Nitrile rubber material resistant to 150 DEG C hot air
Through formula adjustment and process preparation, a nitrile rubber material that is resistant to 150°C hot air was prepared, which solved the problem of insufficient heat resistance of existing nitrile rubber and enabled high-temperature applications and cost reduction in the automotive field.
Patent Information
- Application Number
- CN202310427069.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-22
AI Technical Summary
The heat resistance of existing nitrile rubber is insufficient and cannot meet the high-temperature application requirements of peripheral rubber parts in the automotive field, resulting in limitations such as limited application and increased costs.
Through formula adjustment, nitrile rubber, ethylene propylene rubber, magnesium oxide, cerium oxide and other materials are used, combined with vulcanized cross-linking agent and polyester plasticizer, to prepare a nitrile rubber material that is resistant to 150°C hot air. Refining, refining and vulcanization process preparation.
In a hot air environment of 150°C, the material does not become brittle and remains soft and elastic, reducing production costs and energy consumption, extending its service life, and is simple to operate.
Smart Images

Figure BDA0004188874200000061 
Figure BDA0004188874200000071 
Figure BDA0004188874200000072
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber sealing materials, and in particular to a nitrile rubber material resistant to 150°C hot air. Background Art
[0002] Nitrile rubber is a polymer elastomer obtained by copolymerization of butadiene and acrylonitrile. Nitrile rubber is known for its excellent oil resistance. Among the existing rubbers, its oil resistance is second only to acrylic rubber and fluororubber. However, its price is the lowest among the three, which is 1 / 3 of acrylic rubber and 1 / 10 of fluororubber. It is widely used in oil-resistant products such as seals, gaskets, hoses, diaphragms, etc.
[0003] However, the heat resistance of nitrile rubber is only 100℃ for a long time and 120℃ for a short time. It is 50℃ lower than acrylate and 100℃ lower than fluororubber. In the current automotive field where rubber is used in large quantities, except for a small number of parts near the combustion chamber whose operating temperature is above 200℃, the operating temperature of most peripheral rubber parts is only between 130 and 150℃. The existing nitrile rubber is not able to withstand high temperatures, which limits its application in this field. Currently, only more expensive acrylate rubber can be selected. At present, hydrogenation treatment can also be used for nitrile rubber to increase the saturation of nitrile rubber and increase the high temperature resistance of nitrile rubber to 150℃. However, the synthesis conditions are harsh and the equipment requirements are high, which ultimately leads to a 10-fold increase in cost and limited application. If the high temperature resistance of nitrile rubber can be increased by 20 to 30℃ without significantly increasing the cost by adjusting the formula, it will be possible to improve the insufficiency of the selection of peripheral sealing materials for automobile engines, reduce the cost of existing materials, and increase the application field of nitrile rubber. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a nitrile rubber material resistant to 150° C. hot air.
[0005] The invention provides a 150°C hot air resistant nitrile rubber material, wherein the raw materials include, by weight: 80-120 parts of nitrile rubber, 10-20 parts of ethylene propylene rubber, 20-50 parts of silicon dioxide, 90-125 parts of heat-resistant agent, 5-10 parts of antioxidant, 2-5 parts of vulcanization crosslinking agent, and 1-5 parts of polyester plasticizer;
[0006] The heat-resistant agent is composed of magnesium oxide and cerium oxide in a weight ratio of (70-120): (5-20).
[0007] Preferably, the magnesium oxide is at least one of light magnesium oxide, heavy magnesium oxide, and active magnesium oxide.
[0008] Preferably, the antioxidant is at least one of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, the reaction product of acetone and diphenylamine, octylated diphenylamine, 4,4-bis(a,a-dimethylbenzyl)diphenylamine, 2-thiolbenzimidazole zinc salt, and nickel dibutyldithiocarbamate.
[0009] Preferably, the vulcanization crosslinking agent is at least one of dicumyl peroxide, 1,4-bis-tert-butylperoxycumene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, triallyl isocyanurate, and trimethylolpropane trimethacrylate.
