Flexible rubber roller sleeve for charging roller, preparation process of flexible rubber roller sleeve and charging roller
By using a combination of EPDM rubber and nitrile rubber in the charging roller and adding conductive carbon black, oil-resistant agent, anti-aging agent and other ingredients, the problem of insufficient anti-aging performance of the charging roller is solved, and the oil resistance and anti-aging are improved. properties, extending service life.
Patent Information
- Application Number
- CN202411052474.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-22
AI Technical Summary
The existing charging roller's anti-aging performance is insufficient, especially at high temperatures, it is prone to molecular chain breakage and oxidative aging, and its tolerance to oil substances is not strong enough, resulting in dimensional changes and reduced printing quality.
Use a combination of 20-30 parts by weight of EPDM rubber and 70-80 parts by weight of nitrile rubber, add 5-15 parts by weight of conductive carbon black, 1-3 parts by weight of accelerator, 2-4 parts by weight of activator, 1.5 ~ 2.5 parts by weight of vulcanizing agent, 1.5-2.5 parts by weight of oil-resistant agent, 1-3 parts by weight of anti-aging agent and 20-30 parts by weight of fillers are used to improve the oil resistance and aging resistance of the rubber through vulcanization treatment and preparation process.
The oil resistance and anti-aging properties of the flexible rubber roller cover for charging rollers are significantly improved, the rubber aging process is delayed, and the physical and mechanical properties and service life are enhanced.
Smart Images

Figure BDA0004975318900000071 
Figure BDA0004975318900000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of charging rollers, and in particular to a flexible rubber roller cover for a charging roller and a preparation process thereof, and a charging roller. Background Art
[0002] The charging roller is a new environmentally friendly charging method. This method reduces the generation of ozone, charges evenly and is noiseless. It is widely used in laser printers and low-speed copiers. During the printing process, a large amount of ink is absorbed on the surface of the rubber roller. When the printing is stopped, aliphatic hydrocarbon oil is often used to clean the surface of the rubber roller, so the rubber roller needs to have strong oil resistance. This is mainly because the rubber roller with poor oil resistance is easy to expand or shrink, resulting in dimensional changes and affecting printing.
[0003] A Chinese invention patent with publication number CN105367840A discloses a rubber roller with antistatic function, comprising natural latex and water, characterized in that 10-15 parts of EPDM rubber, 5-10 parts of modified PVC resin, 5-10 parts of emulsified liquid paraffin, and 5-10 parts of magnesium hydroxide are also added.
[0004] The rubber roller has insufficient anti-aging performance, and is prone to molecular chain breakage and oxidation aging at high temperatures, resulting in a decline in its performance; the rubber roller is not tolerant enough to oily substances, and grease penetrates into the rubber material, accelerating rubber aging. Summary of the invention
[0005] In order to improve the aging resistance and oil resistance of the rubber roller and enhance the printing quality, the present application provides a flexible rubber roller cover for a charging roller.
[0006] The present application provides a flexible rubber roller cover for a charging roller, which adopts the following technical solution: A flexible rubber roller cover for a charging roller, the flexible rubber roller cover for the charging roller is made of the following components in parts by weight: 20 to 30 parts by weight of EPDM rubber, 70 to 80 parts by weight of nitrile rubber, 5 to 15 parts by weight of conductive carbon black, 1 to 3 parts by weight of an accelerator, 2 to 4 parts by weight of an active agent, 1.5 to 2.5 parts by weight of a vulcanizing agent, 1.5 to 2.5 parts by weight of an oil resistant agent, 1 to 3 parts by weight of an anti-aging agent, and 20 to 30 parts by weight of a filler; The oil-resistant agent is at least one of oleamide, erucamide and stearamide; The anti-aging agent is at least one of sodium thiosulfate and ammonium thiosulfate.
