High-insulativity polyolefin composition as well as preparation method and application thereof
Through the combined use of polyethylene grafted silicone rubber and coated silane coupling agent mica powder, the problem of reduced oil resistance and insulation performance of low-smoke halogen-free polyolefin materials in the existing technology has been solved, and the polyolefin composition has been realized in complex applications. Excellent performance under working conditions, suitable for cable materials.
Patent Information
- Application Number
- CN202411030329.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The oil resistance and insulation properties of existing low-smoke halogen-free polyolefin materials are reduced after adding flame retardants, making it difficult to meet the requirements for flame retardancy, insulation, oil resistance and mechanical properties under complex working conditions at the same time.
By chemically cross-linking polyethylene grafted silicone rubber with polyethylene materials, and using mica powder coated with silane coupling agent, the compatibility and mechanical properties of the material are improved, the oil resistance and insulation properties of silicone rubber are increased, and the PE and EVA are base resins, and hydroxide and montmorillonite are selected as flame retardants.
The polyolefin composition has excellent oil resistance, insulation, flame retardancy and mechanical properties at high temperatures, meets the flame retardant requirements of the national standard, and is suitable for cable materials.
Smart Images

Figure BDA0004969756090000021 
Figure BDA0004969756090000091 
Figure BDA0004969756090000101
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of polymer materials, and specifically relates to a high-insulation polyolefin composition and a preparation method and application thereof. Background Art
[0002] Low smoke halogen-free polyolefin cross-linked insulation materials are usually made of a series of polyolefin resins such as PE / EVA / POE, and in order to meet the characteristics of low smoke and halogen-free, a large amount of hydroxide flame retardant filling is often required to meet the flame retardant requirements. For special cables under complex working conditions, their working environment is often faced with various oil liquids such as fuel oil and mineral oil, and ordinary polyolefin materials themselves have poor oil resistance. After adding a large amount of hydroxide, their density is destroyed, resulting in worse oil resistance.
[0003] At present, the oil resistance of cable materials is mainly improved by introducing strong polar resins, such as nitrile rubber, bisphenol A resin, polyphenylene sulfide, EVA with high VA content, etc. However, the introduction of strong polar resins will lead to a significant reduction in the overall insulation performance of the material and cannot meet the resistance performance requirements of the insulation material. In addition, the oil resistance of cable materials can also be improved by adding methyl vinyl silicone rubber, but the improvement of oil resistance is limited.
[0004] Therefore, it is necessary to develop a polyolefin composition that has excellent oil resistance, insulation, flame retardancy, as well as mechanical properties such as tensile strength and elongation at break. Summary of the invention
[0005] Based on the defects of the prior art, the purpose of this application is to provide a high-insulation polyolefin composition and its preparation method and application, and the obtained polyolefin composition has excellent oil resistance, insulation, flame retardancy, as well as mechanical properties such as tensile strength and elongation at break.
[0006] In order to achieve the above object, the present application provides a polyolefin composition, comprising the following components in parts by weight:
[0007] Polyethylene 19-36 parts;
[0008]
[0009] Silicone rubber has good oil resistance and excellent insulation, but its compatibility with polyolefin materials is poor. Directly adding silicone rubber to polyolefin materials or using conventional methods to improve compatibility (such as adding coupling agents) cannot achieve good compatibility, resulting in the failure to give full play to the advantages of silicone rubber in oil resistance and insulation, and also resulting in poor mechanical properties and flame retardant properties of the material. The inventor unexpectedly discovered that grafting polyethylene to silicone rubber, so that silicone rubber and polyethylene are tightly combined by chemical crosslinking, can significantly improve the compatibility of silicone rubber with polyolefin materials, effectively give full play to the advantages of silicone rubber in oil resistance and insulation, and reduce the impact of silicone rubber addition on the mechanical properties and flame retardant properties of the material.
[0010] Mica powder is mainly silicate, which has a similar electrical potential to silicone rubber, so mica powder can be well dispersed in silicone rubber. Compared with other layered silicates, the layered structure of mica powder is larger and has a better barrier effect. Using silane coupling agent to coat mica powder can improve the compatibility of mica powder with polyolefin systems, so that it can not only block solvents and improve the oil resistance of the material, but also enhance the compatibility of the overall material system, further improving mechanical, oil resistance and other properties.
