is 1.2 or more, the mass (X1) being the initial mass of a triacetyl cellulose film having a short side of 2 cm × a long side of 4 cm × a thickness of 80 μm, and the mass (X2) being the mass of the triacetyl cellulose film after being immersed in 35 g of the compound (C) having an ethylenically unsaturated group at 25°C for 2 hours.

[0030] [5]: An antistatic hard coat film according to any one of [1] to [4], wherein when a cross section of the antistatic hard coat film in the thickness direction is observed using a scanning electron microscope, the ratio of the film thickness of the mixed layer to the total film thickness of the hard coat layer and the mixed layer is 70% or more.

[0031] Effects of the Invention

[0032] By using the antistatic hard coat-forming composition of the present invention, it is possible to provide an antistatic hard coat film having suppressed interference fringes and excellent adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic cross-sectional view showing an example of the structure of the antistatic hard coat film according to the present embodiment. DETAILED DESCRIPTION

[0034] Hereinafter, preferred embodiments of the present invention will be described. In addition, in this specification, the numerical range specified by "~" includes the numerical values ​​recorded before and after "~" as the range of the lower limit and the upper limit. In addition, in this specification, "film" and "sheet" are not distinguished by thickness. In other words, the "sheet" of this specification includes a thin film-like object, and the "film" of this specification includes a sheet-like object with thickness.

[0035] In addition, in this specification, when "(meth)acrylic acid" is described, it means "acrylic acid or methacrylic acid" unless otherwise specified.

[0036] In addition, the “antistatic hard coat film” is sometimes referred to as the “hard coat film”, the “antistatic hard coating layer” is sometimes referred to as the “hard coating layer”, the “antistatic copolymer (A)” is sometimes referred to as the “copolymer (A)”, the “compound (B) having three or more ethylenically unsaturated groups” is sometimes referred to as the “compound (B)”, the “compound (C) having one ethylenically unsaturated group” is sometimes referred to as the “compound (C)”, and the “compound (c1) having one ethylenically unsaturated group” is sometimes referred to as the “compound (c1)”.

[0037] Unless otherwise specified, various components mentioned in the present specification may be used alone or in combination of two or more.

[0038] 《Antistatic hard coating》

[0039] The antistatic hard coat film of the present invention is a hard coat film comprising a triacetylcellulose film, a mixed layer, and a hard coat layer.

[0040] <Triacetyl cellulose film>

[0041] The triacetyl cellulose film used in the present invention may be of an optically transparent grade that can be used as a substrate for a polarizing plate, etc. The thickness of the triacetyl cellulose film is not particularly limited, but is generally about 10 to 500 μm in terms of strength, workability such as handling, and thinness, and is particularly preferably 20 to 250 μm.

[0042] <Mixed layer>

[0043] The mixed layer is a layer formed by dissolving or swelling the triacetyl cellulose film with the antistatic hard coat forming composition. Furthermore, when observing a cross section of the hard coat film in the thickness direction with a scanning electron microscope, the ratio of the film thickness of the mixed layer to the total film thickness of the hard coat layer and the mixed layer is 65% or more.

[0044] The film thickness ratio is more preferably 67% or more, and further preferably 70% or more. In addition, from the aspect of improving adhesion, it is preferably 90% or less. By making the film thickness ratio of the mixed layer 65% or more, interference fringes can be reduced. From the viewpoint of being conducive to reducing interference fringes, the solution with a high film thickness ratio is preferred.

[0045] <Hard coating>

[0046] The hard coating layer of the present invention is formed by applying an antistatic hard coating layer-forming composition, and curing it by irradiating ultraviolet rays after drying the solvent. The antistatic hard coating layer-forming composition comprises an antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E).

[0047] In order to make the film thickness ratio of the above-mentioned mixed layer more than 65%, it is important to contain a compound (C) having an ethylenically unsaturated group and a solvent (E). When the antistatic hard coat forming composition is applied to the triacetyl cellulose film, the triacetyl cellulose film is eroded by the compound (C) having an ethylenically unsaturated group and the solvent (E), thereby forming a mixed layer. The film thickness ratio of the mixed layer can be controlled by the type of compound (C) and solvent (E), and their content. In particular, in order to easily make the film thickness ratio of the mixed layer more than 65%, it is preferred that the compound (C) is the case of the compound (c1) described later or / and the solvent (E) is the case of the solvent (e1) described later. That is, it is particularly preferred that the compound (C) is the compound (c1) and the solvent (E) is the solvent (e1).

[0048] In addition, the film thickness ratio of the mixed layer can be made greater than 65% by mass by adjusting the nonvolatile component concentration of the antistatic hard coat-forming composition or by using a manufacturing method such as applying the hard coat-forming composition to a triacetylcellulose film and then leaving it to stand to improve substrate permeability (substrate erosion).

[0049] (Antistatic hard coat forming composition)

[0050] The antistatic hard coat layer-forming composition comprises an antistatic copolymer (A), a compound having three or more ethylenically unsaturated groups (B), a compound having one ethylenically unsaturated group (C), a photopolymerization initiator (D), and a solvent (E).

[0051] Furthermore, it is preferred that the compound (C) is a compound having one ethylenically unsaturated group and having a mass change value [(X2) / (X1)] described later of 1.2 or more.

[0052] Furthermore, it is preferred that the solvent (E) has a haze change value [(Y2)-(Y1)] described below of 0.10 or more.

[0053] It is particularly preferred that compound (C) is a compound (c1) having one ethylenically unsaturated group and having a mass change value [(X2) / (X1)] of 1.2 or more, and solvent (E) is a solvent (e1) having a haze change value [(Y2)-(Y1)] of 0.10 or more.

[0054] This improves the permeability of the substrate and effectively reduces interference fringes.

[0055] From the viewpoint of improving substrate permeability, the non-volatile component concentration of the antistatic hard coat forming composition is preferably below 70 mass %, more preferably below 60 mass %. From the viewpoint of suppressing the reduction of the coating haze, the non-volatile component is preferably above 25 mass %, more preferably above 35 mass %. By adjusting the non-volatile component of the antistatic hard coat forming composition, the film thickness ratio of the mixed layer is easily controlled to be above 65 mass %.