[0007] By adopting the above technical scheme, EPDM rubber and nitrile rubber have good compatibility and can improve the oil resistance and aging resistance of rubber; conductive carbon black has a smaller particle size and a larger specific surface area, which can be better dispersed in rubber materials and improve the conductivity. Rubber accelerators can accelerate the degree of crosslinking between vulcanizers and rubber molecules, activate rubber molecular chains, and make rubber molecules more likely to interact with fillers. The activator can increase the activity of the accelerator and further improve the vulcanization speed and vulcanization efficiency. The oil-resistant agent can form a lipophilic interaction with the ink molecules, thereby increasing the viscosity of the ink, thereby effectively preventing oil substances from penetrating into the material; the oil-resistant agent can also increase the crosslinking density between rubber molecules, reduce the penetration of ink molecules, improve the oil resistance of rubber, and thus improve the aging resistance of rubber. Anti-aging agents delay the aging process by capturing free radicals and inhibiting the physical and chemical effects of oxidation reactions, thereby achieving a mitigating effect on rubber aging. Thiosulfate is both oxidizing and reducing. On the one hand, it can capture free radicals generated in rubber materials, thereby inhibiting the reaction initiated by free radicals; on the other hand, it can react with free radicals in oxygen and convert them into inactive substances, thereby preventing the oxidation reaction.
[0008] The accelerator comprises N-cyclohexyl-2-benzothiazole sulfenamide and tetrabenzylthiuram disulfide, and the mass ratio of the N-cyclohexyl-2-benzothiazole sulfenamide to the tetrabenzylthiuram disulfide is 1:0.1-0.5.
[0009] By adopting the above technical scheme, the scorch time of tetrabenzylthiuram disulfide accelerator is very short, and vulcanization can be completed in a short time. The scorch time of N-cyclohexyl-2-benzothiazolesulfonamide is long, the vulcanization start is fast, there is flatness, and the performance is good. The combination of the two can improve the scorch safety and the rubber vulcanization reaction rate, and improve the physical and mechanical properties of the vulcanized rubber.
[0010] Preferably, the active agent includes an organic active agent and an inorganic active agent, the organic active agent is at least one of benzoic acid and stearic acid, and the inorganic active agent is zinc oxide; the mass ratio of the organic active agent to the inorganic active agent is (0.2-0.4):1.
[0011] By adopting the above technical solution, benzoic acid, as an active compound, can promote the vulcanization reaction of rubber. At the same time, benzoic acid can also promote the reaction between the vulcanizer and the rubber molecules to improve the vulcanization efficiency. Benzoic acid also has the effect of enhancing the hardness and wear resistance of rubber. The principle is that benzoic acid molecules can be decomposed into benzene and formic acid during heating, and benzene molecules can form chemical bonds with rubber molecules, thereby improving the strength and hardness of rubber; formic acid molecules can disrupt the fiber structure on the surface of rubber, making it smoother, thereby improving the wear resistance of rubber.
[0012] Stearic acid has an activation effect, and it has an acidic activation effect on the double bonds of rubber molecules, thereby accelerating the formation of cross-linking bonds and increasing the cross-linking density of vulcanized rubber. Zinc oxide can react with the vulcanizing agent in rubber to promote the cross-linking reaction, enhance the degree of vulcanization of rubber, and improve the strength, hardness, elasticity and wear resistance of rubber. At the same time, it can also increase the tensile and tear strength of rubber and increase the service life of rubber products.
[0013] Preferably, the vulcanizing agent is sulfur or zinc sulfide, and the mass ratio of sulfur to zinc sulfide is 1:1-2.
[0014] By adopting the above technical solution, sulfur plays a key role in the rubber vulcanization process. It can cross-link the rubber molecular chains to form a network structure. This transformation improves the physical properties of rubber, such as heat resistance, aging resistance and mechanical properties. Zinc sulfide, as a rubber additive, is mainly used to assist the vulcanization reaction of rubber and promote chemical cross-linking between rubber molecules, thereby enhancing the physical properties and heat resistance of rubber. Zinc sulfide can also stabilize the performance of rubber and prevent rubber aging, deterioration and decomposition. At the same time, zinc sulfide is also a UV absorber, which can effectively prevent UV aging of rubber products.
[0015] Preferably, the filler is at least one of titanium dioxide, carbon black, aluminum silicate and calcium silicate.
