Functional graphene oxide, preparation method thereof and obtained rubber material
By using vinyl end-capped active graphene oxide and fluoroelastic rubber in fluoroelastic rubber, the problem of insufficient dispersion and curing reactivity of graphene oxide in fluoroelastic matrix is solved, and high-strength and high-thermal oxygen aging is achieved and highly conductive fluoroelastic materials, suitable for special service environments.
Patent Information
- Application Number
- CN202411048239.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-26
AI Technical Summary
The dispersion and curing reactivity of graphene oxide in the fluoroelastic matrix are insufficient, resulting in poor aging performance under high temperature environments, making it difficult to effectively improve the aging resistance of fluoroelastic.
Functional graphene oxide determined by X-ray diffractometer test has 2θ of 4.1-4.77° and layer spacing is 1.85-2.15 nm. Vinyl-terminated active graphene oxide is combined with fluoroelastomer, and isocyanate graft modification method is used to combine it with isocyanate grafting Highly reactive graphene oxide was prepared to enhance its dispersion ability and curing reactivity in fluoroelastomer.
The prepared fluoro-rubber/vinyl end-capped graphene oxide composite material exhibits high strength, high heat oxygen aging resistance and high conductivity, which is suitable for special service environments and significantly improves the aging resistance of fluoro-rubber.
Smart Images

Figure CN119019760A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber materials, and in particular relates to functional graphene oxide and a preparation method thereof and the obtained rubber material. Background Art
[0002] As an amorphous material, rubber is in a highly elastic state at room temperature, and the main moving unit of its molecule is the "chain segment". The carbon atoms in the side chain or main chain of fluororubber (FKM) contain fluorine, the element with the strongest electronegativity in the periodic table. The fluorine atoms are closely arranged around the carbon atoms, and the fluorine atoms have a large radius, so the fluorine atoms can shield the CC bond, ensuring the stability of its main chain, giving the FKM carbon-carbon chain chemical inertness, and is a special rubber with excellent heat resistance, oil resistance, chemical resistance and mechanical properties.
[0003] One of the important applications of FKM in the oil and gas production process is the O-ring used as a sealing device in the packer. However, at high temperatures, fluororubber will undergo oxidation and decomposition, free radicals will gradually be generated, the oxidation reaction will gradually intensify, and the CF bond protection in the CC main chain of fluororubber will be broken, resulting in the destruction of the rubber molecular chain. The rubber will age and the performance will continue to deteriorate, and eventually the sealing failure behavior will occur. Adding carbon materials to the rubber matrix can construct a carbon-based nanomaterial free radical capture network in the rubber matrix. By capturing and quenching the newly generated free radicals in the aging process of fluororubber, the initiation of free radicals on the rubber macromolecular chain can be effectively inhibited, and the aging resistance of fluororubber can be improved. Therefore, adding carbon materials such as graphene and carbon nanotubes with strong thermal conductivity to the polyurethane elastomer matrix is an important research direction.
[0004] Graphene is a two-dimensional lattice structure formed by hexagonal arrangement of carbon atoms, a single-layer carbon material. It has many unique physical and chemical properties, including excellent electrical conductivity, thermal conductivity, mechanical strength and electron cloud delocalization characteristics. When graphene is added to composite materials as a reinforcing agent, it can improve the mechanical properties and wear resistance of the material. In order to achieve the ideal composite effect, it is crucial to improve the dispersion ability of graphene in the polymer matrix.