[0056] [Antistatic Copolymer (A)]

[0057] The antistatic copolymer (A) has structural units derived from compounds (a-1) and (a-2), and is obtained by free radical copolymerization of a compound (a-3) copolymerizable with the above-mentioned (a-1) and (a-2) in an alcohol solvent as required, wherein the compound (a-1) is a monomer having a quaternary ammonium salt group represented by the following general formula (1), and the compound (a-2) is a monomer having an alkylene oxide chain represented by the following general formula (2).

[0058] General formula (1)

[0059] CH2=C(R 1 )COZ(CH2) k N + (R 2 )(R 3 )R 4 ·X -

[0060] (Where R 1 Indicates H or CH3, R 2 ~R 4 represents a hydrocarbon group having 1 to 9 carbon atoms, Z represents an oxygen atom or an NH group, k represents an integer of 1 to 10, and X ― represents a univalent anion);

[0061] General formula (2)

[0062] CH2=C(R 5 )COO(AO) n R 6

[0063] (Where R 5 Indicates H or CH3, R 6 represents hydrogen or a hydrocarbon group having 1 to 22 carbon atoms, n represents an integer of 2 to 200, and A represents an alkylene group having 2 to 4 carbon atoms).

[0064] <Compound having a quaternary ammonium salt group (a-1)>

[0065] The compound (a-1) having a quaternary ammonium salt group is represented by the above general formula (1). In the general formula (1), R 2 ~R 4 In the case of a hydrocarbon group having 1 to 9 carbon atoms, the hydrocarbon group may be substituted or unsubstituted, preferably an unsubstituted group, preferably an unsubstituted alkyl group. As the unsubstituted alkyl group, either a branched alkyl group or an unbranched alkyl group may be used.

[0066] In R 2 ~R 4 When the number of carbon atoms is greater than 10, the hydrophobicity of the produced antistatic copolymer (A) is high, and as a result, the hygroscopicity of the antistatic layer containing the antistatic copolymer (A) decreases, and good antistatic performance may not be obtained.

[0067] As R of the general formula (1) 2 ~R 4 The unsubstituted alkyl group in is preferably an alkyl group having 1 to 3 carbon atoms, and from the viewpoint of easy availability, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, etc. are preferred.

[0068] The compound (a-1) having a quaternary ammonium salt group can be obtained, for example, by quaternizing (meth)acrylates or (meth)acrylamides having an amino group with a quaternizing agent. Alternatively, commercially available (meth)acrylates or (meth)acrylamides having a quaternary ammonium salt group can be used.

[0069] Examples of (meth)acrylates having an amino group used to form the compound (a-1) having a quaternary ammonium salt group in which Z is an oxygen atom of the general formula (1) include dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, dimethylaminobutyl (meth)acrylate, diethylaminoethyl (meth)acrylate, diethylaminopropyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, dibutylaminoethyl (meth)acrylate, and dihydroxyethylaminoethyl (meth)acrylate.

[0070] Examples of (meth)acrylamides having an amino group for forming the compound (a-1) having a quaternary ammonium salt group in which Z is an NH group of the general formula (1) include dimethylaminoethyl (meth)acrylamide, dimethylaminopropyl (meth)acrylamide, dimethylaminobutyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, diethylaminopropyl (meth)acrylamide, dipropylaminoethyl (meth)acrylamide, dibutylaminoethyl (meth)acrylamide, and dihydroxyethylaminoethyl (meth)acrylamide.

[0071] As the quaternizing agent for quaternizing the above-mentioned (meth)acrylates having an amino group and the above-mentioned (meth)acrylamides having an amino group, various halides such as alkylbenzyl chloride, benzyl chloride, alkyl chloride, alkyl bromide, alkyl sulfates such as dimethyl sulfate, diethyl sulfate, dipropyl sulfate, sulfonates such as methyl p-toluenesulfonate, methyl benzenesulfonate, and alkyl phosphoric acids such as trimethyl phosphate can be used.

[0072] <Compound having an alkylene oxide chain (a-2)>

[0073] Next, the compound (a-2) having an alkylene oxide chain, which is another essential component for forming the antistatic copolymer (A) used in the present invention, will be described.

[0074] The compound (a-2) having an alkylene oxide chain is represented by the general formula (2) and can be obtained by, for example, ring-opening polymerization of ethylene oxide with an alkyl alcohol and then transesterifying it with methyl (meth)acrylate or reacting it with (meth)acryloyl chloride.

[0075] In the above general formula (2), the alkyleneoxy group (AO) is an alkyleneoxy group having 2 to 4 carbon atoms, and examples thereof include ethylene oxide, propylene oxide, and butylene oxide. In addition, alkyleneoxy groups having different carbon atoms may exist in the same monomer.

[0076] The number (n) of alkylene oxide groups is an integer of 2 to 200, preferably an integer of 10 to 100. When the number is less than 2 or 201 or more, sufficient compatibility with the compound (B) having three or more ethylenically unsaturated groups in the molecule described below may not be obtained.

[0077] R 6 It is hydrogen or a hydrocarbon group having 1 to 22 carbon atoms. When the carbon number is 23 or more, the raw material is expensive and thus it is not practical.

[0078] The hydrocarbon group having 1 to 22 carbon atoms may be a substituted or unsubstituted group, preferably an unsubstituted group, preferably an unsubstituted alkyl group. As the unsubstituted alkyl group, either a branched unsubstituted alkyl group or an unbranched unsubstituted alkyl group may be used.

