Waterproof antibacterial plastic functional master batch and preparation method thereof
Through the preparation of composite antibacterial agents and ultrasonic dispersion technology, the problem of insufficient antibacterial sustainability of existing plastic products has been solved, effective inhibition of bacteria and molds and long-term antibacterial effects have been achieved, and the water resistance of plastic products has been improved.
Patent Information
- Application Number
- CN202410846302.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
AI Technical Summary
The organic antibacterial agents added to the masterbatch of existing plastic products have poor toxicological safety and poor chemical stability, resulting in insufficient antibacterial sustainability and inability to effectively inhibit the reproduction of microorganisms.
Using composite antibacterial agents, a multi-layer composite antibacterial agent is prepared by combining carbon nanotubes with materials such as silver nitrate and polyvinylpyrrolidone. It combines ultrasonic dispersion and centrifugal processing technology to increase the stability and efficiency of the antibacterial agent, and performs under ultraviolet light Catalyze ROS to destroy microbial cells.
Significantly improves the antibacterial performance, can effectively inhibit the reproduction of bacteria and mold, maintain long-term antibacterial effects, and further inhibit microorganisms through ion and protein complex reactions, significantly improving the water-resistant antibacterial performance of plastic products.
Smart Images

Figure CN118812940A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic functional masterbatch, in particular to a water-resistant and antibacterial plastic functional masterbatch and a preparation method thereof. Background Art
[0002] With the continuous development of current social economy, plastic materials are widely used in various fields such as agriculture, industry, construction, packaging, cutting-edge defense industry and people's daily life.
[0003] Since the environment is full of bacteria, fungi, viruses and other pathogenic microorganisms, a large number of which will become one of the killers of human health, people pay more and more attention to this, and people are beginning to pay more attention to environmental hygiene, and plastic products with antibacterial functions are becoming more and more popular.
[0004] Currently, the antimicrobial agents added are generally organic antimicrobial agents and inorganic antimicrobial agents. Existing plastic products add organic antimicrobial agents to masterbatches to improve the antimicrobial properties of plastic products. However, organic antimicrobial agents have poor toxicological safety and, during the processing of plastic products, due to high temperatures, they lead to poor chemical stability, which in turn affects the antimicrobial properties of microorganisms and the antimicrobial sustainability is also insufficient.
[0005] Based on this, a water-resistant and antibacterial plastic functional masterbatch and a preparation method are provided to solve the existing technical problems. Summary of the invention
[0006] The purpose of the present invention is to provide a water-resistant and antibacterial plastic functional masterbatch and a preparation method thereof, so as to solve the deficiencies in the prior art.
[0007] The technical solution adopted by the present invention is as follows:
[0008] A water-resistant and antibacterial plastic functional masterbatch, comprising a base resin, an additive, and an antibacterial agent;
[0009] Wherein, the mass ratio of base resin and additive is: 75:10-20;
[0010] The additives include: antioxidants, coupling agents, lubricants, and inorganic fillers;
[0011] Wherein, the mixed mass ratio of antioxidant, coupling agent, lubricant and inorganic filler is: 2-3:2-5:1-1.5:20-30;
[0012] The antibacterial agent used is a composite antibacterial agent;
[0013] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 1-8wt%.
[0014] As a further technical solution, the matrix resin is a mixture of any one or more of polyethylene, polyvinyl chloride, polypropylene, polystyrene, polyurethane, phenolic resin, and urea-formaldehyde resin.
[0015] As a further technical solution, the preparation method of the composite antibacterial agent is:
[0016] First, the carbon nanotubes are added to the acid treatment solution and immersed for 40 minutes, then filtered, washed with water until neutral, and dried to obtain treated carbon nanotubes;
[0017] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0018] Among them, the stirring speed is 300r / min;
[0019] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0020] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0021] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0022] As a further technical solution, the acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0023] Among them, the mass fraction of sulfuric acid is 5-8%, and the mass fraction of nitric acid is 1-2%;
[0024] The carbon nanotubes and the acid treatment solution are mixed in a ratio of 10-15 g: 150 mL;
[0025] The immersion temperature of the immersion treatment is 80°C.
[0026] As a further technical solution, the concentration of the silver nitrate solution is 0.3-0.5 mol / L;
[0027] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200mL:3-4g;
[0028] The mixing ratio of the treated carbon nanotubes and the composite liquid is 12-18 g:150 mL.
[0029] As a further technical solution, the mixing ratio of the dispersion and the sodium hydroxide solution is 4:1;
[0030] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0031] As a further technical solution, the antioxidant is antioxidant 1010 or antioxidant DLTP;
[0032] The coupling agent is an organosilicon coupling agent;
[0033] The lubricant is polyethylene wax;
[0034] The inorganic filler is calcium carbonate.
