Anti-skid wear-resistant sole processing technology

By using the smelting and vulcanization treatment of styrene-butadiene rubber, modified graphene and modified ABS masterbatch in the sole processing technology, combined with the application of white carbon black and anti-skid particles, the problem of insufficient anti-skid and wear resistance of existing rubber soles is solved. , significantly improving the hardness and anti-slip performance of the soles.

CN118812907APending Publication Date: 2024-10-22WENZHOU LIBUDA SHOES IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310407546.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing rubber soles have poor anti-slip and wear resistance and cannot meet the usage requirements.

Method used

A non-slip and wear-resistant shoe sole processing technology is adopted. After smelting styrene-butadiene rubber, modified graphene and modified ABS masterbatch in a smelting machine, white carbon black, ethyl hydrogen-containing silicone oil, epoxy propylene ether and catalyst are added. Mix and stir, then add rubber softening oil, heat stabilizer and vulcanizing agent, mix and add foaming agent and wear-resistant agent, and finally vulcanize and mold in a vulcanizer, and spray anti-skid particles on the surface of the sole.

Benefits of technology

The hardness, toughness and anti-slip performance of the soles are improved, the mechanical properties of the rubber are enhanced through the combination of modified ABS and graphene, and the surface roughness is increased through anti-slip particles, which significantly improves the anti-slip performance of the soles.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of sole manufacturing, in particular to an anti-skid wear-resistant sole processing technology which comprises the following steps: S1, weighing butadiene styrene rubber, modified graphene and modified ABS (acrylonitrile butadiene styrene) master batch according to a proportion, putting into a smelting machine for smelting, and filtering an obtained solution after the butadiene styrene rubber, the modified graphene and the modified ABS master batch are completely molten to obtain a filter cake; then white carbon black, ethyl hydrogen-containing silicone oil, epoxy propylene ether and a salt catalyst are added into the solution for primary mixing and stirring, then a basic catalyst is added into the solution for secondary mixing and stirring, and a mixed solution is obtained; s2, the mixed solution is placed in a storage tank, it is guaranteed that the mixed solution is in a liquid state all the time, after heat preservation and standing are conducted, rubber softening oil, a heat stabilizer and a vulcanizing agent are put into the mixed solution to be stirred to be uniform, then the mixture is fed into a mixing mill to be mixed for 5-10 min at the temperature of 100-120 DEG C, then a foaming agent and a wear-resisting agent are added, mixing continues to be conducted for 4-6 min at the temperature of 100-120 DEG C, and pouring liquid is obtained; the rubber sole can effectively solve the problems that an existing rubber sole is poor in anti-skid and wear-resistant performance and cannot meet the use requirement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sole manufacturing, in particular to a process for processing anti-skid and wear-resistant soles. Background Art

[0002] Rubber is a commonly used material for making soles, but the existing rubber soles have poor anti-skid and wear-resistant properties and cannot meet the use requirements.

[0003] Therefore, a non-slip and wear-resistant sole processing technology is needed to solve the problems raised in the above background technology. Summary of the invention

[0004] The purpose of the present invention is to provide a non-slip and wear-resistant sole processing technology to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A process for processing a non-slip and wear-resistant sole comprises the following steps:

[0007] S1, weighing styrene-butadiene rubber, modified graphene and modified ABS masterbatch in proportion and putting them into a melting machine for melting, filtering the obtained solution after they are completely melted, and then adding white carbon black, ethyl hydrogen silicone oil, epoxy propylene ether and salt catalyst into the solution for mixing and stirring once, and then adding alkaline catalyst into the solution for secondary mixing and stirring to obtain a mixed solution;

[0008] S2, placing the mixed liquid in a storage tank to ensure that the mixed liquid is always in a liquid state, keeping it warm and standing, adding rubber softening oil, heat stabilizer and vulcanizing agent into the mixed liquid and stirring it evenly, then sending it into a mixer, mixing it at 100-120°C for 5-10min, then adding a foaming agent and a wear-resistant agent, and continuing to mix it at 100-120°C for 4-6min to obtain a casting liquid;

[0009] S3, select a sole mold, clean and preheat the sole mold, then evenly spray a demoulding liquid into the sole mold, evenly pour a pouring liquid into the sole mold, after pouring, evenly spray anti-skid particles on the surface of the pouring liquid, send it into a vulcanizer for vulcanization and molding, take it out after vulcanization and wait for it to return to room temperature, then demould it to obtain an anti-skid and wear-resistant sole.