[0011] The polyolefin composition uses PE and EVA as base resins, selects hydroxide and montmorillonite as flame retardants, and adds PE-g-SiR, mica powder coated with a silane coupling agent, radiation initiator, etc., and has excellent high-temperature oil resistance, insulation performance, and mechanical properties such as tensile strength and elongation at break, and can also meet the flame retardancy requirements of the national standard GB / T 32129-2015, and is suitable for use as a cable material.
[0012] Preferably, the mass percentage of silicone rubber in the polyethylene grafted silicone rubber is 28%-72%, such as 28%, 30%, 40%, 50%, 60%, 70% or 72%, etc., which can not only utilize silicone rubber to better improve high temperature oil resistance, but also make silicone rubber easier to disperse in the polyolefin system, avoid self-crosslinking of silicone rubber, and better improve the compatibility of silicone rubber with the polyolefin system.
[0013] More preferably, the mass percentage of silicone rubber in the polyethylene grafted silicone rubber is 38%-62%, such as 38%, 40%, 45%, 50%, 55%, 60% or 62%, so as to better improve the balance between the mechanical properties and high temperature oil resistance of the material.
[0014] Optionally, the preparation method of the polyethylene grafted silicone rubber comprises the following steps: mixing and dispersing polyethylene and silicone rubber, performing a first open milling, adding an initiator, performing a second open milling, and then extruding and granulating to obtain the polyethylene grafted silicone rubber. Exemplarily, the silicone rubber has at least one of methyl, vinyl, and phenyl.
[0015] Preferably, when preparing the polyethylene grafted silicone rubber, the mass of the silicone rubber used is 28%-72% of the total mass of the polyethylene and silicone rubber used, such as 28%, 30%, 40%, 50%, 60%, 70% or 72%.
[0016] Preferably, when preparing the polyethylene grafted silicone rubber, the mass of the initiator used is 0.05% to 1% of the total mass of the polyethylene and silicone rubber used.
[0017] Preferably, the temperature of the first grinding is 100-120° C., and the grinding time is 5-10 min.
[0018] Preferably, the temperature of the second refining is 110-130° C., and the refining time is 10-15 min.
[0019] Preferably, when preparing the polyethylene grafted silicone rubber, the extrusion temperature is 160-180°C.
[0020] Preferably, when preparing the polyethylene grafted silicone rubber, granulation is carried out underwater.
[0021] Preferably, when preparing the polyethylene grafted silicone rubber, the initiator used is an organic peroxide. As an example, the organic peroxide includes at least one of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisopropylbenzene peroxide, and di-tert-butyl diisopropylbenzene peroxide.
[0022] Preferably, when preparing the polyethylene grafted silicone rubber, the polyethylene used includes metallocene linear low-density polyethylene.
[0023] Preferably, the mass percentage of the silane coupling agent in the mica powder coated with the silane coupling agent is 0.3%-4%, such as 0.3%, 0.5%, 1%, 2%, 3% or 4%, etc., so as to avoid self-crosslinking of the silane coupling agent, and to utilize the silane coupling agent to better improve the compatibility of the mica powder with the polyolefin system and improve the mechanical properties of the material.
[0024] More preferably, the mass percentage of the silane coupling agent in the mica powder coated with the silane coupling agent is 0.8%-2.2%, such as 0.8%, 1%, 1.5%, 2% or 2.2%, etc., to further improve the mechanical properties of the material.
[0025] The mass percentage of the silane coupling agent in the mica powder coated with the silane coupling agent=(W1-W0 / W0)*100%, wherein W1 represents the weight of the mica powder coated with the silane coupling agent, and W0 represents the weight of the mica powder before coating.
[0026] The silane coupling agent may be either an epoxy group-containing silane coupling agent or an epoxy group-free silane coupling agent. For example, in one embodiment, the silane coupling agent includes at least one of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane and 3-acryloxypropyltrimethoxysilane.
[0027] Preferably, the silane coupling agent contains epoxy groups. The epoxy groups in the epoxy silane coupling agent have strong polarity, which forms a strong interaction between it and EVA, thereby improving the dispersibility and making the mechanical properties and insulation properties of the material such as tensile strength and elongation at break better.
[0028] As an example, the epoxy group-containing silane coupling agent includes at least one of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and 3-(2,3-epoxypropoxy)propyltriethoxysilane.