[0035] A method for preparing a water-resistant and antibacterial plastic functional masterbatch comprises the following steps:
[0036] S1. Add each component into a high-speed mixer in order according to the proportion of each component, stir for 10 minutes, and obtain a mixture;
[0037] S2. The uniformly mixed materials are sent to the feeding barrel of a twin-screw extruder, and after melt extrusion, water cooling and pelletizing, water-resistant and antibacterial plastic functional masterbatch is obtained.
[0038] As a further technique: the stirring speed in the high-speed mixer described in step S1 is 5000 r / min.
[0039] Beneficial effects:
[0040] The plastic functional masterbatch prepared by the present invention has excellent antibacterial properties. The present invention has a greatly improved antibacterial effect compared with conventional antibacterial agents by introducing the prepared composite antibacterial agent, and has a good antibacterial effect not only on bacteria, but also on fungi such as molds, and overall shows an excellent effect of inhibiting the reproduction of microorganisms. Since the matrix resin of the present invention is polyethylene, polyvinyl chloride, polypropylene, polystyrene, polyurethane, phenolic resin, urea-formaldehyde resin, etc., the plastic products made thereof have excellent water resistance and can withstand long-term underwater use.
[0041] The present invention prepares a composite antibacterial agent by adopting a specific method. Under the irradiation of ultraviolet light, water or oxygen will be catalyzed to generate ROS. The ROS can destroy the dynamic balance of oxidants and antioxidants in microbial cells, thereby inducing oxidative stress in the microbial cells, and then promoting oxidative damage in the microbial cell tissues, which can achieve the purpose of causing the microbial cells to lose activity in a relatively short period of time and achieving the purpose of antibacterial.
[0042] More importantly, in the process of generating ROS, the active ingredients of the composite antibacterial agent of the present invention only act as catalysts for the ROS generation reaction, rather than reaction raw materials. That is to say, the reaction itself does not consume the active ingredients in the composite antibacterial agent and can be carried out repeatedly, thereby enabling it to continuously maintain efficient antibacterial properties.
[0043] In terms of direct sterilization effect, the ions produced by the composite antimicrobial agent can inhibit the synthesis of microbial peptidoglycan, cause the rupture of microbial cell walls, and then destroy the cell structure of the microorganism, thereby achieving the purpose of antibacterial. When the active ingredients of the composite antimicrobial agent enter the microbial cells, they will also react with the proteins in the cells to destroy the spatial structure of the proteins. They mainly act on the enzymes in the microbial cells, thereby inhibiting the entire physiological reaction process in the microbial cells, making it impossible to continue to divide and reproduce, inhibiting respiration, and achieving the purpose of antibacterial. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a bar chart of the antibacterial durability test of the embodiments and comparative examples. DETAILED DESCRIPTION
[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] A water-resistant and antibacterial plastic functional masterbatch, comprising a base resin, an additive, and an antibacterial agent;
[0047] Wherein, the mass ratio of base resin and additive is: 75:10-20;
[0048] The additives include: antioxidants, coupling agents, lubricants, and inorganic fillers;
[0049] Wherein, the mixed mass ratio of antioxidant, coupling agent, lubricant and inorganic filler is: 2-3:2-5:1-1.5:20-30;
[0050] The antibacterial agent used is a composite antibacterial agent;
[0051] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 1-8wt%.
[0052] The matrix resin is any one or more mixtures of polyethylene, polyvinyl chloride, polypropylene, polystyrene, polyurethane, phenolic resin and urea-formaldehyde resin.
[0053] The preparation method of the composite antibacterial agent is as follows:
[0054] First, the carbon nanotubes are added to the acid treatment solution and immersed for 40 minutes, then filtered, washed with water until neutral, and dried to obtain treated carbon nanotubes;
[0055] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0056] Among them, the stirring speed is 300r / min;
[0057] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0058] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0059] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0060] The acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0061] Among them, the mass fraction of sulfuric acid is 5-8%, and the mass fraction of nitric acid is 1-2%;
[0062] The carbon nanotubes and the acid treatment solution are mixed in a ratio of 10-15 g: 150 mL;
[0063] The immersion temperature of the immersion treatment is 80°C.
[0064] The concentration of silver nitrate solution is 0.3-0.5 mol / L;
[0065] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200mL:3-4g;
[0066] The mixing ratio of the treated carbon nanotubes and the composite liquid is 12-18 g:150 mL.