[0010] Preferably, the polyester plasticizer is polymerized from sebacic acid and adipic acid, and has a molecular weight of 5000-8000.
[0011] Preferably, the acrylonitrile content in the nitrile rubber is 17-50%, and the Mooney viscosity is 30-80 units.
[0012] Preferably, the EPDM rubber is EPDM terpolymer, EPDM dipolymer or a combination thereof; the ethylene content in the EPDM rubber is 65-80%, and the Mooney viscosity is 30-80 units.
[0013] A method for preparing a nitrile rubber material resistant to 150°C hot air is characterized in that it comprises the following steps: weighing raw materials by weight, adding them into an internal mixer, mixing them to obtain a rubber mix, then mixing and forming them, and then vulcanizing them to obtain the nitrile rubber material resistant to 150°C hot air.
[0014] Preferably, the debinding temperature of the internal mixing is 100-120°C.
[0015] Preferably, the temperature of the open refining is 40-70°C.
[0016] Preferably, the vulcanization pressure is 150-200Kgf / cm 2 , temperature is 160-190℃, time is 5-10min.
[0017] The beneficial effects of the present invention are as follows:
[0018] The present invention uses common nitrile rubber as a base material, and obtains a nitrile rubber material with excellent high temperature resistance through formula optimization. After being placed in a hot air environment at 150°C for 70 hours, the material has no brittleness phenomenon and maintains the soft and elastic properties of the rubber, and can continue to be used as a sealing material without the need for complex hydrogenation treatment, and is simple to operate, with low energy consumption and low cost during the production process. DETAILED DESCRIPTION
[0019] The technical solution of the present invention is described in detail below through specific embodiments.
[0020] In the following examples and comparative examples, the polyester plasticizer is polymerized from sebacic acid and adipic acid, and has a molecular weight of 5000-8000; the acrylonitrile content in the nitrile rubber is 17-50%, and the Mooney viscosity is 30-80 units; the EPDM rubber is EPDM, and has an ethylene content of 65-80% and a Mooney viscosity of 30-80 units.
[0021] Example 1
[0022] A nitrile rubber material resistant to hot air at 150°C comprises, by weight, 80 parts of nitrile rubber, 50 parts of silicon dioxide, 10 parts of ethylene propylene rubber, 90 parts of heat-resistant agent, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of a reaction product of acetone and diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of 1,4-di-tert-butyl peroxyisopropylbenzene, 2 parts of triallyl isocyanurate and 3 parts of polyester plasticizer; wherein the heat-resistant agent is composed of active magnesium oxide and cerium oxide in a weight ratio of 70:20.
[0023] The preparation method of the nitrile rubber material is as follows: weigh the raw materials by weight, add them to a banbury mixer and knead them at 120°C, remove the rubber to obtain a mixed rubber, and then knead them at 55°C to form a mixed rubber, and then knead them at a pressure of 170Kgf / cm 2、 Vulcanize at 175°C for 8 minutes to obtain the product.
[0024] Example 2
[0025] A nitrile rubber material resistant to hot air at 150°C, wherein the raw materials include, by weight: 100 parts of nitrile rubber, 15 parts of ethylene propylene rubber, 40 parts of silicon dioxide, 125 parts of heat-resistant agent, 2 parts of 4,4-bis(a,a-dimethylbenzyl)diphenylamine, 2 parts of 2-thiolbenzimidazole zinc salt, 1 part of nickel dibutyl dithiocarbamate, 2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and 1 part of polyester plasticizer; wherein the heat-resistant agent is composed of light magnesium oxide and cerium oxide in a weight ratio of 120:5.
[0026] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0027] Example 3
[0028] A nitrile rubber material resistant to hot air at 150°C, wherein the raw materials include, by weight: 120 parts of nitrile rubber, 20 parts of ethylene propylene rubber, 20 parts of silicon dioxide, 110 parts of heat-resistant agent, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of octylated diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of nickel dibutyl dithiocarbamate, 2 parts of diisopropylbenzene peroxide, 3 parts of trimethylolpropane trimethacrylate, and 5 parts of polyester plasticizer; wherein the heat-resistant agent is composed of light magnesium oxide, heavy magnesium oxide, and cerium oxide in a weight ratio of 80:20:10.