[0029] Optionally, the method for preparing the mica powder coated with a silane coupling agent comprises the following steps: soaking the mica powder in a solution containing a silane coupling agent, heating and stirring to perform a coating and grafting reaction, then separating the solid from the liquid, and drying the obtained solid to obtain the mica powder with the surface coated with a silane coupling agent.
[0030] Preferably, the mass fraction of the silane coupling agent in the solution containing the silane coupling agent is 0.8wt%-3wt%.
[0031] Preferably, the mass ratio of the mica powder to the solution containing the silane coupling agent is 1:(0.5-5).
[0032] Preferably, the soaking time is 5-10 minutes.
[0033] Preferably, the heating and stirring temperature is 70-90° C., and the heating and stirring time is 0.5-2 h.
[0034] As an example, the solvent in the solution containing the silane coupling agent includes at least one of ethanol, acetone, and methanol.
[0035] Preferably, the polyethylene has a melt flow rate of 0.5-4 g / 10 min at 190° C. and 2.16 kg load, such as 0.5 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 2 g / 10 min, 2.5 g / 10 min, 3 g / 10 min or 4 g / 10 min, etc. The melt flow rate is measured in accordance with GB / T3682.1-2018.
[0036] Preferably, the mass percentage of the polyethylene in the polyolefin composition is above 13%, such as 13%, 15%, 20% or 25%.
[0037] Preferably, the polyethylene is metallocene linear low density polyethylene.
[0038] Preferably, the mass percentage of vinyl acetate in the ethylene-vinyl acetate copolymer is 25%-35%, such as 25%, 27%, 30%, 33% or 35%.
[0039] Preferably, the hydroxide includes at least one of aluminum hydroxide and magnesium hydroxide;
[0040] Preferably, the radiation initiator includes at least one of TAIC (triallyl isocyanurate), TMPTMA (trimethylolpropane trimethacrylate), and TMPTA (trimethylol propane triacrylate);
[0041] Preferably, the polyolefin composition further comprises 2-5 parts by weight of an antioxidant, wherein the antioxidant comprises at least one of a hindered phenol antioxidant, a phosphite antioxidant, and a thioether antioxidant.
[0042] The polyolefin composition described in the present application may contain common additives such as color powder, lubricant, anti-UV agent, etc. without impairing the effects of the present application.
[0043] Optionally, the method for preparing the polyolefin composition comprises the following steps: mixing and dispersing raw materials except hydroxide, montmorillonite and mica powder coated with a silane coupling agent to obtain a premix;
[0044] The premix, hydroxide, montmorillonite and mica powder coated with silane coupling agent are mixed and kneaded in proportion, and then extruded and granulated to obtain a polyolefin composition.
[0045] Preferably, the banburying temperature is 130-140°C; the extrusion temperature is 140-160°C.
[0046] Optionally, during the preparation of the premix, the mixing and dispersing speed is 1000-2000 rpm.
[0047] Optionally, the extrusion granulation is carried out in a two-stage single-screw extruder.
[0048] The present application also provides application of the polyolefin composition in cable materials.
[0049] Compared with the prior art, the beneficial effects of this application are:
[0050] (1) The present application improves the oil resistance and insulation of the polyethylene and ethylene-vinyl acetate copolymer system by adding polyethylene grafted silicone rubber; and improves the oil resistance and mechanical properties of the system by adding mica powder coated with a silane coupling agent.
[0051] (2) The polyolefin composition of the present application has excellent high temperature oil resistance and insulation performance, as well as excellent tensile strength and elongation at break, and can meet the flame retardant requirements of the national standard GB / T 32129-2015, and is suitable for use as a cable material. DETAILED DESCRIPTION
[0052] In order to better illustrate the purpose, technical scheme and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of this application are all commonly used ordinary reagents and instruments unless otherwise specified. In the present application, the technical features described in an open manner include closed technical schemes composed of the listed features, and also include open technical schemes containing the listed features.