[0010] As a preferred solution of the present invention, the mass ratio of styrene-butadiene rubber, modified graphene and modified ABS masterbatch in S1 is 10:8:3, the melting temperature of the melting machine is 400-550°C, the temperature of the first mixing and stirring is 200-350°C, the first mixing and stirring time is 20-26min, the temperature of the second mixing and stirring is 380-420°C, and the second mixing and stirring time is 35-48min, the salt catalyst is prepared by mixing palladium chloride and copper fluoride in a mass ratio of 1:1, and the base catalyst is triethylamine.

[0011] As a preferred scheme of the present invention, the insulation temperature in S2 is 180-200°C, the insulation time is 30-45min, the wear-resistant agent is made of titanium carbonitride fine powder, silicone oil and EVA mixed in a weight ratio of 2:1:4, the heat stabilizer is polyvinyl pyrrolidone, the vulcanizer is N,N'-m-phenylene bismaleimide, and the foaming agent is AC foaming agent. The mass ratio of the mixed liquid, rubber softening oil, heat stabilizer, vulcanizer, foaming agent and wear-resistant agent is 15:5:2:3:4:7.

[0012] As a preferred solution of the present invention, the preheating temperature of the sole mold in S3 is 80-140°C, the preheating time is 45-60s, the casting liquid is poured into the sole mold at one time, and the sole mold is quickly cooled after the casting is completed, the demoulding liquid is paraffin, the vulcanization temperature of the vulcanizer is 140-180°C, and the vulcanization time is 3-5min.

[0013] As a preferred scheme of the present invention, the preparation method of the modified graphene includes the following steps: putting graphene into deionized water, shaking and then ultrasonically dispersing it, heating it to 80°C and adding γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), filtering and washing to obtain graphene oxide, mixing and stirring the graphene oxide with natural rubber latex, ultrasonically treating it again, mixing and stirring it with acetic acid solution after the treatment, flocculating and settling it, filtering and drying it to obtain the modified graphene.

[0014] As a preferred solution of the present invention, the preparation method of the modified ABS masterbatch comprises the following steps: styrene, acrylonitrile, glycidyl methacrylate, and tert-dodecyl mercaptan are mixed to obtain a mixed solution, glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water, and cumene hydroperoxide are added to the monomer solution, stirred and mixed, and then kept warm for 2 hours, the suspension is heated to 70-80°C, a fluorocarbon surfactant is added to the suspension, mixed and stirred, and then centrifuged, the supernatant is removed, and the remaining solution is demulsified, washed, dehydrated, and dried to obtain the modified ABS masterbatch.

[0015] As a preferred solution of the present invention, the oscillation frequency is 50 Hz-80 Hz, the oscillation time is 30-45 min, the ultrasonic dispersion power is 400 W, the ultrasonic dispersion time is 3-3.5 h, the mixing and stirring rate is 120 r / min-150 r / min, and the mixing and stirring time is 50-60 min.

[0016] As a preferred solution of the present invention, the glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water and isopropyl hydroperoxide need to be added to the monomer solution under nitrogen protection at 65°C, the mixing and stirring speed is 100-300r / min, the mixing and stirring time is 60-90min, the centrifugal treatment speed is 4000-8000r / min, and the centrifugal treatment time is 10-20min.

[0017] As a preferred scheme of the present invention, the specific operating steps of the anti-slip particles are: at room temperature, the hollow glass microspheres and the coupling agent mixture are put into a stirring tank, stirred and mixed evenly, and then put into a 120-150°C oven to dry for 4-8 hours, and the modified hollow glass microspheres are obtained after screening and filtration, and the modified hollow glass microspheres, dye, maleic anhydride grafted polyethylene octene co-elastomer, antioxidant, lubricant, ultraviolet absorber and polyurethane are mixed evenly, and granulated by a granulator to obtain anti-slip particles.

