Rapidly vulcanized chloroprene rubber material and preparation method thereof

Through reasonable proportioning and vulcanization system design, the use of fast-vulcanizing chloroprene rubber material solves the problem of slow vulcanization speed of existing chloroprene dust cover materials, achieves efficient production and excellent mechanical properties, and enhances market competitiveness.

CN118812937APending Publication Date: 2024-10-22ANHUI ZHONGDING SEALING PARTS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310426979.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The vulcanization speed of existing neoprene dust cover materials is slow, resulting in low production efficiency, and the performance cannot meet high temperature and mechanical performance requirements.

Method used

Uses include CR raw rubber, reinforcing agent, vulcanizing agent, magnesium oxide, aluminum magnesium hydrotalcite, active agent, N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethyl Rapidly vulcanized chloroprene rubber materials made from raw materials such as butyl)-N'-phenyl-p-phenylenediamine and 2-mercaptobenzimidazole can significantly improve the vulcanization speed and mechanical properties through reasonable proportions and vulcanization system design.

Benefits of technology

It significantly improves the vulcanization speed and mechanical properties, meets high-temperature production requirements, and improves the production efficiency and market competitiveness of thin dust cover products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004188798480000071
    Figure BDA0004188798480000071
  • Figure BDA0004188798480000081
    Figure BDA0004188798480000081
Patent Text Reader

Abstract

The invention discloses a rapidly vulcanized chloroprene rubber material which comprises the following raw materials in parts by mass: 45-55 parts of CR raw rubber, 25-35 parts of a reinforcing agent, 1.7-4.5 parts of a vulcanizing agent, 0.5-2.5 parts of magnesium oxide, 1.5-3.5 parts of aluminum-magnesium hydrotalcite, 0.1-0.8 part of an active agent, 0.2-1.5 parts of N-isopropyl-N '-phenyl-p-phenylenediamine, 0.2-1.5 parts of N-(1, 2, 4-trimethyl-1, 3-pentanediol monoisobutyrate) and 0.1-0.8 part of a vulcanizing agent. The invention discloses a rapid vulcanization chloroprene rubber material.The rapid vulcanization chloroprene rubber material has the advantages of being high in vulcanization speed, high in mechanical strength and excellent in water resistance and oil resistance, and product competitiveness is high. The rapid vulcanization chloroprene rubber material comprises, by weight, 20-30 parts of chloroprene rubber, 20-30 parts of chloroprene rubber, 20-30 parts of chloroprene rubber, 0.2-1.5 parts of 2, 3-dimethylbutyl)-N '-phenyl p-phenylenediamine, 0.5-1.5 parts of 2-mercapto benzimidazole, 5-24 parts of plasticizer and 0.2-1.5 parts of acceleration.The invention further discloses a preparation method of the rapid vulcanization chloroprene rubber material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber materials, and in particular to a fast-vulcanizing chloroprene rubber material and a preparation method thereof. Background Art

[0002] The ball head dust cover is used at the connection between the steering tie rod and the steering knuckle arm of the automobile steering gear. Generally, 3-4 grams of grease is installed inside the product. When the car turns during driving, the tie rod ball head pin will continue to rotate and swing. At this time, the dust cover installed at the joint can prevent dust, mud and sand from entering the ball head pin. At the same time, it can effectively reduce the friction at the joint, prevent the tie rod joint from getting stuck or breaking due to long-term wear, and cause steering failure and accidents. It is one of the key parts of the steering system. The product has high requirements for strength, wear resistance, grease resistance, water resistance, low temperature resistance and dynamic fatigue. The chloroprene rubber dust cover products commonly used in the market are mainly non-sulfur adjusted chloroprene rubber, which is vulcanized with zinc oxide, magnesium oxide and ethylene thiourea or other environmentally friendly accelerators. Its vulcanization speed is relatively slow and the production efficiency is low. However, some materials with fast vulcanization speed cannot meet the requirements in terms of performance. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a fast-vulcanizing chloroprene rubber material and a preparation method thereof. The preparation method is simple and convenient, and the obtained chloroprene rubber material has good processing performance, a vulcanization speed is greatly increased compared with conventional chloroprene rubber materials, and has excellent mechanical properties. At the same time, it can meet high-temperature production, greatly improving the production efficiency of thin products such as dust covers, thereby enhancing the competitive advantage of such products in the market.

[0004] A fast-vulcanizing chloroprene rubber material provided by the present invention comprises the following raw materials in parts by weight:

[0005] 45-55 parts of CR raw rubber, 25-35 parts of reinforcing agent, 1.7-4.5 parts of vulcanizing agent, 0.5-2.5 parts of magnesium oxide, 1.5-3.5 parts of aluminum-magnesium hydrotalcite, 0.1-0.8 parts of activator, 0.2-1.5 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.2-1.5 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 0.5-1.5 parts of 2-mercaptobenzimidazole, 5-24 parts of plasticizer, and 0.2-1.5 parts of accelerator.

