Polyvinyl alcohol composite hydrogel for wound dressing as well as preparation method and application of polyvinyl alcohol composite hydrogel

By introducing pomegranate peel extract into polyvinyl alcohol and sodium carboxymethylcellulose hydrogel, and using the cyclic freeze-thaw method to prepare polyvinyl alcohol composite hydrogel, the problem in the existing technology that it is difficult to meet the multiple requirements of wound dressings is solved. Efficient wound healing and antibacterial effects are achieved.

CN118812976APending Publication Date: 2024-10-22XINJIANG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410800770.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing technology, it is difficult for polyvinyl alcohol (PVA) hydrogel or its composite to meet the requirements of wound dressings in multiple directions such as mechanical strength, water vapor transmission rate, and swelling rate.

Method used

Polyvinyl alcohol composite hydrogel was prepared using a cyclic freeze-thaw method, adding pomegranate peel extract and sodium carboxymethyl cellulose, optimizing the mass ratio of polyvinyl alcohol and sodium carboxymethyl cellulose and the solvent composition to prepare a hydrogel with a specific swelling rate , water vapor transmission rate and mechanical strength of the dressing.

Benefits of technology

The mechanical strength, water vapor permeability and swelling rate of the polyvinyl alcohol composite hydrogel were improved, meeting the application requirements of wound dressings, and demonstrating good antibacterial and antioxidant effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812976A_ABST
    Figure CN118812976A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wound dressings, and provides polyvinyl alcohol composite hydrogel for wound dressings and a preparation method and application thereof.The polyvinyl alcohol composite hydrogel is prepared through a circulating freeze thawing method, and raw materials for preparing the hydrogel comprise polyvinyl alcohol, sodium carboxymethyl cellulose and a pomegranate peel extract; the mass content of the pomegranate peel extract in the polyvinyl alcohol composite hydrogel is 3%-9%; the mass ratio of the pomegranate peel extract to the polyvinyl alcohol is greater than or equal to 0.8. According to the invention, the pomegranate peel extract is further introduced into a hydrogel system of polyvinyl alcohol and sodium carboxymethyl cellulose, so that the mechanical strength, the water vapor permeability and the swelling rate of the hydrogel of polyvinyl alcohol and sodium carboxymethyl cellulose can be improved at the same time, and the application requirements of wound dressings are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wound dressings, and in particular to a polyvinyl alcohol composite hydrogel for wound dressings, and a preparation method and application thereof. Background Art

[0002] Hydrogel is a polymer of water molecules and hydrophilic polymer networks. The high water content of hydrogel enables it to dissolve and transport ions and many small molecules. Hydrogel can deliver drugs to skin wounds, provide sufficient water and oxygen to the wounds, accelerate wound healing, and have a certain mechanical strength to protect the wounds from secondary damage. Therefore, hydrogel has great application potential in the field of wound dressings.

[0003] Swelling is one of the basic properties of hydrogels. Reference 1 (PVA / Poly(hexamethylene guanidine) / Gallic Acid Composite Hydrogel Films and Their Antibacterial Performance[J].ACS Applied Polymer Materials, 2021, 3(8):3867-3877.) and Reference 2 (Incorporation of ZnO nanoparticles into heparinised polyvinyl alcohol / chitosan hydrogels for wound dressing application[J].International Journal of Biological Macromolecules, 2018, 114:1203-1215.) show that properly swollen hydrogels can absorb wound exudate and promote wound healing, but excessive swelling may lead to dual infection. The swelling rate of an ideal wound dressing is about 100-900%. And document 3 (Self-crosslinked chitosan / Kappa-carrageenan-based biomimetic membranes to combat diabetic burn wound infections [J]. International Journal of Biological Macromolecules, 2022, 197: 157-168.) shows that appropriate water vapor transmission rate (WVTR) is a necessary condition for wound dressings. The WVTR should not be too high, otherwise it may cause wound dehydration; it should not be too low, otherwise it will cause accumulation of wound exudate. The ideal dressing has a WVTR of 2000-2500 g / (m2 ·d) within the scope.