[0016] By adopting the above technical scheme, the addition of titanium dioxide, carbon black, aluminum silicate and calcium silicate can improve the lipophilicity and heat resistance of rubber. The lipophilicity of titanium dioxide is mainly due to the presence of a large number of hydroxyl (-OH) and oxide (=O) functional groups on its surface. These functional groups can react with oily molecules such as hydrogen bonds, thereby inducing the oily molecules to arrange on the surface of titanium dioxide and reducing the penetration of oil. Carbon black, due to its high lipophilicity, can form an oily composite structure in rubber, thereby improving the oil resistance of rubber. Aluminum silicate and calcium silicate can absorb oil and solvent in rubber, reduce the expansion and dissolution of rubber, and improve the weather resistance and corrosion resistance of rubber. In addition, aluminum silicate can also absorb oxygen molecules in rubber, reduce the contact between oxygen and rubber, delay the oxidation process of rubber, and improve the antioxidant performance of rubber. Titanium dioxide, carbon black, aluminum silicate and calcium silicate can also improve the thermal conductivity of rubber, thereby improving the thermal stability and anti-aging performance of rubber.
[0017] Preferably, the components further include 5 to 15 parts by weight of aluminum starch octenylsuccinate.
[0018] By adopting the above technical scheme, aluminum starch octenylsuccinate can react with double bonds in rubber chains to promote the cross-linking reaction of rubber, thereby improving the mechanical properties of rubber; it can also catalyze the cross-linking reaction of rubber molecules, accelerate the cross-linking speed of rubber, and shorten the vulcanization time of rubber.
[0019] The present application also provides a process for preparing a flexible rubber roller cover for a charging roller, comprising the following steps: S1: feeding EPDM rubber and nitrile rubber into an internal mixer in proportion and mixing them evenly, then adding conductive carbon black, oil resistance agent, filler, anti-aging agent, filler and activator, and mixing and heating at the same time to obtain a primary rubber compound; S2: After adding the primary rubber material to the mixing mill, adding the accelerator and the vulcanizing agent, mixing and mixing together, extruding and molding, and obtaining the primary rubber roller cover; S3: vulcanizing the primary rubber sleeve, and cutting the vulcanized rubber roller sleeve into suitable lengths.
[0020] Preferably, in step S2, 5 to 15 parts by weight of aluminum starch octenylsuccinate are also added.
[0021] The present application also provides a charging roller, comprising a conductive roller core and a flexible rubber roller cover covering the outside of the conductive roller core, wherein the flexible rubber roller cover is made by the above-mentioned preparation process of the flexible rubber roller cover for the charging roller.
[0022] In summary, the present application includes at least one of the following beneficial technical effects: 1. By introducing oil-resistant agent and anti-aging agent, the oil-resistant and anti-aging properties of the flexible rubber roller cover for charging roller are improved. This is because the oil-resistant agent can form lipophilic interactions with ink molecules, thereby increasing the viscosity and fluidity of the ink, thereby effectively preventing oil substances from penetrating into the material; the oil-resistant agent can also increase the cross-linking density between rubber molecules, reduce the penetration of ink molecules, and thus improve the anti-aging properties of rubber. Anti-aging agents delay the aging process by capturing free radicals and inhibiting the physical and chemical effects of oxidation reactions, thereby achieving a mitigating effect on rubber aging.
[0023] 2. The addition of fillers not only improves the strength of the rubber roller cover, but also further improves the oil resistance and heat resistance of the flexible rubber roller cover. DETAILED DESCRIPTION
[0024] The present application is further described in detail below in conjunction with embodiments.
[0025] Example 1 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 20kg EPDM rubber, 80kg nitrile rubber, 5kg conductive carbon black, 1kg accelerator, 2kg activator, 1.5kg vulcanizer, 1.5kg oil resistant agent, 1kg anti-aging agent and 20kg filler; The accelerator is 0.91kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.09kg tetrabenzylthiuram disulfide; the activator is 0.33kg benzoic acid and 1.67kg zinc oxide; the vulcanizing agent is 0.75kg sulfur and 0.75kg zinc sulfide; the oil-resistant agent is oleic acid amide; the anti-aging agent is sodium thiosulfate; the filler is titanium dioxide; The method for preparing the flexible rubber roller cover for the charging roller of this embodiment comprises the following steps: S1: Weigh the EPDM rubber and the NBR rubber according to the above weights and mix them in an internal mixer for 5 minutes, then add the above weights of conductive carbon black, oil resistant agent, filler, anti-aging agent, filler and activator; mix at 160°C for 15 minutes to obtain a primary rubber compound; S2: conveying the primary rubber material to an open mill, adding the above-mentioned weight of accelerator and vulcanizer, and mixing on the open mill for 10 minutes to obtain an extrudate, conveying the extrudate to an extruder, extruding and molding, and obtaining a primary rubber roller cover; S3: The primary rubber roller sleeve is continuously conveyed to a tunnel type vulcanization furnace for vulcanization at 230° C. The conveying speed of the primary rubber roller sleeve in the vulcanization furnace is 10 m / min. The vulcanized rubber roller sleeve is cut into suitable lengths.