[0079] Specific examples of the compound (a-2) having an alkylene oxide chain include polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polybutylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate, polyethylene glycol mono(meth)acrylate monomethyl ether, polyethylene glycol mono(meth)acrylate monobutyl ether, polyethylene glycol mono(meth)acrylate monooctyl ... Polyethylene glycol mono(meth)acrylate monobenzyl ether, polyethylene glycol mono(meth)acrylate monophenyl ether, polyethylene glycol mono(meth)acrylate monodecyl ether, polyethylene glycol mono(meth)acrylate monododecyl ether, polyethylene glycol mono(meth)acrylate monotetradecyl ether, polyethylene glycol mono(meth)acrylate monohexadecyl ether, polyethylene glycol mono(meth)acrylate monooctadecyl ether, poly(ethylene glycol-propylene glycol) mono(meth)acrylate octyl ether, poly(ethylene glycol-propylene glycol) mono(meth)acrylate octadecyl ether, poly(ethylene glycol-propylene glycol) mono(meth)acrylate nonylphenyl ether, and the like.

[0080] <Compound (a-3) copolymerizable with (a-1) and (a-2)>

[0081] The antistatic copolymer (A) used in the present invention can be obtained by using a compound (a-1) having a quaternary ammonium salt group and a compound (a-2) having an alkylene oxide chain as monomers for copolymerization, and then optionally using a compound (a-3) that can copolymerize with the above (a-1) and (a-2) as a monomer, and obtaining it by free radical copolymerization in an alcohol solvent.

[0082] The compound (a-3) copolymerizable with (a-1) and (a-2) in the present invention is not particularly limited as long as it is a compound having one ethylenically unsaturated group, and examples thereof include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; various (meth)acrylates such as benzyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, butoxyethyl (meth)acrylate, cyanoethyl (meth)acrylate, and glycidyl (meth)acrylate; styrene, methylstyrene, and the like.

[0083] The antistatic copolymer (A) used in the present invention can be obtained by radical copolymerizing the compounds (a-1), (a-2) and the arbitrarily used compound (a-3) in an alcohol solvent.

[0084] Regarding the usage of compounds (a-1), (a-2) and (a-3), in a total of 100% by mass of the radical polymerizable compound, from the viewpoint of antistatic performance, compound (a-1) is preferably 30 to 60% by mass, and from the viewpoint of compatibility with the compound (B) having three or more ethylenically unsaturated groups described later, compound (a-2) is preferably 10 to 50% by mass. Compound (a-3) is used in the range of 0 to 50% by mass as required for the purpose of adjusting the antistatic property, solubility and rigidity of the generated antistatic copolymer (A).

[0085] The antistatic copolymer (A) can be obtained by mixing the compounds (a-1), (a-2) and (a-3) optionally used in the above-mentioned quantitative ratios by a solution polymerization method using a polymerization initiator such as a peroxide-based or azobis-based polymerization initiator.

[0086] The solvent used in the polymerization is not particularly limited as long as it is an alcohol solvent, but it is preferable to use an alcohol solvent selected from methanol, ethanol, isopropanol, n-butanol, isobutanol, cyclohexanol, 2-methoxyethanol, 2-ethoxyethanol, 2-propoxyethanol, 2-butoxyethanol, 1-methoxy-2-propanol, 3-methoxy-1-propanol, 1-ethoxy-2-propanol, 2-ethoxy-1-propanol and 3-ethoxy-1-propanol.

[0087] The amount of the antistatic copolymer (A) is preferably 1 to 20 parts by mass, more preferably 5 to 15 parts by mass, relative to a total of 100 parts by mass of the compound (B) having three or more ethylenically unsaturated groups and the compound (C) having one ethylenically unsaturated group described later. When 1 part by mass or more, sufficient antistatic performance can be obtained, and when 20 parts by mass or less, the adhesion of the hard coat layer formed can be improved.

[0088] [Compound having three or more ethylenically unsaturated groups (B)]

[0089] Next, the compound (B) having three or more ethylenically unsaturated groups used in the antistatic hard coat layer-forming composition of the present invention will be described.

[0090] The compound (B) having three or more ethylenically unsaturated groups is preferably a crosslinking reactive compound having at least three or more (meth)acryloyl groups in the molecule, and may contain an ether bond, a thioether bond, an ester bond, an amide bond, a urethane bond, or the like in the molecule.

[0091] Compound (B) is a compound having three or more ethylenically unsaturated groups. Examples thereof include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, tri(acryloxyethyl)isocyanurate, caprolactone-modified tri(acryloxyethyl)isocyanurate, trimethylolethane tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, alkyl-modified dipentaerythritol tri(meth)acrylate, alkyl-modified dipentaerythritol tetra(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, and the like. Ester compounds of polyols and (meth)acrylic acid such as polyurethane poly(meth)acrylate, polyester poly(meth)acrylate, polyether poly(meth)acrylate, polyacrylic acid poly(meth)acrylate, polyalcohol acid poly(meth)acrylate, polyepoxy poly(meth)acrylate, polyspiroacetal poly(meth)acrylate, polybutadiene poly(meth)acrylate, polythiol polyene poly(meth)acrylate, polysilicon poly(meth)acrylate, etc.; ester compounds synthesized from polyols, polyacids and (meth)acrylic acid, for example, ester compounds synthesized from trimethylolethane / succinic acid / acrylic acid = 2 / 1 / 4 (molar ratio), etc.

[0092] From the aspect of close adhesion, compound (B) is preferably pentaerythritol tri (meth) acrylate, pentaerythritol tetra (meth) acrylate, dipentaerythritol five (meth) acrylate, dipentaerythritol six (meth) acrylate, polyurethane poly (meth) acrylate, polyester poly (meth) acrylate, polyether poly (meth) acrylate, and polyacrylic acid poly (meth) acrylate, more preferably pentaerythritol tri (meth) acrylate, pentaerythritol tetra (meth) acrylate, dipentaerythritol six (meth) acrylate, polyurethane poly (meth) acrylate, and polyester poly (meth) acrylate. These components can be combined arbitrarily. It is particularly preferred to combine polyurethane poly (meth) acrylate with urethane, pentaerythritol poly (meth) acrylate or / and dipentaerythritol poly (meth) acrylate.

[0093] The content of compound (B) in a total of 100% by mass of compound (B) and the compound (C) having one ethylenically unsaturated group described later is preferably 70 to 97% by mass, more preferably 80 to 95% by mass. This range is preferred because it can increase the coating strength and improve the adhesion.