[0006] Preferably, the vulcanizing agent consists of indirect zinc oxide and ethylene thiourea; preferably, the mass ratio of the indirect zinc oxide to ethylene thiourea is (1.5-3.5): (0.2-1.0).

[0007] Preferably, the plasticizer is dioctyl sebacate, ethylene glycol adipate or a combination thereof; preferably, the plasticizer is composed of dioctyl sebacate and ethylene glycol adipate in a mass ratio of (2-9):(3-15).

[0008] Preferably, the reinforcing agent is quick-pressed black, natural gas semi-reinforcing carbon black or a combination thereof.

[0009] Preferably, the active agent is stearic acid.

[0010] Preferably, the accelerator is tetramethylthiuram disulfide, dibenzothiazole disulfide or a combination thereof.

[0011] Preferably, the CR raw rubber is xanthate-adjusted chloroprene rubber, and the Mooney viscosity is 60-80 under the test conditions of ISO289UML (1+4) 100°C.

[0012] In the present invention, N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 2-mercaptobenzimidazole are compounded as an anti-aging system.

[0013] In the present invention, magnesium oxide and magnesium aluminum hydrotalcite are compounded as an acid absorption and scorch prevention system.

[0014] In the present invention, magnesium oxide and magnesium aluminum hydrotalcite with acid absorption and scorch prevention effects and 2-mercaptobenzimidazole with aging resistance are used in a suitable ratio, and a rapid vulcanization system is formed under a suitable vulcanization system. While greatly improving the vulcanization speed, the chloroprene rubber material also has a good scorch time, solving the problem that the rapid vulcanization chloroprene rubber material is easy to scorch and has poor production and storage safety.

[0015] A method for preparing the fast-vulcanized chloroprene rubber material comprises the following steps:

[0016] S1, weighing raw materials by mass, adding them into an internal mixer for mixing, and then discharging the materials to obtain a mixed rubber;

[0017] S2, refining the mixed rubber, and then vulcanizing and molding to obtain.

[0018] Preferably, in S1, the mixing time is 5-10 min, and the discharge temperature is 90-122°C.

[0019] Preferably, in S2, the temperature of the opening refining is 40-80°C.

[0020] Preferably, in S2, the vulcanization molding temperature is 165-185°C, the time is 150-420s, and the pressure is 140-180Kgf / cm 2 .

[0021] The beneficial effects of the present invention are as follows:

[0022] The invention selects and matches suitable raw materials, reasonably adjusts the proportion of the raw materials, and especially selects appropriate amounts of magnesium oxide and magnesium aluminum hydrotalcite with the antioxidant 2-mercaptobenzimidazole for acid absorption and scorch prevention to match them to achieve an unexpected synergistic and mutually promoting effect. The obtained chloroprene rubber material has not only good processing performance, but also a greatly increased vulcanization speed compared with conventional chloroprene rubber materials, excellent mechanical properties, and can meet high-temperature production requirements, has the advantages of fast vulcanization speed, high scorch safety, good low-temperature performance, excellent water resistance, oil resistance and dynamic fatigue resistance, greatly improves the production efficiency of thin products such as dust covers, and enhances the competitive advantage of such products in the market. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is described in detail below through specific embodiments.

[0024] In the following examples and comparative examples, the CR raw rubber was purchased from Nippon Denka DCR-66, and the Mooney viscosity was 60-80 under the test conditions of ISO289UML (1+4) 100°C.

[0025] Example 1

[0026] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0027] 50 parts of CR raw rubber, 26 parts of quick-pressed black, 2.5 parts of zinc oxide, 1 part of magnesium oxide, 2 parts of hydrotalcite, 0.3 parts of stearic acid, 0.7 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.7 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 1.5 parts of 2-mercaptobenzimidazole, 6 parts of dioctyl sebacate, 8 parts of ethylene glycol adipic acid, 0.5 parts of ethylene thiourea, and 0.5 parts of tetramethylthiuram disulfide.

[0028] Its preparation method is:

[0029] S1, weighing raw materials by mass, adding them into an internal mixer and mixing for 8 minutes, and then discharging the materials at 115° C. to obtain a mixed rubber;

[0030] S2, the mixed rubber is opened and mixed at 45 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 175 ° C, the time is 200s, and the pressure is 150Kgf / cm 2 .