[0026] In step S2, the temperature of the extruder process is divided into three sections (feeding section, compression section, metering section), and the temperatures are set to 60° C., 65° C., and 65° C. The temperatures at the latter two ends are the same, so that the extrudate has a stable preheating process.
[0027] The preparation method of the charging roller of this embodiment includes the following steps: sleeve the flexible rubber roller sleeve on the conductive roller core, dry it, cut the flexible rubber roller sleeve sleeved on the conductive roller core, grind, clean and dry it, spray and dry it.
[0028] The method for preparing the slurry used in spraying comprises the following steps: 3 g of graphene powder was ultrasonically dispersed in 1000 ml of N,N-dimethylamide, and then 100 g of aqueous polyurethane emulsion was added to the above graphene solution and stirred at high speed for 15 min to obtain a uniform slurry.
[0029] Example 2 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 30kg EPDM rubber, 70kg nitrile rubber, 15kg conductive carbon black, 3kg accelerator, 4kg activator, 2.5kg vulcanizer, 2.5kg oil resistant agent, 3kg anti-aging agent and 30kg filler; The accelerator is 2.73kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.27kg tetrabenzylthiuram disulfide; the activator is 0.67kg benzoic acid and 3.33kg zinc oxide; the vulcanizing agent is 1.25kg sulfur and 1.25kg zinc sulfide; the oil-resistant agent is oleic acid amide; the anti-aging agent is sodium thiosulfate; the filler is titanium dioxide; The rest is the same as in Example 1.
[0030] Example 3 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 25kg EPDM rubber, 75kg nitrile rubber, 10kg conductive carbon black, 2kg accelerator, 3kg activator, 2kg vulcanizer, 2kg oil resistant agent, 2kg anti-aging agent and 25kg filler; The accelerator is 1.82kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.18kg tetrabenzylthiuram disulfide; the activator is 0.5kg benzoic acid and 2.5kg zinc oxide; the vulcanizing agent is 1kg sulfur and 1kg zinc sulfide; the oil-resistant agent is oleic acid amide; the anti-aging agent is sodium thiosulfate; the filler is titanium dioxide; The rest is the same as in Example 2.
[0031] Example 4 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 25kg EPDM rubber, 75kg nitrile rubber, 10kg conductive carbon black, 2kg accelerator, 3kg activator, 2kg vulcanizer, 2kg oil resistant agent, 2kg anti-aging agent and 25kg filler; The accelerator is 1.33kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.67kg tetrabenzylthiuram disulfide; the activator is 0.5kg benzoic acid, 2.14kg zinc oxide and 0.36kg stearic acid; the vulcanizer is 0.5kg sulfur and 1.5kg zinc sulfide; the oil-resistant agent is 1kg oleamide and 1kg erucamide; the anti-aging agent is sodium thiosulfate; the filler is 10kg titanium dioxide and 15kg carbon black; The rest is the same as in Example 3.
[0032] Example 5 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 25kg EPDM rubber, 75kg nitrile rubber, 10kg conductive carbon black, 2kg accelerator, 3kg activator, 2kg vulcanizer, 2kg oil resistant agent, 2kg anti-aging agent and 25kg filler; The accelerator is 1.54kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.67kg tetrabenzylthiuram disulfide; the activator is 0.5kg benzoic acid, 2.31kg zinc oxide and 0.19kg stearic acid; the vulcanizing agent is 0.8kg sulfur and 1.2kg zinc sulfide; the oil-resistant agent is 2kg erucamide; the anti-aging agent is ammonium thiosulfate; the filler is 10kg titanium dioxide, 10kg carbon black, and 5kg calcium silicate; The rest is the same as Example 4.