[0094] [Compound (C)]

[0095] Compound (C) is a compound with an ethylenically unsaturated group, and similarly to the organic solvent (E) described later, it has the effect of improving the substrate permeability of the antistatic hard coat forming composition to the triacetyl cellulose film. When the antistatic hard coat forming composition is applied to the triacetyl cellulose film, the triacetyl cellulose film is eroded by the compound (C), so that the antistatic hard coat forming composition is impregnated, the film thickness ratio of the mixed layer can be improved, and interference fringes can be reduced. The organic solvent (E) described later is to play the above-mentioned effect during the period from film coating to drying, relative to this, compound (C) can be considered to be able to play the effect during the period from film coating to ultraviolet irradiation.

[0096] Examples of the compound (C) include ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and 2-(meth)acryloyloxyethyl acid phosphate; and styrene, α-butylene glycol (meth)acrylate, and ester compounds such as ... -methylene and other styrene compounds; silane compounds such as γ-(meth)acryloxypropyltrimethoxysilane and γ-(meth)acryloxypropyltriethoxysilane; nitrogen-containing compounds such as 2-(N,N-dimethylamino)ethyl(meth)acrylate, N-hydroxymethyl(meth)acrylamide, diethyl(meth)acrylamide, N-vinyl-ε-caprolactam and acryloylmorpholine; fluorine-containing compounds such as trifluoroethyl(meth)acrylate and 2,2,3,3,3-pentafluoropropyl(meth)acrylate; polymerizable silicone compounds whose main chain is a silicone component and one end is modified by a (meth)acrylate group.

[0097] From the viewpoint of easily controlling the film thickness ratio of the mixed layer to be above 65%, which is beneficial for reducing interference fringes, the preferred compound (C) is a compound (c1) having a mass change value [(X2) / (X1)] of mass (X1) and mass (X2) of 1.2 or more, wherein mass (X1) is the initial mass of a triacetyl cellulose film having a short side of 2 cm × a long side of 4 cm × a thickness of 80 μm, and mass (X2) is the mass of the triacetyl cellulose film after immersing the triacetyl cellulose film in 35 g of a compound (C) having an ethylenically unsaturated group at 25°C for 2 hours.

[0098] The mass change value [(X2) / (X1)] is more preferably 2.0 to 10.0, and even more preferably 3.0 to 6.0. The compound (C) satisfying this mass change value can improve adhesion and is more advantageous for reducing interference fringes. The more preferred range of [(X2) / (X1)] is 3.5 to 4.5.

[0099] When the mass change value [(X2) / (X1)] of compound (C) is exemplified, it is acryloylmorpholine (3.9), 4-hydroxybutyl acrylate (2.9), tetrahydrofurfuryl acrylate (1.5), N-vinyl-ε-caprolactam (4.3), diethylacrylamide (5.2), lauryl acrylate (1.0), isobornyl acrylate (1.0), and phenoxyethyl acrylate (1.1). As compound (c1), acryloylmorpholine, N-vinyl-ε-caprolactam, diethylacrylamide, etc. are preferably used.

[0100] From the viewpoint of improving the permeability to the substrate and effectively reducing interference fringes, acryloyl morpholine and N-vinyl-ε-caprolactam are more preferred, and acryloyl morpholine is even more preferred.

[0101] The content of compound (C) is preferably 3 to 30% by mass, more preferably 4 to 25% by mass, and further preferably 5 to 20% by mass relative to a total of 100% by mass of compound (B) and compound (C). By making the content of compound (C) 3% or more by mass, the effect of reducing interference fringes based on substrate penetration becomes greater, and by being 30% or less by mass, the coating strength can be improved, and the adhesion is more excellent, so it is preferred.

[0102] [Photopolymerization initiator (D)]

[0103] The photopolymerization initiator (D) is not particularly limited as long as it has the function of initiating free radical polymerization by photoexcitation, and examples thereof include acetophenone compounds, benzoin compounds, benzophenone compounds, phosphine oxide compounds, ketal compounds, anthraquinone compounds, thioxanthone compounds, etc. Specifically, examples thereof include benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diethoxyacetophenone, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, N,N-dimethylaminobenzoic acid isoamyl ester, 2-chlorothioxanthone, 2,4-diethylthioxanthone, etc. In addition, a known organic amine may be added as a sensitizer.

[0104] The amount of the photopolymerization initiator (D) used is preferably 0.1 to 20 parts by mass, more preferably 1 to 15 parts by mass, relative to 100 parts by mass of the total of the compound (B) and the compound (C). 0.1 to 20 parts by mass can provide a sufficient polymerization initiation effect and effectively improve adhesion.

[0105] In the antistatic hard coat layer-forming composition of the present invention, a sensitizer may be used together with the photopolymerization initiator (D).

[0106] Examples of the sensitizer include amine sensitizers, anthracene sensitizers, thioxanthone sensitizers, etc. The sensitizers may be used alone or in combination of two or more.

[0107] Examples of the amine sensitizer include trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate, isoamyl p-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4′-bis(diethylamino)benzophenone.

[0108] Examples of the anthracene-based sensitizer include 9,10-dibutoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, and 9,10-bis(2-ethylhexyloxy)anthracene.

[0109] Thioxanthone sensitizers include, for example, 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, etc. As representative examples of commercial products, EPA (manufactured by Nippon Kayaku Co., Ltd.) can be exemplified in amine sensitizers, DBA and DEA (manufactured by Kawasaki Chemicals Co., Ltd.) can be exemplified in anthracene sensitizers, and DETX and ITX (manufactured by Lambson) can be exemplified in thioxanthone sensitizers.

[0110] The sensitizer is preferably a thioxanthone-based sensitizer or the like.

[0111] When a sensitizer is used, the content thereof is preferably 0.1 to 10 parts by mass based on 100 parts by mass in total of the compound (B) and the compound (C).