[0053] Examples and Comparative Examples
[0054] Each embodiment and comparative example provides a polyolefin composition. The compositions of these polyolefin compositions are shown in Tables 1 to 2, and the preparation method comprises the following steps:
[0055] Putting metallocene linear low-density polyethylene, ethylene-vinyl acetate copolymer, polyethylene grafted silicone rubber (or silicone rubber, if any), radiation initiator and antioxidant into a high-speed mixer in proportion and mixing and dispersing at a speed of 1500 rpm to obtain a premix;
[0056] The obtained premix, hydroxide, montmorillonite and mica powder coated with silane coupling agent (or mica powder, if any) are put into an internal mixer in proportion, and after internal mixing in the internal mixer, extrusion granulation is carried out through a double-stage single screw extruder to obtain a polyolefin composition, wherein the temperature of the internal mixer is controlled at 135° C., and the temperature of the single screw extruder is controlled at 140-160° C. Unless otherwise specified, the steps and process parameters used in the preparation methods of the embodiments and comparative examples are the same.
[0057] The raw material information used in the above embodiments and comparative examples is as follows:
[0058] MLLDPE 1: melt flow rate 3.5 g / 10 min, LLDPE Exceed 3518PA, ExxonMobil;
[0059] MLLDPE 2: melt flow rate 2 g / 10 min, LLDPE Exceed 2012MA, ExxonMobil;
[0060] MLLDPE 3: melt flow rate is 1g / 10min, LLDPE ENABLE 2010PA, ExxonMobil;
[0061] EVA: The mass percentage of vinyl acetate is 27%, EVAUL00328, ExxonMobil;
[0062] Silicone rubber: methyl vinyl silicone rubber, CHN3500U, Shin-Etsu, Japan;
[0063] PE-g-SiR 1: The silicone rubber has a mass percentage of 40% and is homemade. The specific preparation method comprises the following steps: the above-mentioned MLLDPE 1 and silicone rubber are mixed and dispersed in a weight ratio of 6:4, and the mixture is placed in an open mill and kneaded at a temperature of 110° C. to fully mix the two material melts, and then 0.1wt% of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane by the total weight of MLLDPE 1 and silicone rubber is added, and the kneading is continued at a temperature of 120° C. The kneaded mixture is extruded at a temperature of 170° C. by a twin-screw extruder and pelletized by underwater cutting to obtain PE-g-SiR 1;
[0064] PE-g-SiR 2: silicone rubber content is 50% by weight, homemade, and its preparation method is different from that of PE-g-SiR1 in that the mass ratio of MLLDPE 1 to silicone rubber is 5:5;
[0065] PE-g-SiR 3: The mass percentage of silicone rubber is 60%, which is homemade. The difference between its preparation method and PE-g-SiR1 is that the mass ratio of MLLDPE 1 to silicone rubber is 4:6;
[0066] PE-g-SiR 4: The mass percentage of silicone rubber is 30%, which is homemade. The difference between its preparation method and PE-g-SiR1 is that the mass ratio of MLLDPE 1 to silicone rubber is 7:3;
[0067] PE-g-SiR 5: The mass percentage of silicone rubber is 70%, which is homemade. The difference between its preparation method and PE-g-SiR1 is that the mass ratio of MLLDPE 1 to silicone rubber used is 3:7;
[0068] Mica powder: MICA C-4000, IMERYS;
[0069] Mica powder 1 coated with silane coupling agent: the mass percentage of silane coupling agent is 1.5%, which is homemade. The specific preparation method includes the following steps: dissolving the silane coupling agent in ethanol to obtain a solution with a mass fraction of 2% of the silane coupling agent, soaking the above mica powder in the solution at a solid-liquid ratio of 3g:4g, soaking for 10min, heating and stirring at 80°C for 1h to carry out coating and grafting reaction, then separating the solid and the liquid, and drying the obtained solid. At this time, the powder and the silane coupling agent form a strong chemical bond to obtain mica powder 1 coated with silane coupling agent, wherein the silane coupling agent used is 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, KBM-303, Shin-Etsu, Japan;
[0070] Mica powder 2 coated with silane coupling agent: the mass percentage of silane coupling agent is 1%, and the mica powder is homemade. The preparation method thereof is different from that of mica powder 1 coated with silane coupling agent in that the specific preparation method comprises the following steps: dissolving the silane coupling agent in ethanol to obtain a solution with a mass percentage of 2% of the silane coupling agent, and immersing the mica powder in the solution at a solid-liquid ratio of 1g:1g;