[0005] The composite modification effect of graphene on FKM can be improved by modification. Common methods of graphene oxide modification include covalent modification by introducing new functional groups to adjust the properties and functions of graphene oxide and non-covalent modification by adsorbing or adsorbing other molecules or functional groups onto the surface of graphene oxide through non-covalent bond interactions (such as π-π stacking, van der Waals forces, hydrogen bonds, etc.), thereby changing its properties or enhancing its performance. However, even after modification, the hydroxyl activity on the modified graphene oxide is relatively low, making it difficult to effectively disperse in the polyurethane matrix and participate in the curing reaction. Summary of the invention
[0006] The present invention provides a functional graphene oxide and a preparation method thereof and a rubber material obtained therefrom, aiming to solve the problems of the dispersibility of graphene oxide in a FKM matrix and its ability to participate in curing reactivity, and to compound FKM with vinyl-terminated active graphene oxide to prepare a high-strength, high-resistance to heat and oxygen aging and high-conductivity FKM composite material suitable for promotion and application in special service environments.
[0007] In order to achieve the above-mentioned purpose, the present invention provides a functional graphene oxide. When tested by an X-ray diffractometer at a scanning speed of 5° / min and a scanning range of 3° to 60°, the 2θ of the functional graphene oxide is 4.1-4.77°, the interlayer spacing is 1.85-2.15nm, and the grafting rate of vinyl functional groups measured from room temperature to 600°C under N2 atmosphere is 53.5-87.6%.
[0008] As a preference, the method comprises the following steps:
[0009] The graphene oxide grafted with isocyanate was dissolved in dimethyl sulfoxide, nitrogen was introduced, and then the mixture was sealed and ultrasonically dispersed uniformly.
[0010] Hydroxyethyl methacrylate is stirred and heated in the presence of a sufficient amount of dimethyl sulfoxide solvent, and then the above dispersion is added dropwise, and 2-3 drops of catalyst dibutyltin dilaurate are added, and grafting modification is performed under a nitrogen atmosphere to obtain vinyl-terminated graphene oxide (HEMA@GO), i.e., functional graphene oxide. The preparation principle is as follows: Figure 2 shown.
[0011] Preferably, the mass ratio of graphene oxide grafted with isocyanate to dimethyl sulfoxide is 1:500-1:800, preferably 1:600;
[0012] The mass ratio of isocyanate-grafted graphene oxide to hydroxyethyl methacrylate is 1:50-1:150, preferably 1:100.
[0013] Preferably, the stirring heating temperature ranges from 60 to 80° C., preferably 70° C.; and the grafting modification reaction time is 8 to 12 h, preferably 10 h.
[0014] Preferably, the graphene oxide containing isocyanate grafting is prepared by the following method:
[0015] Graphene oxide GO is dissolved in a dimethyl sulfoxide solution, and after ultrasonic mixing, it is slowly added dropwise to a modification solution with diisocyanate as a modifier, dibutyltin dilaurate as a catalyst, and dimethyl sulfoxide solution as a solvent. The graphene oxide GO is grafted with diisocyanate under a nitrogen atmosphere. After the reaction is completed, it is centrifuged, washed, and dried to obtain graphene oxide grafted with isocyanate. The preparation principle is as follows: Figure 1shown.
[0016] Preferably, the mass ratio of graphene oxide GO to dimethyl sulfoxide solution is 1:500-1:800, preferably 1:600;
[0017] The mass ratio of diisocyanate, dibutyltin dilaurate and dimethyl sulfoxide solution in the modified solution is 1:5-1:8, preferably 1:6;
[0018] The mass ratio of graphene oxide GO to diisocyanate in the modified solution is 1:50-1:150, preferably 1:10;
[0019] The reaction is carried out in a nitrogen atmosphere at 50-90°C for 5-9 hours, preferably at 65°C for 7 hours.
[0020] Preferably, the diisocyanate is selected from at least one of isophorone diisocyanate (IPDI), toluene diisocyanate (TDI) and 4,4-diisocyanate diphenylmethane (MDI), preferably toluene diisocyanate (TDI).
[0021] The present invention provides a rubber material, which is prepared by using the functional graphene oxide described in the above technical solution.