[0112] [Solvent (E)]

[0113] Solvent (E) has the effect of improving the base material permeability of antistatic hard coat forming composition to triacetyl cellulose film.When antistatic hard coat forming composition is applied on triacetyl cellulose film, triacetyl cellulose film is eroded by solvent (E), so that antistatic hard coat forming composition is impregnated, the film thickness ratio of mixed layer can be improved, and interference fringes are reduced. That is, solvent (E) brings into play its effect in the stage before solvent volatilization is dried by heating. In addition, when residual solvent (E) in hard coat, film hardness can be reduced and the basic performance of hard coats such as scratch resistance is brought to adverse effect, therefore it is necessary to make solvent (E) dry before ultraviolet irradiation.

[0114] Examples of the solvent (E) include dibutyl ether, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dimethoxyethane, Alkane, 1,3-dioxolane, 1,3,5-trioxane Ethers such as alkanes, tetrahydrofuran, anisole, phenethyl ether, propylene glycol monomethyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone; esters such as ethyl formate, propyl formate, pentyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, dimethyl carbonate, γ-butyrolactone;

[0115] In addition, methyl 2-methoxyacetate, methyl 2-ethoxyacetate, ethyl 2-ethoxyacetate, ethyl 2-ethoxypropionate, ethylene glycol monomethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, 1,2-diacetoxyacetone, acetylacetone, diacetone alcohol, methyl acetoacetate, ethyl acetoacetate, and the like can be mentioned.

[0116] The solvent (E) is preferably a solvent (e1) having a haze change value [(Y2)-(Y1)] of 0.10 or more between the haze value (Y1) and the haze value (Y2), wherein the haze value (Y1) is the initial haze value of a triacetyl cellulose film having a short side of 10 cm×a long side of 10 cm×a thickness of 80 μm, and the haze value (Y2) is the haze value of the triacetyl cellulose film after 0.1 g of the solvent (E) is dropped onto the triacetyl cellulose film at 25° C., the film is allowed to stand for 2 minutes, and then heated at 60° C. for 1 minute. The solvent (e1) is preferred from the viewpoint that the film thickness ratio of the mixed layer can be easily controlled to be 65% or more, which is advantageous for reducing interference fringes.

[0117] The haze change value [(Y2)-(Y1)] is more preferably 0.10 to 0.80, and further preferably 0.11 to 0.40. The solvent (E) satisfying these haze change values ​​can improve substrate permeability without reducing the haze of the coating film, thereby effectively reducing interference fringes.

[0118] When the haze change value [(Y2)-(Y1)] of the solvent (E) is exemplified, it is dimethyl carbonate (0.15), ethyl acetate (0.47), acetone (0.81), methyl ethyl ketone (0.42), 1,3-dioxolane (0.48), methyl isobutyl ketone (0.01), isopropyl alcohol (0.04), and propylene glycol monomethyl ether (0.00). As the solvent (e1), it is preferably selected from dimethyl carbonate, ethyl acetate, acetone, methyl ethyl ketone and 1,3-dioxolane.

[0119] From the viewpoint of being able to effectively suppress a decrease in the haze of the coating film, improving substrate permeability, and effectively reducing interference fringes, dimethyl carbonate, methyl ethyl ketone, 1,3-dioxolane, or ethyl acetate is more preferred, and dimethyl carbonate is even more preferred.

[0120] In 100% by mass of the hard coat-forming composition, the total content of the compound (C) and the solvent (E) is preferably 30 to 80% by mass, more preferably 40 to 70% by mass. When it is 30% by mass or more, the adhesion can be further improved by improving the substrate permeability, and when it is 80% by mass or less, the substrate permeability will not be too high, and the deterioration of the coating haze can be further suppressed.

[0121] The mass ratio of compound (C) / solvent (E) is preferably 0.03 to 0.30, more preferably 0.05 to 0.20. When it is 0.03 or more, the adhesion can be improved, and when it is 0.30 or less, sufficient substrate permeability can be ensured, so the effect of reducing interference fringes is further improved.

[0122] The antistatic hard coat layer-forming composition of the present invention may contain other additives as required. Examples of other additives include plasticizers, surface conditioners, light stabilizers, antioxidants, and polymerization inhibitors.

[0123] <Manufacturing of antistatic hard coat film>

[0124] The method for producing the antistatic hard coat film is not particularly limited and can be produced by a conventionally known method such as coating a triacetylcellulose film with a composition for forming an antistatic hard coat layer.

[0125] For example, after applying the antistatic hard coat-forming composition of the present invention on a triacetyl cellulose film, the solvent is dried as needed, and then the antistatic hard coat-forming composition after application is crosslinked and cured by irradiating the position with active energy rays, thereby obtaining an antistatic hard coat film having a triacetyl cellulose film, a mixed layer, and a hard coat layer.

[0126] Thereby, an antistatic hard coat film can be obtained in which, when a cross section of the antistatic hard coat film is observed with a scanning electron microscope, the ratio of the thickness of the mixed layer to the total thickness of the hard coat layer and the mixed layer is 65% or more.

[0127] Furthermore, it is preferred that the antistatic hard coat layer-forming composition is applied onto a triacetylcellulose film and left to stand because the substrate permeability can be improved and the film thickness ratio of the mixed layer can be easily set to 65% by mass or more.

[0128] Examples of the coating method include bar coating, blade coating, spin coating, reverse coating, die coating, spray coating, roll coating, gravure coating, micro gravure coating, lip coating, air knife coating, and dipping.

[0129] As the active energy ray, electron beams can be used, or ultraviolet rays emitted from a light source such as a xenon lamp, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultrahigh-pressure mercury lamp, a metal halide lamp, a carbon arc lamp, or a tungsten lamp can be used.

[0130] The thickness of the hard coating layer is not particularly limited as long as the hard coating property can be maintained, and is usually 1 to 20 μm, preferably 2 to 15 μm. The total thickness of the hard coating layer and the mixed layer is also not particularly limited, but in order to reduce interference fringes, it is preferably 0.5 to 100 μm, more preferably 1.1 to 30 μm, and further preferably 1.2 to 25 μm.

[0131] The film thickness of the hard coating film is not particularly limited, but is preferably 50 to 300 μm, more preferably 81 to 100 μm, and further preferably 82 to 95 μm.