[0071] Mica powder 3 coated with silane coupling agent: the mass percentage of silane coupling agent is 2%, and it is homemade. The preparation method thereof is different from that of mica powder 1 coated with silane coupling agent in that the specific preparation method comprises the following steps: dissolving the silane coupling agent in ethanol to obtain a solution with a mass percentage of 2% of the silane coupling agent, and immersing the mica powder in the solution at a solid-liquid ratio of 1g:2g;
[0072] Mica powder 4 coated with silane coupling agent: The mass percentage of silane coupling agent is 0.5%, and it is homemade. The preparation method thereof is different from that of mica powder 1 coated with silane coupling agent in that the specific preparation method comprises the following steps: dissolving the silane coupling agent in ethanol to obtain a solution with a mass percentage of 2% of the silane coupling agent, and immersing the mica powder in the solution at a solid-liquid ratio of 3g:2g;
[0073] Mica powder 5 coated with silane coupling agent: the mass percentage of silane coupling agent is 3%, and it is homemade. The preparation method thereof is different from that of mica powder 1 coated with silane coupling agent in that the specific preparation method comprises the following steps: dissolving the silane coupling agent in ethanol to obtain a solution with a mass percentage of 2% of the silane coupling agent, and immersing the mica powder in the solution at a solid-liquid ratio of 1g:4g;
[0074] Mica powder coated with silane coupling agent 6: the mass percentage of silane coupling agent is 1%, and it is homemade. The preparation method thereof is different from that of mica powder coated with silane coupling agent 2 in that the silane coupling agent used is 3-(2,3-epoxypropoxy)propyltriethoxysilane, model GX-560, purchased from Anhui Sibao Organic Silicon New Materials Co., Ltd.;
[0075] Mica powder 7 coated with silane coupling agent: the mass percentage of silane coupling agent is 1%, and it is homemade. The preparation method thereof is different from that of mica powder 2 coated with silane coupling agent in that the silane coupling agent used is γ-(2,3-epoxypropoxy)propyltrimethoxysilane, model GX-561, purchased from Anhui Sibao Organic Silicon New Materials Co., Ltd.;
[0076] Mica powder 8 coated with silane coupling agent: the mass percentage of silane coupling agent is 1%, and it is homemade. The preparation method thereof is different from that of mica powder 2 coated with silane coupling agent in that the silane coupling agent used is vinyl silane coupling agent, model SG-SI 172, and the manufacturer is Nanjing Shuguang Chemical;
[0077] Montmorillonite: DK-1, Zhejiang Fenghong;
[0078] Radiation initiator: TAIC, commercially available;
[0079] Antioxidant: a mixture of antioxidant 3114, antioxidant PEP-36 and antioxidant IRGANOX PS 802FD, with a mass ratio of 1:1:1, all of which are commercially available.
[0080] The melt flow rate of each of the above MLLDPEs was measured in accordance with GB / T3682.1-2018, and the test conditions were as follows: 190°C, 2.16 kg load;
[0081] The mass percentage of the silane coupling agent in the above-mentioned mica powders coated with silane coupling agent is calculated according to the following formula: mass percentage of the silane coupling agent in the mica powder coated with silane coupling agent = (W1-W0 / W0)*100%, wherein W1 represents the weight of the mica powder coated with the silane coupling agent, and W0 represents the weight of the mica powder before coating.
[0082] Unless otherwise specified, the components and raw materials used in the examples and comparative examples of the present application are of the same type.
[0083] The polyolefin compositions obtained in the examples and comparative examples were pressed on a flat vulcanizer at 180°C for 10 min, with a pressure of 15 MPa and a thickness of 1 mm. After being placed at 25°C for 16 h, they were irradiated with a high-energy electron beam with an irradiation dose of 15 Mrad. The irradiated samples were subjected to the following performance tests:
[0084] Tensile strength and elongation at break before oil soaking: refer to standard GB / T 1040.2-2018;
[0085] Oil resistance test: soak the specimens in 903# mineral oil at 100℃ for 72h, and then test the tensile strength and elongation at break of the material after soaking in oil according to the above method.
[0086] Tensile strength retention rate after oil resistance = tensile strength before oil soaking / tensile strength after oil soaking * 100%,
[0087] Retention rate of elongation at break after oil resistance = elongation at break before oil soaking / elongation at break after oil soaking * 100%;
[0088] Flame retardant grade test: GB / T 32129-2015;
[0089] Volume resistivity test: GBT 1410-2006.
[0090] The test results are shown in Tables 1-2.