[0018] As a preferred solution of the present invention, the hollow glass microspheres have a particle size of 20-35 μm and a strength of 12000-16000 ps. The mass ratio of the coupling agent mixture to the hollow glass microspheres is 3:100. The coupling agent mixture is prepared by mixing H560 coupling agent, epoxy resin and deionized water in a mass ratio of 1:10:280. The mass ratio of the modified hollow glass microspheres, the dye, the maleic anhydride grafted polyethylene octene co-elastomer, the antioxidant, the lubricant, the ultraviolet absorber and the polyurethane is 10:2:3:1.2:0.6:0.5. The dye is glyceryl monostearate and the ultraviolet absorber is a salicylate.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. In the present invention, styrene-butadiene rubber, modified graphene and modified ABS masterbatch are put into a melting machine for melting, and after they are completely melted, white carbon black, ethyl hydrogen silicone oil, epoxy propylene ether, salt catalyst and alkaline catalyst are added to the solution for mixing and stirring to obtain a mixed solution, and the mixed solution is placed in a storage tank to ensure that the mixed solution is always in a liquid state. After heat preservation and standing, rubber softening oil, heat stabilizer and vulcanizing agent are put into the mixed solution and stirred evenly, and a foaming agent and a wear-resistant agent are added and mixed to obtain a casting solution, and a sole mold is selected. The sole mold is cleaned and preheated, and then the mold release liquid is evenly sprayed into the sole mold, and the pouring liquid is evenly poured into the sole mold. After the pouring is completed, the anti-skid particles are evenly sprayed on the surface of the pouring liquid, and it is sent to the vulcanizer for vulcanization molding. After the vulcanization is completed, it is taken out and returned to room temperature, and then demolded to obtain an anti-skid and wear-resistant sole. Modified ABS with a core-shell structure is used to improve styrene-butadiene rubber. The modified ABS is composed of polybutene as the core, and the copolymer of styrene and acrylonitrile grafted on the outside of polybutene wraps the polybutene particles, thereby improving the hardness of the sole. The invention discloses a novel method for improving the performance of the rubber and the processability of the rubber. The invention discloses a ... The low surface polarity of silica is combined with the addition reaction of ethyl hydrogen silicone oil and propylene oxide under the action of a catalyst, and then the epoxy group on the addition product and the terminal hydroxyl group of the terminal hydroxyl liquid styrene butadiene rubber are used to generate a three-dimensional cross-linked network polymer under the action of an alkaline catalyst, thereby synergistically improving the compatibility of silica in the styrene butadiene rubber network polymer and achieving the uniformity of silica dispersion, thereby increasing the mechanical properties and wear resistance of styrene butadiene rubber. Adding anti-skid particles to the casting liquid can increase the surface roughness of the manufactured sole and improve the anti-skid performance of the sole. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0023] Embodiment, the present invention provides a technical solution:

[0024] A process for processing a non-slip and wear-resistant sole comprises the following steps:

[0025] S1, weighing styrene-butadiene rubber, modified graphene and modified ABS masterbatch in proportion and putting them into a melting machine for melting, filtering the obtained solution after they are completely melted, and then adding white carbon black, ethyl hydrogen silicone oil, epoxy propylene ether and salt catalyst into the solution for mixing and stirring once, and then adding alkaline catalyst into the solution for secondary mixing and stirring to obtain a mixed solution;

[0026] S2, placing the mixed liquid in a storage tank to ensure that the mixed liquid is always in a liquid state, keeping it warm and standing, adding rubber softening oil, heat stabilizer and vulcanizing agent into the mixed liquid and stirring it evenly, then sending it into a mixer, mixing it at 100-120°C for 5-10min, then adding a foaming agent and a wear-resistant agent, and continuing to mix it at 100-120°C for 4-6min to obtain a casting liquid;

[0027] S3, select a sole mold, clean and preheat the sole mold, then evenly spray a demoulding liquid into the sole mold, evenly pour a pouring liquid into the sole mold, after pouring, evenly spray anti-skid particles on the surface of the pouring liquid, send it into a vulcanizer for vulcanization and molding, take it out after vulcanization and wait for it to return to room temperature, then demould it to obtain an anti-skid and wear-resistant sole.