[0029] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0030] Comparative Example 1
[0031] The difference between Comparative Example 1 and Example 1 is that the heat-resistant agent is replaced by a reinforcing agent, carbon black, as follows:
[0032] A nitrile rubber material, whose raw materials include, by weight: 80 parts of nitrile rubber, 50 parts of silicon dioxide, 10 parts of ethylene propylene rubber, 90 parts of reinforcing agent carbon black, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of reaction product of acetone and diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of 1,4-di-tert-butyl peroxyisopropylbenzene, 2 parts of triallyl isocyanurate, and 3 parts of polyester plasticizer.
[0033] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0034] Comparative Example 2
[0035] The difference between Comparative Example 2 and Example 1 is that white carbon black and diatomaceous earth are used instead of the heat-resistant agent, as follows:
[0036] A nitrile rubber material, whose raw materials include, by weight: 80 parts of nitrile rubber, 50 parts of silicon dioxide, 10 parts of ethylene propylene rubber, 40 parts of white carbon black, 50 parts of diatomaceous earth, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of reaction product of acetone and diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of 1,4-di-tert-butyl peroxyisopropylbenzene, 2 parts of triallyl isocyanurate, and 3 parts of polyester plasticizer.
[0037] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0038] Comparative Example 3
[0039] The only difference between Comparative Example 3 and Example 1 is that active magnesium oxide is used as a heat-resistant agent, as follows:
[0040] A nitrile rubber material, whose raw materials include, by weight: 80 parts of nitrile rubber, 50 parts of silicon dioxide, 10 parts of ethylene propylene rubber, 90 parts of active magnesium oxide, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of reaction product of acetone and diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of 1,4-di-tert-butyl peroxyisopropylbenzene, 2 parts of triallyl isocyanurate, and 3 parts of polyester plasticizer.
[0041] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0042] Comparative Example 4
[0043] The only difference between Comparative Example 4 and Example 1 is that cerium oxide is used as a heat-resistant agent, as follows:
[0044] A nitrile rubber material, whose raw materials include, by weight: 80 parts of nitrile rubber, 50 parts of silicon dioxide, 10 parts of ethylene propylene rubber, 90 parts of cerium oxide, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of reaction product of acetone and diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of 1,4-di-tert-butyl peroxyisopropylbenzene, 2 parts of triallyl isocyanurate, and 3 parts of polyester plasticizer.
[0045] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0046] Comparative Example 5
[0047] The difference between Comparative Example 5 and Example 1 is that the heat-resistant agent is composed of active magnesium oxide and cerium oxide in a weight ratio of 65:25, as follows:
[0048] A nitrile rubber material, whose raw materials include, by weight: 80 parts of nitrile rubber, 50 parts of silicon dioxide, 10 parts of ethylene propylene rubber, 90 parts of heat-resistant agent, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2 parts of reaction product of acetone and diphenylamine, 3 parts of 2-thiol benzimidazole zinc salt, 2 parts of 1,4-di-tert-butyl peroxyisopropylbenzene, 2 parts of triallyl isocyanurate, and 3 parts of polyester plasticizer; the heat-resistant agent is composed of active magnesium oxide and cerium oxide in a weight ratio of 65:25.
[0049] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0050] Comparative Example 6
[0051] The difference between Comparative Example 6 and Example 2 is that the heat-resistant agent is composed of active magnesium oxide and cerium oxide in a weight ratio of 121:4, as follows:
[0052] A nitrile rubber material, whose raw materials include, by weight: 100 parts of nitrile rubber, 15 parts of ethylene propylene rubber, 40 parts of silicon dioxide, 125 parts of heat-resistant agent, 2 parts of 4,4-bis(a,a-dimethylbenzyl)diphenylamine, 2 parts of 2-thiol benzimidazole zinc salt, 1 part of nickel dibutyl dithiocarbamate, 2 parts of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and 1 part of polyester plasticizer; wherein the heat-resistant agent is composed of light magnesium oxide and cerium oxide in a weight ratio of 121:4.