[0132] [Example]

[0133] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. In addition, unless otherwise specified, "part" means "part by mass" and "%" means "% by mass".

[0134] The amounts in the tables are parts by mass and are converted to non-volatile components excluding the solvent. A blank column in the table indicates that no content is added.

[0135] <Mass change value of compound (C) [(X2) / (X1)]>

[0136] The mass change value [(X2) / (X1)] of the compound (C) was determined by the following method.

[0137] First, the initial mass (X1) of a triacetyl cellulose film having a short side of 2 cm × a long side of 4 cm × a thickness of 80 μm is measured. Next, the triacetyl cellulose film is immersed in 35 g of a compound (C) having one ethylenically unsaturated group at 25°C for 2 hours. After that, the triacetyl cellulose film is taken out, and after being gently wiped with a wipe paper (Kimtowel), the mass (X2) of the triacetyl cellulose film is measured. In addition, as the triacetyl cellulose film, a triacetyl cellulose film having a thickness of 80 μm (manufactured by Fujifilm Corporation) is used (this film is also used in the haze measurement described later).

[0138] <Haze change value of solvent (E) [(Y2)-(Y1)]>

[0139] The haze change value [(Y2) - (Y1)] of the solvent (E) is determined by the following method.

[0140] First, the initial haze value (Y1) of a triacetyl cellulose film with a short side of 10 cm × a long side of 10 cm × a thickness of 80 μm was determined. Next, 0.1 g of a solvent (E) was added dropwise to the triacetyl cellulose film at 25°C and allowed to stand for 2 minutes. Thereafter, the triacetyl cellulose film was heated at 60°C for 1 minute and the haze value (Y2) of the triacetyl cellulose film was measured after returning to room temperature.

[0141] (synthesis example)

[0142] (Production of Compound (a-2) Having an Alkylene Oxide Chain)

[0143] 511.7 parts of stearyl alcohol, 752.9 parts of toluene, and 2 parts of potassium hydroxide were added to an autoclave equipped with a stirrer, a thermometer, an alkylene oxide inlet, and a nitrogen inlet. Next, the system was replaced with nitrogen and the pressure in the reaction vessel was 8 kgf / cm 2 Then, ethylene oxide in an amount of 30 times the mole of stearyl alcohol was injected under pressure at a temperature of 90° C. or less over 4 hours, and the mixture was reacted at 90° C. for 5 hours.

[0144] Next, air was passed to remove unreacted ethylene oxide, and then 42.0 parts of KYOWAAD600 (adsorption aid of alkali (earth) metal hydroxide) manufactured by Kyowa Chemical Industry Co., Ltd. was added, and the mixture was treated under dry air conditions of 5 kPa and 30° C. for 2 hours, followed by filtration. Toluene was removed from the obtained filtrate by heating and reducing pressure to obtain polyethylene oxide addition alcohol.

[0145] 317.7 parts of the obtained polyethylene oxide addition alcohol were transferred to a flask equipped with a stirring device, a thermometer, an air introduction tube, a liquid addition pipeline and a distillation tower, and 200 parts of methyl methacrylate (10 times the mole of the polyethylene oxide addition alcohol) and 0.04 parts of hydroquinone monomethyl ether were added, and heated to 80°C while blowing dry air. After that, 0.2 parts of tetraisopropyl orthotitanate were added every 1 hour to carry out an ester exchange reaction. During the reaction, methanol and methyl methacrylate generated as by-products were distilled out of the reaction system in the form of an azeotropic mixture as needed. After 4 hours, the reaction was terminated when the alcohol conversion rate reached 95%.

[0146] The obtained solution was cooled, washed with water, dehydrated, concentrated, and filtered to obtain a compound (a-2) having 30 ethylene oxide groups and an octadecyl group.

[0147] In addition, the number of alkylene oxide groups is represented by the molar ratio (theoretical value) of the alkylene oxide and the alcohol used in the alkylene oxide addition step.

[0148] <Production of antistatic copolymer (A) (copolymerization process)>

[0149] 30 parts of the above-synthesized (a-2), 50 parts of methacryloyloxyethyltrimethylammonium chloride, 20 parts of cyclohexyl methacrylate, 1.5 parts of azobisisobutyronitrile, and 233 parts of ethanol were added to a flask having a stirring blade, a reflux cooler, and a gas inlet, and reacted at 70° C. for 8 hours under a nitrogen stream. After the reaction was completed, the mixture was cooled to obtain an ethanol solution of an antistatic copolymer (A) (solid content 30% by weight).

[0150] The components used in Table 1 are as follows.

[0151] <Quaternary ammonium salt>

[0152] ·DQ-100: Dimethylaminoethyl methacrylate quaternary ammonium compound (manufactured by Kyoeisha Chemical Co., Ltd.: Lightester DQ-100)

[0153] <Compound having three or more ethylenically unsaturated groups (B)>

[0154] UA-306H: (manufactured by Kyoeisha Chemical Co., Ltd.: hexafunctional urethane acrylate)

[0155] · M405: dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd.: ARONIX M405, hexafunctional monomer)

[0156] ·PET30: Pentaerythritol triacrylate (manufactured by Nippon Kayaku Co., Ltd.: KAYARAD PET30, trifunctional monomer)

[0157] <Compound having one ethylenically unsaturated group (C)>

[0158] It should be noted that the numerical value in the brackets is the mass change value [(X2) / (X1)].