[0004] Polyvinyl alcohol (PVA) is a water-soluble polyhydroxy polymer that has been made into hydrogels for wound dressings due to its excellent mechanical strength, biocompatibility and non-toxicity. However, the polyvinyl alcohol (PVA) hydrogels or polyvinyl alcohol hydrogels combined with other natural compounds prepared in the prior art are difficult to meet the requirements of wound dressings in multiple aspects such as the above-mentioned mechanical strength, water vapor permeability and swelling rate.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The present invention provides a polyvinyl alcohol composite hydrogel for wound dressing and a preparation method and application thereof, so as to solve the defect that polyvinyl alcohol (PVA) hydrogel or polyvinyl alcohol composite hydrogel of other natural compounds in the prior art is difficult to meet the requirements of wound dressing in multiple aspects such as the above-mentioned mechanical strength, water vapor permeability and swelling rate.

[0007] In a first aspect, the present invention provides a polyvinyl alcohol composite hydrogel prepared by a cyclic freeze-thaw method; the raw materials for preparing the polyvinyl alcohol composite hydrogel include polyvinyl alcohol, sodium carboxymethyl cellulose and pomegranate peel extract.

[0008] The mass content of the pomegranate peel extract in the polyvinyl alcohol composite hydrogel is 3% to 9%.

[0009] The mass ratio of the pomegranate peel extract to polyvinyl alcohol is greater than or equal to 0.8, preferably 0.8-1.15.

[0010] The pomegranate peel extract is prepared by taking pomegranate peel as a main raw material, taking ethanol as an extraction solvent and taking petroleum ether as an extraction solvent.

[0011] According to the polyvinyl alcohol composite hydrogel provided by the present invention, the mass ratio of the polyvinyl alcohol to sodium carboxymethyl cellulose is 12:0.1-0.2.

[0012] According to the polyvinyl alcohol composite hydrogel provided by the present invention, the solvent for preparing the hydrogel includes glycerol and water; preferably, the mass ratio of the glycerol to water is 0.5-1.5:1.

[0013] According to the polyvinyl alcohol composite hydrogel provided by the present invention, the swelling rate of the polyvinyl alcohol composite hydrogel is 150% to 900%, and the water vapor permeability is 2000 to 2500 g / (m 2 d), the tensile strength is 0.3 MPa or more.

[0014] In a second aspect, the present invention also provides a method for preparing the polyvinyl alcohol composite hydrogel as described above, comprising: preparing pomegranate peel extract; The pomegranate peel extract is added to a mixed solution of polyvinyl alcohol and sodium carboxymethyl cellulose to obtain a hydrogel solution; The hydrogel solution is prepared by a cyclic freeze-thaw method to obtain the polyvinyl alcohol composite hydrogel.

[0015] According to the method for preparing the polyvinyl alcohol composite hydrogel provided by the present invention, the preparation of a mixed solution of polyvinyl alcohol and sodium carboxymethyl cellulose comprises: Adding polyvinyl alcohol to a mixed solution of glycerol and water to obtain a polyvinyl alcohol solution; Adding sodium carboxymethyl cellulose to a mixed solution of glycerol and water to obtain a sodium carboxymethyl cellulose solution; The polyvinyl alcohol solution and the sodium carboxymethylcellulose solution are mixed.

[0016] Preferably, the mass concentration of polyvinyl alcohol in the polyvinyl alcohol solution is 5-15%.

[0017] Preferably, the mass concentration of sodium carboxymethyl cellulose in the sodium carboxymethyl cellulose solution is 0.5-2%.

[0018] According to the preparation method of the polyvinyl alcohol composite hydrogel provided by the present invention, the cyclic freeze-thaw method comprises: the freezing temperature is -90 to -10°C, and the thawing temperature is 4 to 25°C.

[0019] Preferably, the freeze-thaw cycle method comprises: freezing at a temperature of -30 to -10°C for 5 to 10 hours, and thawing at a temperature of 20 to 25°C for 0.5 to 3 hours.

[0020] No stirring is required between two consecutive freeze-thaw cycles.

[0021] According to the preparation method of the polyvinyl alcohol composite hydrogel provided by the present invention, the preparation of pomegranate peel extract includes: preparing pomegranate peel powder from the washed pomegranate peel, then mixing the pomegranate peel powder with an ethanol aqueous solution, standing for extraction at a certain temperature, extracting the obtained supernatant with petroleum ether, rotating and concentrating, and then freeze-drying to obtain the extract.

[0022] Preferably, the volume fraction of the ethanol aqueous solution is 40-60%.

[0023] Preferably, the mass volume ratio of the pomegranate peel powder to the ethanol aqueous solution is 100g:4-5L.

[0024] Preferably, the certain temperature is 60-100°C.

[0025] Preferably, the static extraction time is 1 to 2 hours.

[0026] Preferably, the supernatant is extracted with petroleum ether for 3 to 5 times and then concentrated by rotation.