[0022] As a preference, the method comprises the following steps:
[0023] Functional graphene oxide powder is mixed with carbon black and then kneaded evenly with a fluororubber matrix on an open mill, and then a vulcanizing agent and a vulcanizing agent are added in sequence to obtain a mixed rubber, which is vulcanized after standing to obtain a fluororubber / vinyl-terminated functional graphene oxide composite material, i.e., a rubber material.
[0024] Preferably, the amount of functional graphene oxide powder added to the rubber material is 0.2-1 part by weight.
[0025] Compared with the prior art, the advantages and positive effects of the present invention are:
[0026] 1. The present invention provides a functional graphene oxide with large interlayer spacing and high vinyl functional group grafting rate and a preparation method thereof. The method optimizes the chemical process of HEMA and diisocyanate functionalized graphene oxide, and uses wet chemical reaction to prepare a large amount of reactive functional graphene oxide with large interlayer spacing, so that graphene oxide becomes a highly active intermediate that can exist stably.
[0027] 2. The functional graphene oxide provided by the present invention can effectively participate in the compounding of FKM without harsh conditions, which saves energy and can well maintain the lamellar structure of graphene. In addition, the interlayer spacing of the functional graphene oxide is enlarged, which improves its dispersion ability in the fluororubber matrix, and helps it to exert the reinforcement, anti-aging and conductive functionality of two-dimensional graphene. The prepared fluororubber / vinyl-terminated functional graphene oxide composite material, that is, the rubber material has the advantages of high strength, high resistance to heat and oxygen aging and high conductivity, and is suitable for promotion and application in special service environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The preparation principle of toluene diisocyanate modified GO provided in the embodiment of the present invention;
[0029] Figure 2 The preparation principle of hydroxyethyl methacrylate modified NCO@GO provided in the embodiment of the present invention;
[0030] Figure 3 Infrared spectra of GO, TGO and HEMA@GO provided in the embodiments of the present invention;
[0031] Figure 4 XRD patterns of GO, TGO and HEMA@GO provided in the embodiments of the present invention. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] Take 30mL DMSO solution, 10mL TDI and 4 drops of DBTDL and pour them into a 100mL single-necked flask, and stir at 65°C; take another 0.1g GO powder and put it in a digestion tube, add 30mL DMSO solution to the digestion tube with GO powder, shake it to mix, and ultrasonicate it for 0.5h. After the ultrasonication is completed, slowly add the GO dispersion into the single-necked flask, react at 65°C in a nitrogen atmosphere for 7h. After the reaction is completed, the product is centrifuged, washed and dried to obtain TDI-functionalized graphene oxide (TGO).
[0035] Example 2
[0036] Take 30mL DMSO solution, 10mL IPDI and 4 drops of DBTDL and pour them into a 100mL single-necked flask, and stir at 65°C; take another 0.1g GO powder and put it in a digestion tube, add 30mL DMSO solution to the digestion tube with GO powder, shake it to mix, and ultrasonicate it for 0.5h. After the ultrasonication is completed, slowly add the GO dispersion into the single-necked flask, react at 65°C in a nitrogen atmosphere for 7h. After the reaction is completed, the product is centrifuged, washed and dried to obtain IPDI-functionalized graphene oxide (IGO).
[0037] Example 3
[0038] Take 30mL DMSO solution, 10mL MDI and 4 drops of DBTDL and pour them into a 100mL single-necked flask, and stir at 65°C; take another 0.1g GO powder and put it in a digestion tube, add 30mL DMSO solution to the digestion tube with GO powder, shake it to mix, and ultrasonicate it for 0.5h. After the ultrasonication is completed, slowly add the GO dispersion into the single-necked flask, react at 65°C in a nitrogen atmosphere for 7h. After the reaction is completed, the product is centrifuged, washed and dried to obtain MDI-functionalized graphene oxide (MGO).