[0028] Furthermore, in S1, the mass ratio of styrene-butadiene rubber, modified graphene and modified ABS masterbatch is 10:8:3, the melting temperature of the melting machine is 400-550°C, the temperature of the first mixing and stirring is 200-350°C, the first mixing and stirring time is 20-26min, the temperature of the second mixing and stirring is 380-420°C, and the second mixing and stirring time is 35-48min, the salt catalyst is prepared by mixing palladium chloride and copper fluoride in a mass ratio of 1:1, and the base catalyst is triethylamine.

[0029] Furthermore, the insulation temperature in S2 is 180-200°C, the insulation time is 30-45min, the wear-resistant agent is made of titanium carbonitride fine powder, silicone oil and EVA in a weight ratio of 2:1:4, the heat stabilizer is polyvinyl pyrrolidone, the vulcanizer is N,N'-m-phenylene bismaleimide, the foaming agent is AC foaming agent, and the mass ratio of the mixed liquid, rubber softening oil, heat stabilizer, vulcanizer, foaming agent and wear-resistant agent is 15:5:2:3:4:7.

[0030] Furthermore, in S3, the preheating temperature of the sole mold is 80-140°C, the preheating time is 45-60s, the pouring liquid is poured into the sole mold at one time, and the sole mold is quickly cooled after pouring, the demoulding liquid is paraffin, the vulcanization temperature of the vulcanizer is 140-180°C, and the vulcanization time is 3-5min.

[0031] Furthermore, the preparation method of modified graphene includes the following steps: putting graphene into deionized water, shaking and then ultrasonically dispersing it, heating it to 80°C, adding γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), filtering and washing to obtain graphene oxide, mixing and stirring the graphene oxide with natural rubber latex, ultrasonically treating it again, mixing and stirring it with acetic acid solution after the treatment, flocculating and settling it, filtering and drying it to obtain modified graphene.

[0032] Furthermore, the preparation method of the modified ABS masterbatch includes the following steps: mixing styrene, acrylonitrile, glycidyl methacrylate, and tert-dodecyl mercaptan to obtain a mixed solution, adding glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water, and cumene hydroperoxide to the monomer solution, stirring and mixing, and then keeping warm for 2 hours, heating the suspension to 70-80°C, adding a fluorocarbon surfactant to the suspension, mixing and stirring, and centrifuging, removing the supernatant, and demulsifying, washing, dehydrating, and drying the remaining solution to obtain the modified ABS masterbatch.

[0033] Furthermore, the oscillation frequency is 50 Hz-80 Hz, the oscillation time is 30-45 min, the ultrasonic dispersion power is 400 W, the ultrasonic dispersion time is 3-3.5 h, the mixing and stirring rate is 120 r / min-150 r / min, and the mixing and stirring time is 50-60 min.

[0034] As a preferred embodiment of the present invention, glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water and isopropyl hydroperoxide need to be added to the monomer solution under nitrogen protection at 65°C, the mixing and stirring speed is 100-300r / min, the mixing and stirring time is 60-90min, the centrifugal treatment speed is 4000-8000r / min, and the centrifugal treatment time is 10-20min.

[0035] Furthermore, the specific operating steps of the anti-skid particles are as follows: at room temperature, the hollow glass microspheres and the coupling agent mixture are put into a stirring tank, stirred and mixed evenly, and then put into a 120-150°C oven to dry for 4-8 hours, and the modified hollow glass microspheres are obtained after sieving and filtering, and the modified hollow glass microspheres, dye, maleic anhydride grafted polyethylene octene co-elastomer, antioxidant, lubricant, ultraviolet absorber and polyurethane are mixed evenly, and granulated by a granulator to obtain the anti-skid particles.