[0027] In a third aspect, the present invention further provides a wound dressing, comprising the polyvinyl alcohol composite hydrogel as described above.

[0028] According to the wound dressing provided by the present invention, the polyvinyl alcohol composite hydrogel is used to destroy bacterial cell membranes; preferably, the cumulative release rate of the pomegranate peel extract of the polyvinyl alcohol composite hydrogel within 72 hours is more than 60%.

[0029] The present invention provides a polyvinyl alcohol composite hydrogel for wound dressing, a preparation method and an application thereof. By further introducing pomegranate peel extract into a hydrogel system of polyvinyl alcohol and sodium carboxymethyl cellulose, it is found that when a specific content of pomegranate peel extract is added, the mechanical strength, water vapor permeability and swelling rate of the hydrogel of polyvinyl alcohol and sodium carboxymethyl cellulose can be improved at the same time, reaching a swelling rate of 150% to 900%, and a water vapor permeability of 2000 to 2500 g / (m 2 d) The tensile strength is above 0.3MPa, which meets the application requirements of wound dressing.

[0030] The release of PPE in the polyvinyl alcohol composite hydrogel prepared by the present invention is mainly attributed to the concentration difference between the inside and the outside, and the cumulative release rate can exceed 70%. It has good free radical scavenging effect and antibacterial effect, and its scavenging rate for DPPH and ABTS free radicals is greater than 90%, and the antibacterial rate for S. aureus and E. coli can reach more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 These are the test results of different substances provided by the present invention, wherein (a) is the FTIR spectrum and (b) is the XRD diagram.

[0033] Figure 2 These are the test results of the transparency of different hydrogels provided by the present invention.

[0034] Figure 3 These are the test results of the swelling properties and hydrophilicity of different hydrogels provided by the present invention; wherein (a) is swelling property and (b) is hydrophilicity.

[0035] Figure 4 It is the test result of the water vapor permeability of different hydrogels provided by the present invention.

[0036] Figure 5 These are the test results of the anti-drying properties of different hydrogels provided by the present invention; wherein (a) is the water loss rate curve, and (b) is the water content.

[0037] Figure 6 1 is a graph showing the tensile test results of different hydrogels provided by the present invention, wherein (a) is a stress-strain curve, (b) is a tensile strength, and (c) is an elongation at break.

[0038] Figure 7 1 and 1. The antioxidant test results of different hydrogels provided by the present invention are shown in FIG. 1 , wherein FIG. (a) shows the color change of DPPH solution and ABTS solution, (b) shows the scavenging rate of DPPH free radicals by the hydrogel, and (c) shows the scavenging rate of ABTS free radicals by the hydrogel.

[0039] Figure 8 1 is the release curve of PPE in different hydrogels provided by the present invention.

[0040] Fig. 9 Graphs showing the antibacterial test results of different hydrogels provided by the present invention, wherein (a) is an inhibition zone graph, (b) is an inhibition zone size, (c) is a colony graph after co-culture, (d) is an inhibition rate, and (e) is a fluorescence graph and a SEM graph. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Combine the following Figure 1-Figure 9 The invention describes a polyvinyl alcohol composite hydrogel for wound dressing and a preparation method and application thereof.

[0043] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0044] Specifically, they include:

[0045] The preparation method of the pomegranate peel extract in the embodiment of the present invention is as follows: wash the pomegranate peel, dry it in a cool and dry place, grind it into powder, and pass it through a 40-mesh sieve to obtain pomegranate peel powder.

[0046] Take 100 g of the above pomegranate peel powder and add it to 4.8 L of ethanol (volume fraction 50%), let it stand in a water bath at 80°C for 2 h, filter out the supernatant, extract it with petroleum ether three times, concentrate it by rotation and freeze-dry it to obtain PPE (pomegranate peel extract).

[0047] The following examples are given for the preferred embodiments of the present invention.

[0048] Example 1

[0049] A method for preparing a composite hydrogel, the steps of which are as follows: (1) Using 50% GL (glycerol) aqueous solution as solvent, a 10% PVA (polyvinyl alcohol) solution and a 1% Na-CMC (sodium carboxymethyl cellulose) solution were prepared respectively.

[0050] (2) PVA solution and Na-CMC solution were mixed at a solution mass ratio of 12:1.5 to prepare PVA / Na-CMC solution, referred to as PC solution; (3) PPE (pomegranate peel extract) was added to the PC solution to obtain a hydrogel solution with a PPE mass concentration of 7%.