[0039] Example 4
[0040] 0.1 g TGO and 30 mL DMSO were placed in a digestion tube, sealed after nitrogen was introduced, and dispersed under ultrasound for 0.5 h; 10 mL hydroxyethyl methacrylate (HEMA) and 30 mL DMSO were placed in a single-hole flask, stirred and heated to 60 ° C, and then the TGO dispersion was added dropwise to the hydroxyethyl methacrylate mixed solution, and 4 drops of DBTDL were added, and the reaction was carried out under nitrogen atmosphere for 10 h. After the reaction, the product was centrifuged and washed and then dried to obtain vinyl-terminated graphene oxide (HEMA@GO).
[0041] Example 5
[0042] 0.1 g TGO and 30 mL DMSO were placed in a digestion tube, sealed after nitrogen was introduced, and dispersed under ultrasound for 0.5 h; 10 mL hydroxyethyl methacrylate (HEMA) and 30 mL DMSO were placed in a single-hole flask, stirred and heated to 70 ° C, and then the TGO dispersion was added dropwise to the hydroxyethyl methacrylate mixed solution, and 4 drops of DBTDL were added, and the reaction was carried out under a nitrogen atmosphere for 10 h. After the reaction, the product was centrifuged and washed and then dried to obtain vinyl-terminated graphene oxide (HEMA@GO).
[0043] Example 6
[0044] 0.1 g TGO and 30 mL DMSO were placed in a digestion tube, sealed after nitrogen was introduced, and dispersed under ultrasound for 0.5 h; 10 mL hydroxyethyl methacrylate (HEMA) and 30 mL DMSO were placed in a single-hole flask, stirred and heated to 80 ° C, and then the TGO dispersion was added dropwise to the hydroxyethyl methacrylate mixed solution, and 4 drops of DBTDL were added, and the reaction was carried out under nitrogen atmosphere for 10 h. After the reaction, the product was centrifuged and washed and then dried to obtain vinyl-terminated graphene oxide (HEMA@GO).
[0045] Example 7
[0046] 0.1 g TGO and 30 mL DMSO were placed in a digestion tube, sealed after nitrogen was introduced, and dispersed under ultrasound for 0.5 h; 10 mL hydroxyethyl methacrylate (HEMA) and 30 mL DMSO were placed in a single-hole flask, stirred and heated to 70 ° C, and then the TGO dispersion was added dropwise to the hydroxyethyl methacrylate mixed solution, and 4 drops of DBTDL were added, and the reaction was carried out under nitrogen atmosphere for 8 h. After the reaction, the product was centrifuged and washed and then dried to obtain vinyl-terminated graphene oxide (HEMA@GO).
[0047] Example 8
[0048] 0.1 g TGO and 30 mL DMSO were placed in a digestion tube, sealed after nitrogen was introduced, and dispersed under ultrasound for 0.5 h; 10 mL hydroxyethyl methacrylate (HEMA) and 30 mL DMSO were placed in a single-hole flask, stirred and heated to 70 ° C, and then the TGO dispersion was added dropwise to the hydroxyethyl methacrylate mixed solution, and 4 drops of DBTDL were added, and the reaction was carried out under a nitrogen atmosphere for 12 h. After the reaction, the product was centrifuged and washed and then dried to obtain vinyl-terminated graphene oxide (HEMA@GO).
[0049] Example 9
[0050] Take 0.2 parts of HEMA@GO and mix it with 20 parts of carbon black, then mix it evenly with 100 parts of fluororubber matrix on an open mill, then add 4.5 parts of vulcanizer DBPH and 6 parts of co-vulcanizer TAIC in sequence, and then roll and triangle pack it to get the mixed rubber, place it for 24 hours, vulcanize it at 170°C for 5 minutes, and then post-vulcanize it at 200°C for 12 hours to obtain FKM / HEMA@GO composite material.