[0036] Furthermore, the hollow glass microspheres have a particle size of 20-35 μm and a strength of 12000-16000 ps. The mass ratio of the coupling agent mixture to the hollow glass microspheres is 3:100. The coupling agent mixture is prepared by mixing H560 coupling agent, epoxy resin and deionized water in a mass ratio of 1:10:280. The mass ratio of the modified hollow glass microspheres, the dye, maleic anhydride grafted polyethylene octene co-elastomer, the antioxidant, the lubricant, the ultraviolet absorber and the polyurethane is 10:2:3:1.2:0.6:0.5. The dye is glyceryl monostearate and the ultraviolet absorber is a salicylate.

[0037] Specific implementation cases:

[0038] Put graphene into deionized water, shake and then perform ultrasonic dispersion, the oscillation frequency is -80 Hz, the oscillation time is 45 min, the ultrasonic dispersion power is 400 W, the ultrasonic dispersion time is 3.5 h, heat to 80 ° C, add γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), filter and wash to obtain graphene oxide, mix and stir the graphene oxide with natural rubber latex, the mixing and stirring rate is 150 r / min, the mixing and stirring time is 60 min, perform ultrasonic treatment again, mix and stir with acetic acid solution after the treatment, flocculate and settle, filter and dry to obtain modified graphene;

[0039] Styrene, acrylonitrile, glycidyl methacrylate and tert-dodecyl mercaptan are mixed to obtain a mixed solution, and then glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water and cumene hydroperoxide are added to the monomer solution under nitrogen protection at 65°C, and the mixture is stirred and mixed, and the mixture is kept warm for 2 hours. The mixing and stirring speed is 300 r / min and the mixing and stirring time is 90 minutes. The suspension is heated to 80°C, and a fluorocarbon surfactant is added to the suspension. After mixing and stirring, the mixture is centrifuged at a speed of 8000 r / min and a centrifugal time of 20 minutes. The supernatant is removed and the remaining solution is demulsified, washed, dehydrated and dried to obtain a modified ABS masterbatch.

[0040] Weighing styrene-butadiene rubber, modified graphene and modified ABS masterbatch in a mass ratio of 10:8:3 and putting them into a melting machine for melting, the melting temperature of the melting machine is 550°C, and after they are completely melted, filtering the obtained solution, and then adding white carbon black, ethyl hydrogen silicone oil, epoxy propylene ether and a salt catalyst into the solution for a mixing and stirring, the salt catalyst is prepared by mixing palladium chloride and copper fluoride in a mass ratio of 1:1, the temperature of the first mixing and stirring is 350°C, the mixing and stirring time is 26 minutes, and then adding an alkaline catalyst into the solution for a second mixing and stirring, the alkaline catalyst is triethylamine, the temperature of the second mixing and stirring is 420°C, and the mixing and stirring time is 48 minutes, to obtain a mixed solution;

[0041] The mixed liquid is placed in a storage tank to ensure that the mixed liquid is always in a liquid state, and the mixed liquid is kept still at a temperature of 200°C for 45 minutes. Rubber softening oil, heat stabilizer and vulcanizing agent are added to the mixed liquid and stirred evenly, and then sent to a mixer, mixed at 120°C for 10 minutes, and then a foaming agent and a wear-resistant agent are added. The wear-resistant agent is made by mixing titanium carbonitride fine powder, silicone oil and EVA in a weight ratio of 2:1:4, the heat stabilizer is polyvinyl pyrrolidone, the vulcanizing agent is N, N'-phenylene bismaleimide, and the foaming agent is AC foaming agent. The mass ratio of the mixed liquid, rubber softening oil, heat stabilizer, vulcanizing agent, foaming agent and wear-resistant agent is 15:5:2:3:4:7. Continue mixing at 100-120°C for 4-6 minutes to obtain a casting liquid;