[0051] (4) The hydrogel solution was stirred at 60°C for 2 h, frozen at -20°C for 8 h, thawed at room temperature for 1 h, and the freeze-thaw cycle was continued for 2 more times to obtain a hydrogel, which was designated as PCP-7.

[0052] Example 2

[0053] A method for preparing a composite hydrogel, wherein the steps are substantially the same as those of Example 1, except that the mass concentration of PPE in step (3) is increased to 9%, thereby obtaining a hydrogel, which is designated as PCP-9.

[0054] Comparative Example 1

[0055] A method for preparing a hydrogel is to prepare a PC hydrogel using the PC solution prepared in step (2) of Example 1 according to the method of step (4) of Example 1.

[0056] Comparative Example 2

[0057] A method for preparing a composite hydrogel, wherein the steps are substantially the same as those of Example 1, except that the mass concentration of PPE in step (3) is increased to 3% to obtain a hydrogel, which is designated as PCP-3.

[0058] Comparative Example 3

[0059] A method for preparing a composite hydrogel, wherein the steps are substantially the same as those of Example 1, except that the mass concentration of PPE in step (3) is increased to 5% to obtain a hydrogel, which is denoted as PCP-5.

[0060] The testing method of the present invention comprises: (1) Infrared spectrum test

[0061] The dried hydrogel was mixed with an appropriate amount of solid potassium bromide and its chemical structure was analyzed and tested using a Fourier transform infrared spectrometer at 4000-400 cm -1 Scan within the range.

[0062] (2) XRD test

[0063] The hydrogel samples were freeze-dried and X-ray diffractometer was used to perform XRD analysis on the hydrogels.

[0064] (3) Transparency test

[0065] The transmittance of the hydrogel was tested using a UV-visible spectrophotometer with a scanning range of 400-800 nm.

[0066] (4) Swelling test

[0067] The swelling properties of the hydrogel were tested using the mass method. A certain mass of gel sample was weighed and dried at 60°C to a constant weight (m0), and then the sample was immersed in deionized water at 37°C. The sample was taken out at 0.5h, 1h, 2h, 3h, 5h, 7h, 9h, 12h, 24h, 48h, and 72h, and the surface liquid was wiped off with filter paper, and the mass (mt) was weighed. The swelling rate (SR) was calculated as follows: SR(%)=[(mt-m0) / m0]×100%; Where: m0: dry weight of sample (g); mt: mass of sample at time point t (g).

[0068] (5) Hydrophilicity test

[0069] The water contact angle of the hydrogel surface was tested at room temperature using a contact angle analyzer. 1 μL of deionized water was dropped on the sample surface for measurement. Three different locations were randomly selected for measurement on each sample. Each set of data was recorded and the average value was used as the contact angle of the hydrogel.

[0070] (6) Water vapor transmission rate test

[0071] The water vapor permeability of the hydrogel was tested by the weighing method. PBS was added to the test tube, and then the dried hydrogel was cut into an appropriate circle with a diameter approximately equal to the mouth of the test tube. The sample was covered at the mouth of the test tube and the edges were sealed. Finally, all containers were placed at 37°C and 35% relative humidity for 24 hours. The water vapor permeability (WVTR) was calculated as follows: WVTR = (w1-w0) / A; Where: A is the penetration area of ​​the sample, w1 is the final weight of the container, and w0 is the initial weight of the container.

[0072] (7) Anti-drying test

[0073] The water loss rate is used to evaluate the anti-drying performance of the hydrogel. Different hydrogels were cut into appropriate shapes and weighed (M0), and stored at room temperature for 24 hours. The weight of the hydrogel sample (Mt) was recorded at 0, 1, 3, 5, 7, 9, 12, 24, 48, and 72 hours respectively. The water loss rate (Water loss) is calculated as follows: Water loss (%)=(M0-Mt) / M0×100%; Where: M0 and Mt are the initial weight and weight of the hydrogel at time t, respectively.

[0074] (8) Mechanical properties test

[0075] Use an electronic tensile testing machine to test the tensile properties of the hydrogel. Preparation: Use a thickness gauge to test the thickness of the sample, and cut the hydrogel into a dumbbell shape with an overall length of about 30mm and a width of 10mm at both ends for easy clamping; the length of the middle test part is 10mm and the width is 5mm. Stretch the sample to break at a tensile rate of 50mm / min and record the data. Test each sample 5 times and calculate the tensile performance value of the hydrogel.