[0033] Example 6 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 25kg EPDM rubber, 75kg nitrile rubber, 10kg conductive carbon black, 2kg accelerator, 3kg activator, 2kg vulcanizer, 2kg oil resistant agent, 2kg anti-aging agent and 25kg filler; The accelerator is 1.54kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.67kg tetrabenzylthiuram disulfide; the activator is 0.36kg benzoic acid, 2.14kg zinc oxide and 0.5kg stearic acid; the vulcanizer is 0.8kg sulfur and 1.2kg zinc sulfide; the oil-resistant agent is 1kg erucic acid amide and 1kg stearic acid amide; the anti-aging agent is ammonium thiosulfate; the filler is 10kg titanium dioxide, 10kg carbon black, and 5kg calcium silicate; The rest is the same as Example 5.
[0034] Example 7 This embodiment provides a flexible rubber roller cover for a charging roller, which mainly includes the following components by weight: 25kg EPDM rubber, 75kg nitrile rubber, 10kg conductive carbon black, 2kg accelerator, 3kg activator, 2kg vulcanizer, 2kg oil resistant agent, 2kg anti-aging agent and 25kg filler; The accelerator is 1.54kg N-cyclohexyl-2-benzothiazole sulfenamide and 0.67kg tetrabenzylthiuram disulfide; the activator is 0.36kg benzoic acid, 2.14kg zinc oxide and 0.5kg stearic acid; the vulcanizing agent is 0.8kg sulfur and 1.2kg zinc sulfide; the oil-resistant agent is 2kg stearic acid amide; the anti-aging agent is 1kg thiosulfate ammonium and 1kg sodium thiosulfate; the filler is 10kg titanium dioxide, 10kg carbon black, 5kg aluminum silicate; The rest is the same as Example 6.
[0035] Example 8 The difference between this embodiment and embodiment 7 is that the components of the flexible rubber roller cover for the charging roller also include 5 kg of aluminum starch octenyl succinate; In step S2, when the accelerator and the vulcanizing agent are added, aluminum starch octenyl succinate is also added.
[0036] The rest is the same as Example 7.
[0037] Example 9 The difference between this embodiment and embodiment 8 is that the components of the flexible rubber roller cover for the charging roller further include 10 kg of aluminum starch octenylsuccinate.
[0038] The rest is the same as Example 8.
[0039] Example 10 The difference between this embodiment and embodiment 9 is that the components of the flexible rubber roller cover for the charging roller further include 15 kg of aluminum starch octenylsuccinate.
[0040] The rest is the same as Example 9.
[0041] Comparative Example 1 The difference between this comparative example and Example 10 is that no oil resistant agent is added.
[0042] The rest is the same as Example 10.
[0043] Comparative Example 2 The difference between this comparative example and Example 10 is that no anti-aging agent is added.
[0044] The rest is the same as Example 10.
[0045] Comparative Example 3 The difference between this comparative example and Example 10 is that no oil-resistant agent and anti-aging agent are added.
[0046] The rest is the same as Example 10.
[0047] Performance Testing 1. The flexible rubber roller covers in Examples 1 to 10 and Comparative Examples 1 to 3 were tested for tensile strength and elongation at break according to GB / T528-2009 standard; 2. First, the flexible rubber roller sleeves in Examples 1 to 12 and Comparative Examples 1 to 3 were coated with ink multiple times and kept in a wet state for 18 hours. After 18 hours, they were cleaned with ethyl acetate and dried. Then, they were placed in a heat aging test box at 150° C. for 72 hours in accordance with GB / T 3512-2014 standard, and the tensile strength and elongation at break after aging were tested.
[0048] Table 1 Performance test data of the flexible rubber roller sleeves in Examples 1 to 10 and Comparative Examples 1 to 3 By comparing and analyzing the test data of Examples 1 to 3 and Comparative Examples 1 to 3, it can be seen that by optimizing and adjusting the dosage of the oil resistant agent, the anti-aging agent and the filler, the prepared flexible rubber roller sleeve has good anti-aging performance.
[0049] Comparative analysis of the test data of Examples 3 to 7 shows that the anti-aging performance of the flexible rubber roller sleeve is enhanced by optimizing and adjusting the types of oil-resistant agents, anti-aging agents and fillers. This is mainly because oleamide, erucic acid amide and stearic acid amide can cross-link with rubber molecules on the one hand, increase the cross-linking density of rubber, thereby reducing the gap between the molecules of the finished rubber product, thereby greatly reducing the penetration of ink molecules; on the other hand, they can form lipophilic interactions with pigment molecules, thereby increasing the viscosity of the ink, reducing the penetration of grease molecules into the rubber material, and reducing rubber aging and failure. It can also enhance the anti-friction performance of the rubber material surface, improve the wear resistance of rubber, and extend the service life of rubber materials.