[0159] [Compound (c1)]

[0160] ·ACMO: Acryloylmorpholine (manufactured by KJ Chemical Co., Ltd.: ACMO, monofunctional monomer, 3.9)

[0161] 4-HBA: 4-hydroxybutyl acrylate (Mitsubishi Chemical Corporation: 4HBA, monofunctional monomer, 2.9),

[0162] ·THF-A: Tetrahydrofurfuryl acrylate (manufactured by Kyoeisha Chemical Co., Ltd.: Light acrylate THF-A, monofunctional monomer, 1.5)

[0163] NVP: N-vinyl caprolactam (made by Ashland: V-Cap / RC, monofunctional monomer, 4.3)

[0164] ·DEAA: diethylacrylamide (manufactured by KJ Chemical Co., Ltd.: DEAA, monofunctional monomer, 5.2)

[0165] [Others (other compounds having one ethylenically unsaturated group)]

[0166] LA: Lauryl acrylate (manufactured by Kyoeisha Chemical Co., Ltd.: Light acrylate LA, monofunctional monomer, 1.0)

[0167] IBXA: Isobornyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.: IBXA, monofunctional monomer, 1.0)

[0168] ·PEA: Phenoxyethyl acrylate (manufactured by Kyoeisha Chemical Co., Ltd.: Light acrylate PO-A, monofunctional monomer, 1.1)

[0169] <Photopolymerization initiator (D)>

[0170] · APO: diphenyl-2,4,6-trimethylbenzoylphosphine oxide (manufactured by Daido Chemical Industry Co., Ltd.: DAIDOUV-CURE APO)

[0171] <Solvent (E)>

[0172] It should be noted that the numerical value in the brackets is the haze change value [(Y2)-(Y1)].

[0173] [Solvent (e1)]

[0174] ·DMC: dimethyl carbonate (manufactured by Ube Kosan Co., Ltd., 0.15)

[0175] ·Ethyl acetate (manufactured by Daicel Corporation, 0.47)

[0176] Acetone (Mitsubishi Chemical Corporation, 0.81)

[0177] ·MEK: Methyl ethyl ketone (manufactured by Maruzen Petrochemical Co., Ltd., 0.42)

[0178] 1,3-Dioxolane (manufactured by Toho Chemical Industry Co., Ltd., 0.48)

[0179] [Others (other solvents)]

[0180] MIBK: methyl isobutyl ketone (manufactured by Mitsubishi Chemical Corporation, 0.01)

[0181] ·IPA: Isopropyl alcohol (manufactured by Kishida Chemical Co., Ltd., 0.04)

[0182] ·PGM: Propylene glycol monomethyl ether (manufactured by Daishin Chemical Co., Ltd., 0.00)

[0183] EtOH: ethanol (from antistatic copolymer (A), 0.01)

[0184] <Example 1>

[0185] The ethanol solution of the antistatic copolymer (A) prepared in the synthesis example was added so that the solid content of the antistatic copolymer was 10 parts by mass, and as the compound (B), 50 parts of a urethane prepolymer having as a main component an adduct of pentaerythritol triacrylate and hexamethylene diisocyanate in a ratio of 2:1 (UA-306H, hexafunctional urethane acrylate, manufactured by Kyoeisha Chemical Co., Ltd.), 30 parts of dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd.) Co., Ltd.: ARONIX M405, a hexafunctional monomer), 10 parts of pentaerythritol triacrylate (manufactured by Nippon Kayaku Co., Ltd.: KAYARADPET30, a trifunctional monomer), 10 parts of acryloylmorpholine (manufactured by KJ Chemical Co., Ltd.: ACMO, a monofunctional monomer) as a compound (C), 3 parts of diphenyl-2,4,6-trimethylbenzoylphosphine oxide (manufactured by Daido Chemical Industry Co., Ltd.: DAIDO UV-CURE APO) as a photopolymerization initiator (D), and 428.7 parts of dimethyl carbonate (manufactured by Ube Industries, Ltd.: DMC) as a solvent (E) were mixed to obtain a composition for forming an antistatic hard coat layer.

[0186] Next, the antistatic hard coating composition was applied on a triacetyl cellulose film (manufactured by Fujifilm Corporation) having a thickness of 80 μm at 25°C and a relative humidity of 50% using a No. 10 rod coater, and dried in a hot air oven for 1 minute. Afterwards, ultraviolet rays were irradiated with a high-pressure mercury lamp having an output power of 80 w / cm to cure the coating layer, thereby obtaining an antistatic hard coating film having a triacetyl cellulose film, a mixed layer, and a hard coating layer. The total film thickness of the hard coating layer and the mixed layer was 9.3 μm, and the film thickness of the hard coating film was 87.0 μm. In addition, the film thickness ratio of the above-mentioned mixed layer in the total film thickness of the hard coating layer and the mixed layer was 71.4%.

[0187] <Examples 2 to 36, Comparative Examples 1 to 3>

[0188] As shown in Tables 1 to 4, except for changing the composition and the blending amount (parts by mass), the antistatic hard coat-forming compositions of Examples 2 to 36 and Comparative Examples 1 to 3 were prepared in the same manner as in Example 1 to obtain antistatic hard coat films. The total film thickness of the hard coat layer and the mixed layer of the obtained antistatic hard coat films, the film thickness of the hard coat film, and the film thickness ratio of the mixed layer in the total film thickness of the hard coat layer and the mixed layer are shown in Tables 1 to 4.

[0189] [Evaluation] The antistatic hard coating films obtained in each example and comparative example were measured and evaluated by the following methods. The results are shown in Tables 1 to 4.

[0190] [Thickness ratio of mixed layer]

[0191] The cross section of the obtained antistatic hard coating film in the thickness direction was cut several times with a diamond knife using an ultramicrotome (manufactured by Leica Microsystems, model: EMUC7) to make it smooth, and then the cross section was observed using a scanning electron microscope (manufactured by JEOL Ltd., model: JSM-7800F) at a voltage of 5 kV. The film thickness ratio of the mixed layer was calculated according to the following formula.

[0192] Mixed layer thickness ratio (%) = mixed layer thickness (μm) / (hard coat layer thickness (μm) + mixed layer thickness (μm)) × 100

[0193] [Thickness of antistatic hard coating]

[0194] The film thickness (μm) of the obtained antistatic hard coat film was measured using a digital microscope (manufactured by Nikon Corporation, model: MH-15M).

[0195] [Adhesion]

[0196] The obtained antistatic hard coating film was used to perform a tape adhesion test. The tape adhesion test was performed in accordance with JIS K5600.