[0051] Example 10
[0052] Take 0.5 parts of HEMA@GO and mix it with 20 parts of carbon black, then mix it evenly with 100 parts of fluororubber matrix on an open mill, then add 4.5 parts of vulcanizer DBPH and 6 parts of co-vulcanizer TAIC in sequence, and then roll and triangle pack it to obtain the mixed rubber, place it for 24 hours, vulcanize it at 170°C for 5 minutes, and then post-vulcanize it at 200°C for 12 hours to obtain FKM / HEMA@GO composite material.
[0053] Embodiment 11
[0054] Take 1 part of HEMA@GO and mix it with 20 parts of carbon black, then mix it evenly with 100 parts of fluororubber matrix on an open mill, then add 4.5 parts of vulcanizer DBPH and 6 parts of co-vulcanizer TAIC in sequence, and then roll and triangle pack it to obtain the mixed rubber, place it for 24 hours, vulcanize it at 170°C for 5 minutes, and then post-vulcanize it at 200°C for 12 hours to obtain FKM / HEMA@GO composite material.
[0055] Comparative Example 1
[0056] Take 30mL DMSO solution and 4 drops of DBTDL and pour them into a 100mL single-necked flask, and stir at 65°C; take another 0.1g GO powder and put it in a digestion tube, add 30mL DMSO solution to the digestion tube with GO powder, shake it to mix, and ultrasonicate it for 0.5h. After the ultrasonication is completed, slowly add the GO dispersion into the single-necked flask, stir it at 65°C for 7h in a nitrogen atmosphere, and after the stirring is completed, the product is centrifuged and washed and dried to obtain a GO powder comparison sample.
[0057] Comparative Example 2
[0058] Take 20 parts of carbon black and mix them with 100 parts of fluororubber matrix on an open mill. Then add 4.5 parts of vulcanizer DBPH and 6 parts of co-vulcanizer TAIC in sequence. Then roll and triangle pack the mixture. After the mixed rubber is obtained, place it for 24 hours, vulcanize it at 170°C for 5 minutes, and then post-vulcanize it at 200°C for 12 hours to obtain the FKM composite material.
[0059] Comparative Example 3
[0060] Take 0.5 parts of GO and mix it with 20 parts of carbon black, then mix it evenly with 100 parts of fluororubber matrix on an open mill, then add 4.5 parts of vulcanizer DBPH and 6 parts of co-vulcanizer TAIC in sequence, and then roll it and make a triangle package to get the mixed rubber. After that, let it stand for 24 hours, vulcanize it at 170°C for 5 minutes, and then post-vulcanize it at 200°C for 12 hours to obtain the FKM / GO composite material.
[0061] Performance Testing
[0062] The materials obtained in the above comparative example 1 and examples 1-9 were subjected to infrared spectroscopy (FT-IR) test and X-ray diffraction (XRD) test. The test methods are as follows. The results are shown in Table 1.
[0063] Infrared spectrum (FT-IR) test: TENSOR II infrared spectrometer produced by Bruker Optical Instruments was used for infrared spectrum analysis. KBr crystal powder tablet method was used to test in a vacuum environment, and the test range was 500-4000cm -1 The infrared spectra of GO, TGO and HEMA@GO are shown in Figure 2. Figure 3 As shown. Figure 3 It can be seen that after GO is grafted with toluene diisocyanate, the TGO material has a wavelength of 2268 cm -1 An obvious new infrared peak appeared at the position, which was attributed to the successful grafting of TDI and the successful retention of another -NCO functional group, indicating that the isocyanate-grafted graphene oxide was successfully prepared, and after the re-grafting reaction with HEMA, the -NCO infrared peak disappeared.
[0064] X-ray diffraction (XRD) test: DMAX2500 / PC X-ray diffractometer, scanning speed 5° / min, scanning range 3°~60°, the corresponding relationship between 2θ and interlayer spacing follows the Bragg equation: 2dsinθ=nλ. The XRD patterns of GO, TGO and HEMA@GO are shown in Figure 4 As shown. Figure 4 It can be seen that after GO was grafted with TDI, its 2θ diffraction angle decreased, and after being grafted with HEMA, 2θ was reduced to 4.10 again. According to the Bragg equation, it can be calculated that the interlayer spacing of vinyl-terminated graphene oxide has expanded to 2.15nm.