[0031] Example 2

[0032] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0033] 48 parts of CR raw rubber, 28 parts of quick-pressed black, 2.4 parts of zinc oxide, 1 part of magnesium oxide, 1.9 parts of hydrotalcite, 0.2 parts of stearic acid, 0.5 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.5 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 1 part of 2-mercaptobenzimidazole, 6 parts of dioctyl sebacate, 10 parts of ethylene glycol adipic acid, 0.7 parts of ethylene thiourea, and 0.5 parts of tetramethylthiuram disulfide.

[0034] Its preparation method is:

[0035] S1, weighing raw materials by mass, adding them into an internal mixer and mixing for 5 minutes, and then discharging the materials at 90°C to obtain a mixed rubber;

[0036] S2, the mixed rubber is opened and mixed at 65 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 175 ° C, the time is 180s, and the pressure is 155Kgf / cm 2 .

[0037] Example 3

[0038] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0039] 46 parts of CR raw rubber, 4 parts of NBR raw rubber, 30 parts of quick-pressed black, 2.5 parts of zinc oxide, 1.2 parts of magnesium oxide, 2.2 parts of hydrotalcite, 0.4 parts of stearic acid, 0.7 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.5% of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 1.2 parts of 2-mercaptobenzimidazole, 5 parts of dioctyl sebacate, 7 parts of ethylene glycol adipic acid, 0.5 parts of ethylene thiourea, and 0.5 parts of tetramethylthiuram disulfide.

[0040] Its preparation method is:

[0041] S1. Weigh the raw materials by mass, add them into an internal mixer and mix them for 10 minutes, then discharge them at 122° C. to obtain a mixed rubber;

[0042] S2, the mixed rubber is opened and mixed at 60 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 175 ° C, the time is 190s, and the pressure is 160Kgf / cm 2 .

[0043] Example 4

[0044] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0045] 49 parts of CR raw rubber, 27 parts of quick-pressed black, 2.5 parts of zinc oxide, 2 parts of magnesium oxide, 2 parts of hydrotalcite, 0.4 parts of stearic acid, 0.6 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.8 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 1.1 parts of 2-mercaptobenzimidazole, 5 parts of dioctyl sebacate, 7 parts of ethylene glycol adipic acid, 0.5 parts of ethylene thiourea, and 0.4 parts of tetramethylthiuram disulfide.

[0046] Its preparation method is:

[0047] S1, weighing raw materials by mass, adding them into an internal mixer and mixing for 5 minutes, and then discharging the materials at 90°C to obtain a mixed rubber;

[0048] S2, the mixed rubber is opened and mixed at 70 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 165-185 ° C, the time is 210s, and the pressure is 165Kgf / cm 2 .

[0049] Comparative Example 1

[0050] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0051] 50 parts of CR raw rubber, 26 parts of quick-pressed black, 2.5 parts of zinc oxide, 1 part of magnesium oxide, 0.3 parts of stearic acid, 0.7 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.7 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 1.5 parts of 2-mercaptobenzimidazole, 6 parts of dioctyl sebacate, 8 parts of ethylene glycol adipic acid, 0.5 parts of ethylene thiourea, and 0.5 parts of tetramethylthiuram disulfide.

[0052] Its preparation method is:

[0053] S1, weighing raw materials by mass, adding them into an internal mixer and mixing for 8 minutes, and then discharging the materials at 115° C. to obtain a mixed rubber;

[0054] S2, the mixed rubber is opened and mixed at 45 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 175 ° C, the time is 200s, and the pressure is 150Kgf / cm 2 .

[0055] Comparative Example 2

[0056] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0057] 50 parts of CR raw rubber, 26 parts of quick-pressed black, 2.5 parts of zinc oxide, 1 part of magnesium oxide, 2 parts of hydrotalcite, 0.3 parts of stearic acid, 0.7 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.7 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 6 parts of dioctyl sebacate, 8 parts of ethylene glycol adipic acid, 0.5 parts of ethylene thiourea, and 0.5 parts of tetramethylthiuram disulfide.

[0058] Its preparation method is:

[0059] S1, weighing raw materials by mass, adding them into an internal mixer and mixing for 8 minutes, and then discharging the materials at 115° C. to obtain a mixed rubber;

[0060] S2, the mixed rubber is opened and mixed at 45 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 175 ° C, the time is 200s, and the pressure is 150Kgf / cm 2 .

[0061] Comparative Example 3

[0062] A fast-vulcanizing chloroprene rubber material comprises the following raw materials in parts by weight:

[0063] 50 parts of CR raw rubber, 26 parts of quick-pressed black, 2.5 parts of zinc oxide, 2 parts of hydrotalcite, 0.3 parts of stearic acid, 0.7 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.7 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 1.5 parts of 2-mercaptobenzimidazole, 6 parts of dioctyl sebacate, 8 parts of ethylene glycol adipic acid, 0.5 parts of ethylene thiourea, and 0.5 parts of tetramethylthiuram disulfide.