[0197] The cutter was cut into the antistatic hard coating film to a depth that reached the substrate (TAC film) but did not cut it, and to form 10 grids × 10 grids with a width of 1 mm at intervals, a total of 100 grids. After a transparent tape (25 mm wide, manufactured by Michelbon Co., Ltd.) was attached to the coating surface, the transparent tape was quickly peeled off by hand to evaluate the state of the remaining grids.

[0198] Evaluation benchmark

[0199] +++: No peeling (very good).

[0200] ++: The end of the grid is slightly chipped (good).

[0201] +: 1 to 5 grids of peeling were observed (no problem in practical use).

[0202] NG: 6 or more peelings were observed (not practically applicable).

[0203] [Interference fringes]

[0204] The obtained antistatic hard coating film was cut into 5 cm × 5 cm, and the surface of the TAC substrate on the opposite side of the coating surface was rubbed back and forth about 10 times with paper or a file to make the surface smooth, and then black matte paint was dripped and dried at 70°C for 2 minutes. The 5° absolute reflectivity was measured using a spectrophotometer (manufactured by Hitachi High-Technologies Co., Ltd., model: U-4100), and the reflection curve was observed for ripples.

[0205] Evaluation benchmark

[0206] +++: No moire was observed (very good).

[0207] ++: The above criteria were not achieved. Almost no waviness was observed (good).

[0208] +: The above criteria are not met. Moire is slightly observed (no problem in practical use).

[0209] NG: The above criteria were not met. Waves were observed (not practically applicable).

[0210] [Antistatic properties]

[0211] The obtained antistatic hard coat film was allowed to stand for 24 hours at 25°C and a relative humidity of 50%. Then, a surface resistivity (Ω / □) was measured after 1 minute at a voltage of 100 V under the conditions of a temperature of 25°C and a relative humidity of 50% using a surface resistivity meter manufactured by HIOKI (SM-8000 series SME-8310).

[0212] Evaluation benchmark

[0213] +++: less than 1.0E+09Ω / □ (very good).

[0214] ++: 1.0E+09Ω / □ or more and less than 1.0E+10Ω / □ (good).

[0215] +: 1.0E+10Ω / □ or more and less than 1.0E+11Ω / □ (no problem in actual application).

[0216] NG: 1.0E+11Ω / □ or more (cannot be used in practice).

[0217] [Table 1]

[0218]

[0219] [Table 2]

[0220]

[0221] [Table 3]

[0222]

[0223] [Table 4]

[0224] Table 4

[0225]

[0226] From the results of Tables 1 to 4, it can be confirmed that, by the antistatic hard coating film of the present invention in which the ratio of the film thickness of the mixed layer in the total film thickness of the hard coating layer and the mixed layer formed from the antistatic hard coating layer-forming composition comprising the antistatic copolymer (A), the compound having three or more ethylenically unsaturated groups (B), the compound having one ethylenically unsaturated group (C), the photopolymerization initiator (D), and the solvent (E) is 65% or more, an antistatic hard coating film having suppressed interference fringes and excellent adhesion can be obtained.

[0227] Description of Reference Numerals

[0228] 1: triacetyl cellulose film;

[0229] 2: Mixed layer;

[0230] 3: Hard coating.

Claims

1. An antistatic hard coating film comprising a triacetyl cellulose film, a mixed layer, and a hard coating layer, The hard coating layer is formed from an antistatic hard coating layer-forming composition, wherein the antistatic hard coating layer-forming composition comprises an antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E), The mixed layer is a layer formed by dissolving or swelling the triacetyl cellulose film with the antistatic hard coat layer-forming composition. When a cross section of the antistatic hard coating film in the thickness direction is observed with a scanning electron microscope, the ratio of the thickness of the mixed layer to the total thickness of the hard coating layer and the mixed layer is 65% or more. The antistatic copolymer (A) is a copolymer having structural units derived from a compound (a-1) and a compound (a-2), wherein the compound (a-1) is a monomer having a quaternary ammonium salt group represented by the following general formula (1), and the compound (a-2) is a monomer having an alkylene oxide chain represented by the following general formula (2). General formula (1) CH2=C(R 1 )COZ(CH2) k N + (R 2 )(R 3 )R 4 ·X - (Where R 1 Indicates H or CH3, R 2 ~R 4 represents a hydrocarbon group having 1 to 9 carbon atoms, Z represents an oxygen atom or an NH group, k represents an integer of 1 to 10, and X ― represents a univalent anion); General formula (2) CH2=C(R 5 )COO(AO) n R 6 (Where R 5 Indicates H or CH3, R 6 represents hydrogen or a hydrocarbon group having 1 to 22 carbon atoms, n represents an integer of 2 to 200, and A represents an alkylene group having 2 to 4 carbon atoms).

2. The antistatic hard coating film according to claim 1, wherein The mass ratio of compound (C) / solvent (E) is 0.03 to 0.

30.

3. The antistatic hard coating according to claim 1 or 2, characterized in that: The solvent (E) is selected from the group consisting of dimethyl carbonate, ethyl acetate, acetone, methyl ethyl ketone and 1,3-dioxolane.

4. The antistatic hard coating film according to claim 3, characterized in that: A compound (c1) having an ethylenically unsaturated group, wherein the mass change value between the mass (X1) and the mass (X2) [(X2) / (X1)] is 1.2 or more, wherein the mass (X1) is the initial mass of a triacetyl cellulose film having a short side of 2 cm × a long side of 4 cm × a thickness of 80 μm, and the mass (X2) is the mass of the triacetyl cellulose film after immersing the triacetyl cellulose film in 35 g of the compound (C) having an ethylenically unsaturated group at 25° C. for 2 hours.

5. The antistatic hard coating film according to claim 1 or 2, wherein When a cross section of the antistatic hard coat film in the thickness direction is observed with a scanning electron microscope, the ratio of the thickness of the mixed layer to the total thickness of the hard coat layer and the mixed layer is 70% or more.

Citation Information

Patent Citations

  • Antistatic coating composition

    JP2011225796A

  • Antistatic coating composition

    JP2012102166A

  • Curable composition, cured layer thereof and multilayer body

    WO2007046428A1