[0076] (9) Release kinetics study

[0077] Weigh 10 mg of hydrogel and soak it in 20 mL of PBS, oscillate at 37 ° C and 120 r / min. Take out 3 mL of solution at 0.5, 1, 2, 3, 6, 9, 12, 24, 48, and 72 h, add the same volume of PBS buffer, keep the volume of the solution in the test tube constant, and use the gallic acid standard curve to measure the release of PPE. Among them, the drawing of the gallic acid standard curve includes: weigh 15.2 mg of gallic acid standard and dissolve it in 250 mL of deionized water. Take 5 test tubes, add 1, 2, 3, 4, and 5 mL of gallic acid solution, add 0.5 mL of Folin phenol reagent and 4 mL of 7.5% (w / v) sodium carbonate solution to each test tube, and dilute to 10 mL with deionized water. After reacting in the dark for 30 minutes at room temperature, test the absorbance at a wavelength of 765 nm.

[0078] (10) Antioxidant performance test

[0079] Weigh 200 mg of hydrogel and mix with 4 mL of DPPH and ABTS solution respectively, protect from light, and measure the absorbance of the free radical solution at 512 nm and 734 nm respectively. The free radical scavenging ability (K) of the hydrogel is calculated as follows:

[0080] In the formula, A1: absorbance value of blank group, A0: absorbance value of experimental group

[0081] (11) Antibacterial performance test

[0082] The antibacterial activity of the hydrogel against S. aureus and E. coli was tested by the inhibition zone method and plate count method.

[0083] Inhibition zone method: Cut the hydrogel into a circle with a diameter of 10 mm and sterilize it under UV for 1 hour. Slowly pour the agar culture solution sterilized by high temperature and high pressure into the culture dish and cool it to solidify. Take 100 μL of the bacterial solution (10 6 ~10 7 CFU / mL) was coated on the culture medium and the sterilized hydrogel sample was placed. Finally, the culture dish was placed in a constant temperature environment of 37°C for 18h to 24h, the antibacterial effect was observed, and the diameter of the antibacterial zone was measured.

[0084] Plate counting method: Test the antibacterial rate of hydrogel. Cut the hydrogel into round shapes and sterilize with UV light. 6 ~10 7 CFU / mL) and 5mL PBS were added to the test tube after high temperature and high pressure sterilization, mixed evenly, and incubated at 37°C and 120r / min for 24h. 100μL of the mixture was drawn from the test tube, spread on the culture medium, and recorded the colony after incubation at 37°C for 18h. The bacterial suspension that was not incubated with the hydrogel was used as the blank group, and the experiment was repeated three times. The calculation formula of the antibacterial rate is as follows: Inhibition rate (%) = (number of colonies in the blank control group - number of colonies in the experimental group) / number of colonies in the blank control group × 100%; The bacteria were stained with DAPI and PI, and then dehydrated with ethanol to observe their surface morphology.

[0085] Fluorescence staining was used to detect the integrity of bacterial cell membranes. S. aureus and E. coli bacterial suspensions were mixed with PPE (1×MIC) and cultured for 24 hours, the cells were collected by centrifugation, and the cells were washed with PBS. A mixture of DAPI (40μg / mL) and PI (40μg / mL) was added and stained for 15 minutes in the dark. Excess dye was washed off with PBS, and the bacteria were observed using a fluorescent inverted microscope.

[0086] Use SEM to observe the morphology of bacteria after incubation with PPE. Mix S. aureus and E. coli bacterial suspension with PPE (1×MIC) and co-culture for 24 hours, and collect the bacteria by centrifugation. Soak the bacteria in 2.5% glutaraldehyde solution, place at 4°C for 12 hours, remove the supernatant after centrifugation; use concentration gradient (30, 40, .... 100%) of ethanol to gradually dehydrate the bacteria, each gradient dehydration for 10 minutes, and observe the morphology of the bacteria by SEM.

[0087] The above PPE raw materials, PC hydrogel, PCP-3, PCP-5, PCP-7, PCP-9 were subjected to the above tests, and the test results are as follows: (1) Figure 1 As shown in (a), PC hydrogel at 3382.56 cm -1 A broad peak appears at 2940.09cm, which is related to the stretching vibration of -OH. The stretching vibration of -OH is derived from the multiple cooperative hydrogen bond systems formed by the combination of GL molecules and PVA chains during the freeze-thaw process. -1 and 2886.53cm -1 The double peak of CH stretching is mainly due to the addition of PPE. The -OH vibration peak of the hydrogel has a significant shift from 3382.56 cm -1 Move to 3378.77cm -1 (PCP-3) and 3339.99cm -1 (PCP-7). PC hydrogel at 1647.99cm -1 and 1233cm -1 The absorption peak at 40° moves to a higher wavenumber. In addition, after adding PPE, no new absorption peak appears in the hydrogel spectrum, and only the migration of the absorption peak is observed, indicating that there is no obvious chemical reaction between PPE and the hydrogel.