[0091] Table 1
[0092]
[0093]
[0094]
[0095] Table 2
[0096]
[0097]
[0098] From the above data, it can be seen that the tensile strength of the polyolefin composition obtained in each embodiment of the present application is above 12MPa, the elongation at break is above 190%, the flame retardancy grade is B1, the tensile strength retention rate after oil resistance is above 80%, the elongation at break retention rate after oil resistance is above 80%, and the volume resistivity is above 4*10 13 %above.
[0099] Comparative Example 1 directly uses silicone rubber without grafting it onto polyethylene, resulting in poor compatibility with polyolefins, low mechanical properties such as tensile strength and elongation at break, poor flame retardancy, poor oil resistance, and poor insulation.
[0100] Comparative Example 2 directly uses mica powder without coating it with a silane coupling agent, resulting in poor compatibility between it and the polyolefin system, resulting in low mechanical properties such as tensile strength and elongation at break, poor oil resistance, and poor insulation.
[0101] Comparative Examples 3 and 4 did not add mica powder or silicone rubber, resulting in low mechanical properties such as tensile strength and elongation at break, deviation in oil resistance, and deviation in insulation.
[0102] In Comparative Example 5, due to the high amount of polyethylene grafted silicone rubber used, the silicone rubber is easy to coagulate and produce phase separation, resulting in low mechanical properties such as tensile strength and elongation at break; in Comparative Example 6, due to the high amount of mica powder coated with silane coupling agent used, the mechanical properties such as tensile strength and elongation at break are low, and the volume resistivity decreases.
[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A polyolefin composition, characterized in that The composition comprises the following components in parts by weight:
2. The polyolefin composition according to claim 1, characterized in that The mass percentage of silicone rubber in the polyethylene grafted silicone rubber is 28%-72%, preferably 38%-62%.
3. The polyolefin composition according to claim 1, characterized in that The mass percentage of the silane coupling agent in the mica powder coated with the silane coupling agent is 0.3%-4%, preferably 0.8%-2.2%.
4. The polyolefin composition according to claim 1, characterized in that The silane coupling agent in the mica powder coated with the silane coupling agent contains epoxy groups.
5. The polyolefin composition according to claim 4, characterized in that The silane coupling agent in the mica powder coated with the silane coupling agent includes at least one of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and 3-(2,3-epoxypropoxy)propyltriethoxysilane.
6. The polyolefin composition according to claim 1, characterized in that The polyethylene has a melt flow rate of 0.5-3 g / 10 min at 190° C. and 2.16 kg load.
7. The polyolefin composition according to claim 1, characterized in that Satisfy at least one of (a)-(e): (a) the polyethylene is a metallocene linear low density polyethylene; (b) the hydroxide comprises at least one of aluminum hydroxide and magnesium hydroxide; (c) the radiation initiator comprises at least one of TAIC, TMPTMA and TMPTA; (d) the polyolefin composition further comprises 2-5 parts by weight of an antioxidant, wherein the antioxidant comprises at least one of a hindered phenol antioxidant, a phosphite antioxidant, and a thioether antioxidant; (e) The preparation method of the polyethylene grafted silicone rubber comprises the following steps: mixing and dispersing polyethylene and silicone rubber, performing a first open milling, adding an initiator, performing a second open milling, and then extruding and granulating to obtain the polyethylene grafted silicone rubber.
8. The method for preparing a polyolefin composition according to any one of claims 1 to 7, characterized in that: The following steps are involved: Mixing and dispersing raw materials except hydroxide, montmorillonite and mica powder coated with silane coupling agent to obtain a premix; The premix, hydroxide, montmorillonite and mica powder coated with silane coupling agent are mixed and kneaded in proportion, and then extruded and granulated to obtain a polyolefin composition.
9. The method for preparing a polyolefin composition according to claim 8, wherein: The mixing temperature is 130-140°C; the extrusion temperature is 140-160°C.
10. Use of the polyolefin composition according to any one of claims 1 to 9 in cable materials.
Citation Information
Patent Citations
Low-smoke halogen-free inflaming retarding polyolefin photovoltaic cable sheath polyolefin material and method for preparing same
CN103483673A
Cable material, and preparation method and application thereof
CN106380861A
Halogen-free fire-retardant polyolefin insulating material and preparation method thereof
CN109749219A
Polyethylene composition as well as preparation method and application thereof
CN116396551A
Slidability improver for polyolefin resin, polyolefin resin composition, and molded product thereof
JP2015061893A