[0064] Its preparation method is:

[0065] S1, weighing raw materials by mass, adding them into an internal mixer and mixing for 8 minutes, and then discharging the materials at 115° C. to obtain a mixed rubber;

[0066] S2, the mixed rubber is opened and mixed at 45 ° C through an open roller mill, and then placed in a mold of a vulcanization equipment for vulcanization molding, wherein the vulcanization molding temperature is 175 ° C, the time is 200s, and the pressure is 150Kgf / cm 2 .

[0067] Test example

[0068] The chloroprene rubber materials obtained in the embodiments and comparative examples were subjected to performance tests, and the test results are shown in Table 1:

[0069] Table 1

[0070]

[0071]

[0072] Based on the raw material formula of Example 1, Comparative Example 1 lacks hydrotalcite, Comparative Example 2 lacks 2-mercaptobenzimidazole, and Comparative Example 3 lacks magnesium oxide. Among them:

[0073] ① Comparative Example 1 lacks hydrotalcite, T90 467>>198, is slow vulcanization, and the change in distilled water resistance weight is close to NG;

[0074] ② Comparative Example 2 lacks 2-mercaptobenzimidazole, T90 402>>198 tear strength 35.2<44.6, and heat aging elongation change -16.6 is the worst;

[0075] ③ Comparative Example 3 lacks magnesium oxide, T90 has a fast vulcanization speed, T10 has very poor scorch, tensile permanent deformation of 34.8 is poor, and heat aging hardness changes by +7.6NG.

[0076] It can be seen that the rapid vulcanization system composed of magnesium oxide, magnesium aluminum hydrotalcite and 2-mercaptobenzimidazole is indispensable, otherwise the vulcanization speed is slow or the scorch safety is poor.

[0077] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A fast-vulcanizing chloroprene rubber material, characterized in that: Including the following raw materials by weight: 45-55 parts of CR raw rubber, 25-35 parts of reinforcing agent, 1.7-4.5 parts of vulcanizing agent, 0.5-2.5 parts of magnesium oxide, 1.5-3.5 parts of aluminum-magnesium hydrotalcite, 0.1-0.8 parts of activator, 0.2-1.5 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, 0.2-1.5 parts of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 0.5-1.5 parts of 2-mercaptobenzimidazole, 5-24 parts of plasticizer, and 0.2-1.5 parts of accelerator.

2. The fast-vulcanizing chloroprene rubber material according to claim 1, characterized in that: The vulcanizing agent is composed of indirect zinc oxide and ethylene thiourea; preferably, the mass ratio of the indirect zinc oxide to ethylene thiourea is (1.5-3.5): (0.2-1.0).

3. The fast-vulcanizing chloroprene rubber material according to claim 1, characterized in that: The plasticizer is dioctyl sebacate, ethylene glycol adipate or a combination thereof; preferably, the plasticizer is composed of dioctyl sebacate and ethylene glycol adipate in a mass ratio of (2-9):(3-15).

4. The fast-vulcanizing chloroprene rubber material according to claim 1, characterized in that: The reinforcing agent is quick-pressed furnace black, natural gas semi-reinforcing carbon black or a combination thereof.

5. The fast-vulcanizing chloroprene rubber material according to claim 1, characterized in that: The active agent is stearic acid.

6. The fast-vulcanizing chloroprene rubber material according to claim 1, characterized in that: The accelerator is tetramethylthiuram disulfide, dibenzothiazole disulfide or a combination thereof.

7. The fast-vulcanizing chloroprene rubber material according to claim 1, characterized in that: The CR raw rubber is xanthate-adjusted chloroprene rubber, and the Mooney viscosity is 60-80 under the test conditions of ISO289 UML (1+4) 100°C.

8. A method for preparing a fast-vulcanizing chloroprene rubber material as claimed in any one of claims 1 to 7, characterized in that: The steps include: S1, weighing raw materials by mass, adding them into an internal mixer for mixing, and then discharging the materials to obtain a mixed rubber; S2, refining the mixed rubber, and then vulcanizing and molding to obtain.

9. The method for preparing the fast-vulcanizing chloroprene rubber material according to claim 8, characterized in that: In S1, the mixing time is 5-10 minutes, and the discharge temperature is 90-122°C.

10. The method for preparing the fast-vulcanizing chloroprene rubber material according to claim 8, characterized in that: In S2, the temperature of the open mill is 40-80°C; the temperature of the vulcanization molding is 165-185°C, the time is 150-420s, and the pressure is 140-180Kgf / cm 2 .

Citation Information

Cited By

  • Chloroprene rubber material and preparation method thereof

    CN119899437A

  • A neoprene material and a method for producing the same

    CN119899437B