[0067] The mixing ratio of dispersion liquid and sodium hydroxide solution is 4:1;
[0068] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0069] The antioxidant is antioxidant 1010 or antioxidant DLTP;
[0070] The coupling agent is an organosilicon coupling agent;
[0071] The lubricant is polyethylene wax;
[0072] Polyethylene wax (PE wax), also known as polymer wax or polyethylene wax for short, is widely used due to its excellent cold resistance, heat resistance, chemical resistance and wear resistance. It can increase the gloss and processing performance of products. As a lubricant, it has stable chemical properties and good electrical properties. Polyethylene wax has good compatibility with polyethylene and can improve the fluidity of polyethylene.
[0073] The inorganic filler is calcium carbonate.
[0074] A method for preparing a water-resistant and antibacterial plastic functional masterbatch comprises the following steps:
[0075] S1. Add each component into a high-speed mixer in order according to the proportion of each component, stir for 10 minutes to obtain a mixture; the stirring speed in the high-speed mixer is 5000r / min.
[0076] S2. The uniformly mixed materials are sent to the feeding barrel of a twin-screw extruder, and after melt extrusion, water cooling and pelletizing, water-resistant and antibacterial plastic functional masterbatch is obtained.
[0077] The following are specific embodiments:
[0078] Example 1
[0079] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene, additives, and a composite antibacterial agent;
[0080] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0081] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0082] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0083] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 1wt%.
[0084] The preparation method of the composite antibacterial agent is as follows:
[0085] First, the carbon nanotubes are added to an acid treatment solution and immersed for 40 minutes, then filtered, washed with clean water until neutral, and dried to obtain treated carbon nanotubes; the acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0086] Among them, the mass fraction of sulfuric acid is 5%, and the mass fraction of nitric acid is 1.6%;
[0087] The mixing ratio of the carbon nanotubes and the acid treatment solution is 12 g: 150 mL;
[0088] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0089] Wherein, the stirring speed is 300r / min; the concentration of the silver nitrate solution is 0.4mol / L;
[0090] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200 mL: 3.5 g;
[0091] The mixing ratio of the treated carbon nanotubes and the composite liquid is 15 g:150 mL.
[0092] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0093] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0094] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0095] The immersion temperature of the immersion treatment is 80°C.
[0096] The mixing ratio of dispersion liquid and sodium hydroxide solution is 4:1;
[0097] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0098] Example 2
[0099] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene, additives, and a composite antibacterial agent;
[0100] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0101] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0102] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0103] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 2wt%.
[0104] The preparation method of the composite antibacterial agent is as follows:
[0105] First, the carbon nanotubes are added to an acid treatment solution and immersed for 40 minutes, then filtered, washed with clean water until neutral, and dried to obtain treated carbon nanotubes; the acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0106] Among them, the mass fraction of sulfuric acid is 5%, and the mass fraction of nitric acid is 1.6%;
[0107] The mixing ratio of the carbon nanotubes and the acid treatment solution is 12 g: 150 mL;
[0108] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0109] Wherein, the stirring speed is 300r / min; the concentration of the silver nitrate solution is 0.4mol / L;
[0110] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200 mL: 3.5 g;
[0111] The mixing ratio of the treated carbon nanotubes and the composite liquid is 15 g:150 mL.
[0112] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0113] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0114] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0115] The immersion temperature of the immersion treatment is 80°C.
[0116] The mixing ratio of dispersion liquid and sodium hydroxide solution is 4:1;
[0117] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0118] Example 3
[0119] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene, additives, and a composite antibacterial agent;
[0120] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0121] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0122] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0123] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 4wt%.
[0124] The preparation method of the composite antibacterial agent is as follows:
[0125] First, the carbon nanotubes are added to an acid treatment solution and immersed for 40 minutes, then filtered, washed with clean water until neutral, and dried to obtain treated carbon nanotubes; the acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0126] Among them, the mass fraction of sulfuric acid is 5%, and the mass fraction of nitric acid is 1.6%;
[0127] The mixing ratio of the carbon nanotubes and the acid treatment solution is 12 g: 150 mL;
[0128] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0129] Wherein, the stirring speed is 300r / min; the concentration of the silver nitrate solution is 0.4mol / L;
[0130] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200 mL: 3.5 g;
[0131] The mixing ratio of the treated carbon nanotubes and the composite liquid is 15 g:150 mL.
[0132] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0133] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0134] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0135] The immersion temperature of the immersion treatment is 80°C.
[0136] The mixing ratio of dispersion liquid and sodium hydroxide solution is 4:1;
[0137] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0138] Example 4
[0139] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene, additives, and a composite antibacterial agent;
[0140] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0141] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0142] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0143] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 6wt%.