[0088] like Figure 1As shown in (b), the absorption peaks of the PC hydrogel curve appear at 2θ=19.46° and 40.68°. It can be clearly seen from the figure that the peak at 19.46° is sharper and stronger, indicating that the PC hydrogel has a higher degree of crystallinity, which may be caused by the molecular interaction between the molecular chains. The curve of PCP-3 almost coincides with the curve of PC, indicating that the addition of 3% PPE has little effect on the crystallinity of the hydrogel. As the PPE content in the hydrogel increases, the width of the absorption peak increases and the intensity decreases, indicating that the crystallinity of the hydrogel gradually decreases. This phenomenon may be because the addition of PPE affects the formation of hydrogen bonds between molecular chains and increases the amorphous area.

[0089] (2) Figure 2 As shown in the figure, PC hydrogel has a good transmittance of 75.37-91.31% in the visible light range (400-800nm). This is because GL will disrupt the order of the molecular chain and increase the transmittance of the hydrogel. Compared with PC, due to the influence of the pigment in PPE, as the PPE content in the hydrogel increases, its transmittance gradually decreases, and at 600nm, it is 55.08%, 39.05%, 14.79% and 4.20% respectively.

[0090] (3) Figure 3 As shown in (a), both PC hydrogel and PCP hydrogel showed appropriate swelling behavior and maintained good shape and transparency after swelling for 72 hours. From 0h to 12h, the swelling rate of each component hydrogel increased significantly, and the swelling rate was close to equilibrium after immersion for 12h. The PC hydrogel had the lowest swelling degree, about 167.35±7.07%. With the increase of PPE content, the swelling degree of PCP hydrogel gradually increased, which were 184.41±6.14%, 190.11±9.13%, 206.13±6.95%, and 223.05±6.42%, respectively. This may be because the addition of PPE reduces the number of hydroxyl chain entanglement points on the PVA and GL chains, reduces the rigidity and crystallinity of the hydrogel, and increases the amorphous area.

[0091] PPE is a water-soluble substance, and the hydrophilicity of the hydrogel increases with the increase of PPE content. Figure 3 As shown in (b), the water contact angle of PC is 51.80±3.73°, while after adding PPE, the contact angle decreases to 19.4±2.05° (PCP-9).

[0092] (4) Figure 4 As shown in Figure 2, the WVTR of the PC group was 1373.03±61.22 g / (m 2 ·d), with the increase of PPE content, the WVTR of the hydrogel increased. Among them, the WVTR of PCP-7 and PCP-9 were 2025.56±96.63g / (m2 ·d) and 2041.87±131.86g / (m 2 ·d). Therefore, the prepared PPE-loaded composite hydrogel has an acceptable WVTR.

[0093] (5) Figure 5 As shown in (a), the water loss rates of the hydrogels at 12 h were 27.79 ± 0.31% (PC), 31.21 ± 0.94% (PCP-3), 32.19 ± 0.84% ​​(PCP-5), 35.75 ± 0.75% (PCP-7), and 38.97 ± 1.07% (PCP-9), respectively, and gradually approached the water content of each gel (e.g. Figure 5 (b) As the PPE content increases, the water loss rate of the hydrogel increases, which is consistent with the swelling results. The PC hydrogel has low swelling and hydrophilicity and a slow water loss rate, while the PPE-loaded hydrogel has the opposite effect, which is also related to the properties of the hydrogel. Figure 5 (a) It can also be seen that the hydrogel remains intact after losing water, without collapse, etc. This is because GL can replace water molecules to form hydrogen bonds with PVA and maintain the stability of the gel structure.

[0094] (6) As a wound dressing, the hydrogel needs to have certain mechanical properties to ensure that it can remain intact under external forces to ensure its protection of the wound. Through uniaxial tensile tests, the mechanical test results of PPE composite hydrogel are as follows Figure 6 As shown. With the increase of PPE concentration, the strength and elongation of the hydrogel showed a trend of first increasing and then decreasing. Among them, PCP-7 had the best mechanical properties, with a tensile strength of 0.33±0.02MPa and an elongation at break of 395.99±16.54%. The reason may be that the lower concentration of PPE forms hydrogen bonds or intermolecular interactions with polymer molecules, which enhances the strength and elasticity of the hydrogel. When the PPE concentration is high, it will affect the cross-linking degree and crystallinity of the hydrogel, resulting in a decrease in the mechanical properties of the hydrogel. Therefore, an appropriate PPE concentration can improve the mechanical properties of the composite hydrogel.