[0053] The preparation method of the above-mentioned nitrile rubber material is the same as that of Example 1.
[0054] Test example
[0055] The nitrile rubber materials of Examples 1-3 and the nitrile rubber materials of Comparative Examples 1-6 were subjected to hot air aging at 150° C., and their performances were compared after 70 hours. The test results are shown in Tables 1 and 2.
[0056] Table 1 Performance comparison of Examples 1-3 after hot air aging at 150°C for 70 hours
[0057]
[0058]
[0059] Note: The closer the hardness change, tensile strength change rate, and elongation at break change rate are to 0, the smaller the change value is, which means the material has better high temperature resistance.
[0060] It can be seen from Table 1 that the nitrile rubber material prepared by the present invention has a low air leakage rate at 150° C. and reliable sealing; there is no problem of bulging bubbles during use, it is not easy to be damaged, and has a long service life.
[0061] Table 2 Comparative Examples 1-6 Performance Comparison after Hot Air Aging at 150°C for 70 Hours
[0062]
[0063] Note: The closer the change rate of tensile strength and elongation at break is to -100%, the smaller the change value is, which means the material has better high temperature resistance. The test standard refers to GB / T3512.
[0064] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A nitrile rubber material resistant to 150°C hot air, characterized in that: The raw materials include, by weight: 80-120 parts of nitrile rubber, 10-20 parts of ethylene-propylene rubber, 20-50 parts of silicon dioxide, 90-125 parts of heat-resistant agent, 5-10 parts of antioxidant, 2-5 parts of vulcanization cross-linking agent, and 1-5 parts of polyester plasticizer; The heat-resistant agent is composed of magnesium oxide and cerium oxide in a weight ratio of (70-120): (5-20).
2. The 150°C hot air resistant nitrile rubber material according to claim 1, characterized in that: The magnesium oxide is at least one of light magnesium oxide, heavy magnesium oxide and active magnesium oxide.
3. The 150°C hot air resistant nitrile rubber material according to claim 1, characterized in that: The antioxidant is at least one of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, the reaction product of acetone and diphenylamine, octylated diphenylamine, 4,4-bis(a,a-dimethylbenzyl)diphenylamine, 2-thiol benzimidazole zinc salt, and nickel dibutyl dithiocarbamate.
4. The nitrile rubber material resistant to 150°C hot air according to claim 1, characterized in that: The vulcanization crosslinking agent is at least one of dicumyl peroxide, 1,4-bis-tert-butyl peroxycumene, 2,5-dimethyl-2,5-bis(tert-butyl peroxy)hexane, triallyl isocyanurate, and trimethylolpropane trimethacrylate.
5. The 150°C hot air resistant nitrile rubber material according to claim 1, characterized in that: The polyester plasticizer is polymerized from sebacic acid and adipic acid, and has a molecular weight of 5000-8000.
6. The 150°C hot air resistant nitrile rubber material according to claim 1, characterized in that: The acrylonitrile content in the nitrile rubber is 17-50%, and the Mooney viscosity is 30-80 units.
7. The 150°C hot air resistant nitrile rubber material according to claim 1, characterized in that: The EPDM rubber is EPDM terpolymer, EPDM dipolymer or a combination thereof; the ethylene content in the EPDM rubber is 65-80%, and the Mooney viscosity is 30-80 units.
8. A method for preparing a 150°C hot air resistant nitrile rubber material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: weighing raw materials by weight, adding the raw materials into an internal mixer, performing internal mixing to obtain a mixed rubber, performing open mixing to form the mixed rubber, and performing vulcanization to obtain a nitrile rubber material resistant to hot air at 150°C.