[0144] The preparation method of the composite antibacterial agent is as follows:
[0145] First, the carbon nanotubes are added to an acid treatment solution and immersed for 40 minutes, then filtered, washed with clean water until neutral, and dried to obtain treated carbon nanotubes; the acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0146] Among them, the mass fraction of sulfuric acid is 5%, and the mass fraction of nitric acid is 1.6%;
[0147] The mixing ratio of the carbon nanotubes and the acid treatment solution is 12 g: 150 mL;
[0148] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0149] Wherein, the stirring speed is 300r / min; the concentration of the silver nitrate solution is 0.4mol / L;
[0150] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200 mL: 3.5 g;
[0151] The mixing ratio of the treated carbon nanotubes and the composite liquid is 15 g:150 mL.
[0152] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0153] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0154] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0155] The immersion temperature of the immersion treatment is 80°C.
[0156] The mixing ratio of dispersion liquid and sodium hydroxide solution is 4:1;
[0157] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0158] Example 5
[0159] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene, additives, and a composite antibacterial agent;
[0160] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0161] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0162] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0163] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 8wt%.
[0164] The preparation method of the composite antibacterial agent is as follows:
[0165] First, the carbon nanotubes are added to an acid treatment solution and immersed for 40 minutes, then filtered, washed with clean water until neutral, and dried to obtain treated carbon nanotubes; the acid treatment solution is a mixed solution of sulfuric acid and nitric acid;
[0166] Among them, the mass fraction of sulfuric acid is 5%, and the mass fraction of nitric acid is 1.6%;
[0167] The mixing ratio of the carbon nanotubes and the acid treatment solution is 12 g: 150 mL;
[0168] Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution;
[0169] Wherein, the stirring speed is 300r / min; the concentration of the silver nitrate solution is 0.4mol / L;
[0170] The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200 mL: 3.5 g;
[0171] The mixing ratio of the treated carbon nanotubes and the composite liquid is 15 g:150 mL.
[0172] Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion;
[0173] Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent;
[0174] The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
[0175] The immersion temperature of the immersion treatment is 80°C.
[0176] The mixing ratio of dispersion liquid and sodium hydroxide solution is 4:1;
[0177] The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
[0178] Comparative Example 1:
[0179] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene and additives;
[0180] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0181] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0182] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0183] Comparative Example 2:
[0184] A water-resistant and antibacterial plastic functional masterbatch, comprising polyethylene, additives, and an antibacterial agent;
[0185] Among them, the mixing mass ratio of polyethylene and additives is: 75:15;
[0186] The additives include: antioxidant 1010, silicone coupling agent, polyethylene wax, and calcium carbonate;
[0187] Among them, the mixed mass ratio of antioxidant 1010, silicone coupling agent, polyethylene wax and calcium carbonate is: 2:5:1:25;
[0188] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the antibacterial agent is 1wt%.
[0189] The antimicrobial agent is silver oxide;
[0190] Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the antibacterial agent is 1wt%.
[0191] test:
[0192] The antibacterial performance is tested according to GB / T31402-2015, the test bacteria are Staphylococcus aureus and Escherichia coli, and the antibacterial performance value is calculated according to the following formula.
[0193] R=(U2-U1)-(A2-U1)=U2-A2;
[0194] Where: R is the antibacterial performance value;
[0195] U1 is the logarithmic mean of the number of bacteria immediately after inoculation of the sample without antibacterial treatment, CFU / cm 2 ;
[0196] U2 is the logarithmic mean of the number of bacteria in the sample without antibacterial treatment 24 hours after inoculation, CFU / cm 2 ;
[0197] A2 is the logarithmic mean of the number of bacteria in the antibacterial treated sample 24 hours after inoculation, CFU / cm 2 .
[0198] The test samples were processed into 20cm×10cm×0.2mm films from Example and Comparative Example 2. The specific results are shown in Table 1:
[0199] Table 1
[0200]
[0201]
[0202] It can be seen from Table 1 that the antibacterial performance value of the functional masterbatch prepared in the example is relatively high, indicating that it has excellent antibacterial effect on Escherichia coli and Staphylococcus aureus.
[0203] Antibacterial durability test:
[0204] According to JC / T939-2004 test, the samples of the embodiment and the comparative example were immersed in a distilled water bath at a temperature of 60°C for 20 hours, and the percentage reduction of the antibacterial performance of the samples of the embodiment and the comparative example after immersion was detected:
[0205] Table 2
[0206]
[0207] It can be seen from Table 2 that the plastic functional masterbatch prepared by the present invention has good antibacterial durability.