[0065] Thermogravimetric (TGA) analysis: The thermal stability of the graphene oxide powder before and after modification was analyzed using a TGASTA449C thermogravimeter produced by NETZSCH, Germany. The temperature was raised from room temperature to 600°C at a rate of 10°C / min in a N2 atmosphere, and the grafting rate of hydroxyethyl methacrylate (HEMA) was calculated using the weight loss rate.
[0066] Table 1 2θ angle, interlayer spacing and grafting rate of GO and functionalized graphene oxide
[0067]
[0068] From the data in Table 1, it can be seen that the interlayer spacing of graphene oxide can be expanded to varying degrees by grafting modification of graphene oxide with diisocyanate. The interlayer spacing of MGO and IGO is larger than that of TGO, but the two -NCO groups in MDI have the same activity and can react with the hydroxyl groups on GO, making it difficult to prepare -NCO-terminated graphene. IPDI has a low -NCO grafting rate due to its low reactivity. The interlayer spacing of TGO obtained reaches 1.40nm, and the grafting rate of its -NCO group reaches 79.5%, showing the strongest reactivity. Figure 3 It can be observed that after the -NCO-terminated TGO reacts with HEMA, the -NCO infrared peak disappears, and Figure 4 The 2θ peak in the middle further shifted to the left, confirming the successful grafting modification of GEMA and TGO powder. The grafting reaction carried out at 70°C for 10 h can expand the interlayer spacing of the obtained HEMA@GO to 2.15 nm, and the grafting rate of HEMA reached 87.6%, showing strong reaction ability and enhancement effect, further enhancing its dispersibility in the FKM matrix, which is beneficial to its enhancement and anti-aging properties. For the preparation reaction of HEMA@GO, when the temperature increases, although the reaction rate can be accelerated, it will also lead to increased volatilization of HEMA, which may easily cause safety hazards.
[0069] The performance of the materials obtained in the above comparative examples 2-3 and embodiments 9-11 was tested. The test method is as follows. The results are shown in Table 2.
[0070] Mechanical properties test: According to GB / T16584-1996, AL-7000M uses MZ-4000 tensile testing machine with a tensile rate of 500mm / min to test the mechanical properties.
[0071] Hot air aging test: FKM / HEMA@GO composite materials were cut into dumbbell strips and aged by hot air at 180°C. After a certain period of time, they were taken out for mechanical property testing.
[0072] Table 2 Effect of aging time on the aging behavior of the tensile strength of FKM / HEMA@GO composites
[0073]
[0074] Aging conditions: 180℃ thermal oxygen aging
[0075] From the data in Table 2, it can be seen that the unmodified GO has a weak effect on improving the aging resistance of FKM. In comparison, the modified HEMA@GO composite modification of FKM has a greater improvement in the anti-aging functionality of FKM. It can be seen that the tensile strength of pure FKM decreases rapidly under high temperature conditions, and the tensile strength retention rate of the material aged for 6 days is only 57.45%. The mechanical properties of the FKM composite material with 0.2 parts of HEMA@GO addition are improved compared with FKM and GO / FKM materials. The tensile strength retention rate of the material aged for 6 days is 87.96%. Although the mechanical properties of the FKM composite material with 1 part of HEMA@GO addition fluctuate within 6 days of aging, the overall mechanical properties are relatively stable. The FKM composite material with 0.5 parts of HEMA@GO addition has a good mechanical property retention rate, and the tensile strength retention rate of the material aged for 6 days is 105.02%, showing the best aging resistance.