[0042] At room temperature, hollow glass microspheres and a coupling agent mixture were put into a stirring tank, the hollow glass microspheres had a particle size of 20 μm and a strength of 12000 ps, ​​the coupling agent mixture and the hollow glass microspheres had a mass ratio of 3:100, and the coupling agent mixture was prepared by mixing H560 coupling agent, epoxy resin and deionized water in a mass ratio of 1:10:280. After being stirred and mixed evenly, the mixture was placed in a 150°C oven and dried for 8 hours. After sieving and filtering, the modified hollow glass microspheres were obtained. Hollow glass microspheres, dye, maleic anhydride grafted polyethylene octene co-elastomer, antioxidant, lubricant, ultraviolet absorber and polyurethane are uniformly mixed, the mass ratio of modified hollow glass microspheres, dye, maleic anhydride grafted polyethylene octene co-elastomer, antioxidant, lubricant, ultraviolet absorber and polyurethane is 10:2:3:1.2:0.6:0.5, the dye is glyceryl monostearate, the ultraviolet absorber is salicylate, and granulation is carried out by a granulator to obtain anti-skid particles.

[0043] A sole mold is selected, cleaned and preheated. The preheating temperature of the sole mold is 140°C and the preheating time is 60s. Then, a demoulding liquid is evenly sprayed in the sole mold. The demoulding liquid is paraffin. The pouring liquid is evenly poured into the sole mold. The pouring liquid is poured into the sole mold at one time, and the sole mold is quickly cooled after pouring. After pouring, anti-slip particles are evenly sprayed on the surface of the pouring liquid and sent to a vulcanizer for vulcanization molding. The vulcanization temperature of the vulcanizer is 180°C and the vulcanization time is 5min. After vulcanization, it is taken out and returned to room temperature before demoulding to obtain a non-slip and wear-resistant sole.

[0044] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A non-slip and wear-resistant sole processing technology, characterized in that: The following steps are involved: S1, weighing styrene-butadiene rubber, modified graphene and modified ABS masterbatch in proportion and putting them into a melting machine for melting, filtering the obtained solution after they are completely melted, and then adding white carbon black, ethyl hydrogen silicone oil, epoxy propylene ether and salt catalyst into the solution for mixing and stirring once, and then adding alkaline catalyst into the solution for secondary mixing and stirring to obtain a mixed solution; S2, placing the mixed liquid in a storage tank to ensure that the mixed liquid is always in a liquid state, keeping it warm and standing, adding rubber softening oil, heat stabilizer and vulcanizing agent into the mixed liquid and stirring it evenly, then sending it into a mixer, mixing it at 100-120°C for 5-10min, then adding a foaming agent and a wear-resistant agent, and continuing to mix it at 100-120°C for 4-6min to obtain a casting liquid; S3, select a sole mold, clean and preheat the sole mold, then evenly spray a demoulding liquid into the sole mold, evenly pour a pouring liquid into the sole mold, after pouring, evenly spray anti-skid particles on the surface of the pouring liquid, send it into a vulcanizer for vulcanization and molding, take it out after vulcanization and wait for it to return to room temperature, then demould it to obtain an anti-skid and wear-resistant sole.

2. The process for manufacturing a non-slip and wear-resistant sole according to claim 1, characterized in that: The mass ratio of styrene-butadiene rubber, modified graphene and modified ABS masterbatch in S1 is 10:8:3, the melting temperature of the melting machine is 400-550°C, the temperature of the first mixing and stirring is 200-350°C, the first mixing and stirring time is 20-26min, the temperature of the second mixing and stirring is 380-420°C, and the second mixing and stirring time is 35-48min, the salt catalyst is prepared by mixing palladium chloride and copper fluoride in a mass ratio of 1:1, and the alkali catalyst is triethylamine.

3. The process for manufacturing a non-slip and wear-resistant sole according to claim 1, characterized in that: The insulation temperature in S2 is 180-200°C, and the insulation time is 30-45 minutes. The wear-resistant agent is made by mixing titanium carbonitride fine powder, silicone oil and EVA in a weight ratio of 2:1:4, the heat stabilizer is polyvinyl pyrrolidone, the vulcanizer is N,N'-m-phenylene bismaleimide, and the foaming agent is AC foaming agent. The mass ratio of the mixed liquid, rubber softening oil, heat stabilizer, vulcanizer, foaming agent and wear-resistant agent is 15:5:2:3:4:

7.