[0095] (7) Excessive oxidative stress will produce a large number of free radicals that attack and damage normal cells, delaying the wound healing process. Therefore, wound dressings should have the ability to scavenge free radicals. DPPH and ABTS free radicals have been widely used to detect the antioxidant activity of materials. The scavenging effect of hydrogels on free radicals is shown in Figure 2. Figure 7 As shown. The PC sample as the control group did not show antioxidant activity. The PPE composite hydrogel had a strong scavenging ability against DPPH and ABTS free radicals, making the two free radical solutions transparent ( Figure 7(a)). The scavenging rates of PCP hydrogel on both free radicals were above 90%, while the PC group could hardly scavenge free radicals ( Figure 7 This is because PPE contains a large amount of polyphenolic compounds, which have strong reducing properties. As the concentration of PPE increases and is released, the hydrogel has good antioxidant activity.

[0096] (8) Drug release research is a very important factor, which is directly related to the final therapeutic effect of the active drug. The release curve of PPE in hydrogel is as follows Figure 8 As shown. The release process of PPE has about three stages: initial burst release, sustained release and equilibrium release. The hydrogel rapidly released PPE within 9 hours and gradually approached equilibrium after 12 hours. Among them, the cumulative release rates of PPE within 9 hours were 61.53±1.35% (PCP-3), 63.34±1.67% (PCP-5), 69.49±0.9% (PCP-7), and 73.92±0.97% (PCP-9). At the same time, with the increase of PPE concentration in the hydrogel, the cumulative release rates of each hydrogel within 72 hours increased, which were 65.05±0.45% (PCP-3), 68.61±2.46% (PCP-5), 73.05±1.39% (PCP-7), and 77.27±1.52% (PCP-9).

[0097] In order to explain the release mechanism of PPE, the present invention adopts zero-order model, first-order model, Higuchi model and Korsmeyer-Peppas model to simulate the PPE release kinetics of hydrogel. After fitting the release curve, it is found that the release amount of PPE in all hydrogels has a high degree of fit with the first-order.

[0098] (9) Wound dressings should have antibacterial properties to reduce the possibility of wound infection. The results of the inhibition zone of hydrogel against S. aureus and E. coli are as follows: Fig. 9 As shown in (a), PC hydrogel was used as the control group, and no antibacterial zone was observed. As the concentration of PPE increased, the diameter of the antibacterial zone of the hydrogel gradually increased (e.g. Fig. 9 (b)). Among them, the diameters of the inhibition zones of PCP-3 group against S. aureus and E. coli were 18.65±0.79mm and 16.94±0.46mm, and gradually increased to 23.68±0.36mm and 21.24±0.59mm in PCP-9 group. Fig. 9(c) As shown. A large number of colonies were found in both the blank group and the PC hydrogel, and as the PPE content in the hydrogel increased, the number of colonies on the culture medium gradually decreased. Compared with the PC hydrogel, the inhibition rates of the other four groups of hydrogels against the two bacteria were all above 90% (as shown in Figure 2). Fig. 9 (d)), the inhibition rates of PCP-3 against S. aureus and E. coli were 93.39±0.62% and 93.32±2.65%, respectively, and the inhibition rates of PCP-9 against the two bacteria were 99.82±0.14% and 99.61±0.11%, respectively. The concentration of PPE affected the inhibition rate of the hydrogel, which was consistent with the release curve results (as shown in Fig. Fig. 9 This result may be because PPE contains a large amount of polyphenols, which can effectively inhibit the growth and reproduction of bacteria.