Claims
1. Functional graphene oxide, characterized in that: The 2θ of the functional graphene oxide was 4.1-4.77° and the interlayer spacing was 1.85-2.15nm when tested by an X-ray diffractometer at a scanning speed of 5° / min and a scanning range of 3° to 60°. In addition, the grafting rate of the vinyl functional group measured from room temperature to 600°C under a N2 atmosphere was 53.5-87.6%.
2. The method for preparing functional graphene oxide according to claim 1, characterized in that: The following steps are involved: The graphene oxide grafted with isocyanate was dissolved in dimethyl sulfoxide, and nitrogen was introduced and sealed, and ultrasonic dispersion was performed uniformly. Hydroxyethyl methacrylate is stirred and heated in the presence of a sufficient amount of dimethyl sulfoxide solvent, and then the above dispersion is added dropwise, and 2-3 drops of catalyst dibutyltin dilaurate are added, and grafting modification is carried out under a nitrogen atmosphere to obtain vinyl-terminated graphene oxide, i.e., functional graphene oxide.
3. The method for preparing functional graphene oxide according to claim 2, characterized in that: The mass ratio of graphene oxide grafted with isocyanate to dimethyl sulfoxide is 1:500-1:800, preferably 1:600; The mass ratio of isocyanate-grafted graphene oxide to hydroxyethyl methacrylate is 1:50-1:150, preferably 1:
100.
4. The method for preparing functional graphene oxide according to claim 2, characterized in that: The stirring and heating temperature ranges from 60 to 80° C., preferably 70° C.; the grafting modification reaction time is 8 to 12 hours, preferably 10 hours.
5. The method for preparing functional graphene oxide according to claim 2, characterized in that: Graphene oxide grafted with isocyanate is prepared by the following method: Graphene oxide GO is dissolved in a dimethyl sulfoxide solution, and after ultrasonic mixing, it is slowly added dropwise into a modification solution with diisocyanate as a modifier, dibutyltin dilaurate as a catalyst, and a dimethyl sulfoxide solution as a solvent. The graphene oxide GO is grafted with diisocyanate under a nitrogen atmosphere. After the reaction is completed, it is centrifuged, washed, and dried to obtain graphene oxide grafted with isocyanate.
6. The method for preparing functional graphene oxide according to claim 5, characterized in that: The mass ratio of graphene oxide GO to dimethyl sulfoxide solution is 1:500-1:800, preferably 1:600; The mass ratio of diisocyanate, dibutyltin dilaurate and dimethyl sulfoxide solution in the modified solution is 1:5-1:8, preferably 1:6; The mass ratio of graphene oxide GO to diisocyanate in the modified solution is 1:50-1:150, preferably 1:10; The reaction is carried out in a nitrogen atmosphere at 50-90°C for 5-9 hours, preferably at 65°C for 7 hours.
7. The method for preparing functional graphene oxide according to claim 5, characterized in that: The diisocyanate is selected from at least one of isophorone diisocyanate IPDI, toluene diisocyanate TDI and 4,4-diisocyanate diphenylmethane MDI, preferably toluene diisocyanate TDI.
8. Rubber material, characterized in that It is prepared using the functional graphene oxide described in claim 1.
9. The rubber material according to claim 8, characterized in that The following steps are involved: Functional graphene oxide powder is mixed with carbon black and then kneaded evenly with a fluororubber matrix on an open mill, and then a vulcanizing agent and a vulcanizing agent are added in sequence to obtain a mixed rubber, which is vulcanized after standing to obtain a fluororubber / vinyl-terminated functional graphene oxide composite material, i.e., a rubber material.
10. The rubber material according to claim 8 or 9, characterized in that: The amount of functional graphene oxide powder added to the rubber material is 0.2-1 part by weight.
Citation Information
Cited By
Graphene modified epoxy resin composite anticorrosive paint and preparation method thereof
CN119391268A
Protective wear-resistant long-life silicone rubber and preparation method thereof
CN119432082A
A protective wear-resistant long-life silicone rubber and its preparation method
CN119432082B