[0050] The thermal stability of erucamide is better than that of oleamide. The addition of erucamide further improves the thermal stability of rubber, thereby improving the anti-aging performance of rubber. The thermal stability of stearic acid amide is better than that of erucic acid amide. Stearic acid amide has a long-chain fatty alkyl group, which makes stearic acid amide highly lipophilic, reduces the penetration of ink, and thereby improves the anti-aging performance of rubber.
[0051] Carbon black not only helps rubber resist oxidation and decomposition, but also forms an oily composite structure in rubber, which improves the rubber's oil resistance and thus improves the rubber's aging resistance. Aluminum silicate and calcium silicate can absorb oil and solvents in rubber, reduce rubber expansion and dissolution, improve rubber's weather resistance and corrosion resistance, and thus improve rubber's aging resistance.
[0052] By comparing and analyzing the test data of Examples 7-10, it can be seen that aluminum starch octenylsuccinate can react with double bonds in the rubber chain to increase the cross-linking density of the rubber, increase the chemical bonds between the rubber molecules, and make the molecular structure more compact, thereby making the interaction between the molecules stronger, thereby further improving the aging resistance of the rubber.
Claims
1. A flexible rubber roller cover for a charging roller, characterized in that: The flexible rubber roller cover for the charging roller is made of the following components in parts by weight: 20-30 parts by weight of EPDM rubber, 70-80 parts by weight of nitrile rubber, 5-15 parts by weight of conductive carbon black, 1-3 parts by weight of accelerator, 2-4 parts by weight of active agent, 1.5-2.5 parts by weight of vulcanizing agent, 1.5-2.5 parts by weight of oil resistant agent, 1-3 parts by weight of anti-aging agent, and 20-30 parts by weight of filler; The oil-resistant agent is at least one of oleamide, erucamide and stearamide; The anti-aging agent is at least one of sodium thiosulfate and ammonium thiosulfate.
2. The flexible rubber roller cover for the charging roller according to claim 1, characterized in that: The accelerator comprises N-cyclohexyl-2-benzothiazole sulfenamide and tetrabenzylthiuram disulfide, and the mass ratio of the N-cyclohexyl-2-benzothiazole sulfenamide to the tetrabenzylthiuram disulfide is 1:(0.1-0.5).
3. The flexible rubber roller cover for the charging roller according to claim 1, characterized in that: The active agent comprises an organic active agent and an inorganic active agent, wherein the organic active agent is at least one of benzoic acid and stearic acid, and the inorganic active agent is zinc oxide; the mass ratio of the organic active agent to the inorganic active agent is (0.2-0.4):1, The vulcanizing agent is sulfur and zinc sulfide, and the mass ratio of the sulfur to the zinc sulfide is 1:1-2.
4. The flexible rubber roller cover for the charging roller according to claim 1, characterized in that: The filler is at least one of titanium dioxide, carbon black, aluminum silicate and calcium silicate.
5. The flexible rubber roller cover for the charging roller according to claim 1, characterized in that: The components also include 5 to 15 parts by weight of aluminum starch octenylsuccinate.
6. A process for preparing a flexible rubber roller cover for a charging roller according to any one of claims 1 to 6, characterized in that: The steps include: S1: feeding EPDM rubber and nitrile rubber into an internal mixer in proportion and mixing them evenly, then adding conductive carbon black, oil resistance agent, filler, anti-aging agent, filler and activator, and mixing and heating at the same time to obtain a primary rubber compound; S2: After adding the primary rubber material to the mixing mill, adding the accelerator and the vulcanizing agent, mixing and mixing together, extruding and molding, and obtaining the primary rubber roller cover; S3: vulcanizing the primary rubber sleeve, and cutting the vulcanized rubber roller sleeve into suitable lengths.
7. The process for preparing the flexible rubber roller cover for the charging roller according to claim 7, characterized in that: In step S2, 5 to 15 parts by weight of aluminum starch octenylsuccinate are also added.
8. A charging roller, characterized in that: The charging roller comprises a conductive roller core and a flexible rubber roller cover covering the conductive roller core, wherein the flexible rubber roller cover is prepared by the preparation process of the flexible rubber roller cover for the charging roller according to any one of claims 7 to 8.