4. The process for manufacturing a non-slip and wear-resistant sole according to claim 1, characterized in that: The preheating temperature of the sole mold in S3 is 80-140°C, and the preheating time is 45-60s. The pouring liquid is poured into the sole mold at one time, and the sole mold is quickly cooled after pouring. The demoulding liquid is paraffin. The vulcanizing temperature of the vulcanizer is 140-180°C, and the vulcanizing time is 3-5min.

5. The process for manufacturing a non-slip and wear-resistant sole according to claim 1, characterized in that: The preparation method of the modified graphene comprises the following steps: putting the graphene into deionized water, shaking and then ultrasonically dispersing it, heating it to 80°C and adding γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), filtering and washing to obtain graphene oxide, mixing and stirring the graphene oxide with natural rubber latex, ultrasonically treating it again, mixing and stirring it with acetic acid solution after the treatment, flocculating and settling it, filtering and drying it to obtain the modified graphene.

6. The process for manufacturing a non-slip and wear-resistant sole according to claim 1, characterized in that: The preparation method of the modified ABS masterbatch comprises the following steps: mixing styrene, acrylonitrile, glycidyl methacrylate and tert-dodecyl mercaptan to obtain a mixed solution, adding glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water and cumene hydroperoxide into the monomer solution, stirring and mixing, and then keeping the temperature for 2 hours, heating the suspension to 70-80° C., adding a fluorocarbon surfactant into the suspension, mixing and stirring, and then centrifuging, removing the supernatant, and performing demulsification, washing, dehydrating and drying operations on the remaining solution, so as to obtain the modified ABS masterbatch.

7. The process for manufacturing a non-slip and wear-resistant sole according to claim 5, characterized in that: The oscillation frequency is 50 Hz-80 Hz, the oscillation time is 30-45 min, the ultrasonic dispersion power is 400 W, the ultrasonic dispersion time is 3-3.5 h, the mixing and stirring rate is 120 r / min-150 r / min, and the mixing and stirring time is 50-60 min.

8. The process for manufacturing a non-slip and wear-resistant sole according to claim 6, characterized in that: The glucose, sodium pyrophosphate, ferric sulfate solution, polybutadiene latex, deionized water and cumene hydroperoxide need to be added to the monomer solution under nitrogen protection at 65°C, the mixing and stirring speed is 100-300r / min, the mixing and stirring time is 60-90min, the centrifugal treatment speed is 4000-8000r / min, and the centrifugal treatment time is 10-20min.

9. The process for manufacturing a non-slip and wear-resistant sole according to claim 1, characterized in that: The specific operation steps of the anti-skid particles are as follows: at room temperature, the hollow glass microbeads and the coupling agent mixture are put into a stirring tank, stirred and mixed evenly, and then put into a 120-150° C. oven for drying for 4-8 hours, and sieved and filtered to obtain modified hollow glass microbeads, and the modified hollow glass microbeads, a dye, a maleic anhydride grafted polyethylene octene co-elastomer, an antioxidant, a lubricant, an ultraviolet absorber and polyurethane are evenly mixed, and granulated by a granulator to obtain the anti-skid particles.

10. The process for manufacturing a non-slip and wear-resistant sole according to claim 9, characterized in that: The hollow glass microspheres have a particle size of 20-35 μm and a strength of 12000-16000 ps. The mass ratio of the coupling agent mixture to the hollow glass microspheres is 3:

100. The coupling agent mixture is prepared by mixing H560 coupling agent, epoxy resin and deionized water in a mass ratio of 1:10:

280. The mass ratio of the modified hollow glass microspheres, dye, maleic anhydride grafted polyethylene octene co-elastomer, antioxidant, lubricant, ultraviolet absorber and polyurethane is 10:2:3:1.2:0.6:0.

5. The dye is glyceryl monostearate and the ultraviolet absorber is salicylate.