[0208] Anti-mildew performance test:
[0209] The films (20 cm × 10 cm × 0.2 mm) of the same specifications prepared in the embodiment and the comparative example were tested according to GB / T24128-2018, and the test strain was Aspergillus niger; the evaluation of the fungal growth is shown in Table 3;
[0210] Table 3
[0211] Fungal growth Example 1 No growth Example 2 No growth Example 3 No growth Example 4 No growth Comparative Example 1 Obvious growth and spore production Comparative Example 2 Initial growth
[0212] It can be seen from Table 3 that the plastic functional masterbatch prepared by the present invention has a relatively good inhibitory effect on mold.
[0213] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.
Claims
1. A water-resistant and antibacterial plastic functional masterbatch, characterized in that: Including base resin, additives, antimicrobial agents; Wherein, the mass ratio of base resin and additive is: 75:10-20; The additives include: antioxidants, coupling agents, lubricants, and inorganic fillers; Wherein, the mixed mass ratio of antioxidant, coupling agent, lubricant and inorganic filler is: 2-3:2-5:1-1.5:20-30; The antibacterial agent used is a composite antibacterial agent; Based on the total weight of the water-resistant and antibacterial plastic functional masterbatch, the content of the composite antibacterial agent is 1-8wt%.
2. The water-resistant and antibacterial plastic functional masterbatch according to claim 1, characterized in that: The matrix resin is any one or more of polyethylene, polyvinyl chloride, polypropylene, polystyrene, polyurethane, phenolic resin and urea-formaldehyde resin.
3. The water-resistant and antibacterial plastic functional masterbatch according to claim 1, characterized in that: The preparation method of the composite antibacterial agent is as follows: First, the carbon nanotubes are added to the acid treatment solution and immersed for 40 minutes, then filtered, washed with water until neutral, and dried to obtain treated carbon nanotubes; Prepare a silver nitrate solution, then add polyvinyl pyrrolidone into the silver nitrate solution, stir and mix evenly to obtain a composite solution; Among them, the stirring speed is 300r / min; Adding the treated carbon nanotubes obtained above to the composite liquid, and performing ultrasonic dispersion to obtain a dispersion; Adding sodium hydroxide solution to the dispersion, stirring and reacting under light-proof conditions, the stirring speed is 200 r / min, standing for 4 hours, and then high-speed centrifugation, standing for 1 hour, filtering, washing with anhydrous ethanol and deionized water respectively, and then drying to obtain a multi-layer composite antibacterial agent; The cleaning time using anhydrous ethanol is 10 minutes, and the cleaning time using deionized water is 5 minutes.
4. The water-resistant and antibacterial plastic functional masterbatch according to claim 3, characterized in that: The acid treatment solution is a mixed solution of sulfuric acid and nitric acid; Among them, the mass fraction of sulfuric acid is 5-8%, and the mass fraction of nitric acid is 1-2%; The carbon nanotubes and the acid treatment solution are mixed in a ratio of 10-15 g: 150 mL; The immersion temperature of the immersion treatment is 80°C.
5. The water-resistant and antibacterial plastic functional masterbatch according to claim 3, characterized in that: The concentration of silver nitrate solution is 0.3-0.5 mol / L; The mixing ratio of the silver nitrate solution and polyvinyl pyrrolidone is 200mL:3-4g; The mixing ratio of the treated carbon nanotubes and the composite liquid is 12-18 g:150 mL.
6. The water-resistant and antibacterial plastic functional masterbatch according to claim 1, characterized in that: The mixing ratio of the dispersion and the sodium hydroxide solution is 4:1; The high-speed centrifugal treatment was carried out at a rotation speed of 8000 r / min and a time of 30 min.
7. The water-resistant and antibacterial plastic functional masterbatch according to claim 1, characterized in that: The antioxidant is antioxidant 1010 or antioxidant DLTP; The coupling agent is an organosilicon coupling agent; The lubricant is polyethylene wax; The inorganic filler is calcium carbonate.
8. The method for preparing a water-resistant and antibacterial plastic functional masterbatch according to claim 1, characterized in that: The following steps are involved: S1. Add each component into a high-speed mixer in order according to the proportion of each component, stir for 10 minutes, and obtain a mixture; S2. The uniformly mixed materials are sent to the feeding barrel of a twin-screw extruder, and after melt extrusion, water cooling and pelletizing, water-resistant and antibacterial plastic functional masterbatch is obtained.
9. The method for preparing a water-resistant and antibacterial plastic functional masterbatch according to claim 8, characterized in that: The stirring speed in the high-speed mixer in step S1 is 5000 r / min.