[0099] In order to further prove the antibacterial ability of hydrogels against bacteria, PC hydrogel and PCP-3 hydrogel with the least PPE content were selected as experimental groups, and the integrity of bacterial membranes was studied using DAPI and PI fluorescent dyes, and the surface morphology of bacteria was observed by SEM. Fig. 9 As shown in (e), the bacteria incubated with PC hydrogel were stained blue, with complete bacterial morphology, spherical and rod-shaped, and smooth cell surfaces. The bacteria incubated with PCP-3 hydrogel were stained with significantly more red, and SEM observed that some bacteria had no fixed shape, and the cell surface was damaged, collapsed, and the cell contents leaked. This shows that PPE composite hydrogel can inhibit bacterial growth by destroying the bacterial cell membrane.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A polyvinyl alcohol composite hydrogel prepared by a freeze-thaw cycle method, characterized in that: include: The raw materials for preparing the polyvinyl alcohol composite hydrogel include polyvinyl alcohol, sodium carboxymethyl cellulose and pomegranate peel extract; The mass content of pomegranate peel extract in the polyvinyl alcohol composite hydrogel is 3% to 9%; The mass ratio of the pomegranate peel extract to polyvinyl alcohol is greater than or equal to 0.8; The pomegranate peel extract is prepared by taking pomegranate peel as a main raw material, taking ethanol as an extraction solvent and taking petroleum ether as an extraction solvent.

2. The polyvinyl alcohol composite hydrogel according to claim 1, characterized in that: The mass ratio of the polyvinyl alcohol to sodium carboxymethyl cellulose is 12:0.1-0.

2.

3. The polyvinyl alcohol composite hydrogel according to claim 1 or 2, characterized in that: The solvent for preparing the hydrogel includes glycerol and water; preferably, the mass ratio of glycerol to water is 0.5-1.5:

1.

4. The polyvinyl alcohol composite hydrogel according to any one of claims 1 to 3, characterized in that: The swelling rate of the polyvinyl alcohol composite hydrogel is 150% to 900%, and the water vapor permeability is 2000 to 2500 g / (m 2 d), the tensile strength is 0.3 MPa or more.

5. The method for preparing the polyvinyl alcohol composite hydrogel according to any one of claims 1 to 4, characterized in that: include: preparing pomegranate peel extract; The pomegranate peel extract is added to a mixed solution of polyvinyl alcohol and sodium carboxymethyl cellulose to obtain a hydrogel solution; The hydrogel solution is prepared by a cyclic freeze-thaw method to obtain the polyvinyl alcohol composite hydrogel.

6. The method for preparing the polyvinyl alcohol composite hydrogel according to claim 5, characterized in that: The preparation of the mixed solution of polyvinyl alcohol and sodium carboxymethyl cellulose comprises: Adding polyvinyl alcohol to a mixed solution of glycerol and water to obtain a polyvinyl alcohol solution; Adding sodium carboxymethyl cellulose to a mixed solution of glycerol and water to obtain a sodium carboxymethyl cellulose solution; The polyvinyl alcohol solution and the sodium carboxymethylcellulose solution are mixed. Preferably, the mass concentration of polyvinyl alcohol in the polyvinyl alcohol solution is 5 to 15%; Preferably, the mass concentration of sodium carboxymethyl cellulose in the sodium carboxymethyl cellulose solution is 0.5-2%.

7. The method for preparing the polyvinyl alcohol composite hydrogel according to claim 5 or 6, characterized in that: The freeze-thaw cycle method includes: the freezing temperature is -90 to -10°C, and the thawing temperature is 4 to 25°C; Preferably, the freeze-thaw cycle method comprises: freezing at a temperature of -30 to -10°C for 5 to 10 hours, and thawing at a temperature of 20 to 25°C for 0.5 to 3 hours.

8. The method for preparing the polyvinyl alcohol composite hydrogel according to any one of claims 5 to 7, characterized in that: The preparation of pomegranate peel extract comprises: preparing pomegranate peel powder from washed pomegranate peel, then mixing the pomegranate peel powder with ethanol water solution, extracting at a certain temperature, extracting the obtained supernatant with petroleum ether, rotating and concentrating, and then freeze-drying to obtain the extract. Preferably, the volume fraction of the ethanol aqueous solution is 40-60%; Preferably, the mass volume ratio of the pomegranate peel powder to the ethanol aqueous solution is 100 g: 4-5 L; Preferably, the certain temperature is 60-100°C; Preferably, the static extraction time is 1 to 2 hours; Preferably, the supernatant is extracted with petroleum ether for 3 to 5 times and then concentrated by rotation.

9. A wound dressing, characterized in that: The invention comprises the polyvinyl alcohol composite hydrogel as described in any one of claims 1 to 4.

10. The wound dressing according to claim 9, characterized in that: The polyvinyl alcohol composite hydrogel is used to destroy bacterial cell membranes; preferably, the cumulative release rate of the pomegranate peel extract of the polyvinyl alcohol composite hydrogel within 72 hours is more than 60%.