Application of paraffin oil in flame retardance of paint and application method
By adding paraffin oil to the paint and stirring or ultrasonic treatment, combined with coupling agents and dispersants, the problem of flammable and explosive paints is solved, the flame retardant performance and anti-freeze ability of the paint are improved, the production process is simplified, and Reduced costs.
Patent Information
- Application Number
- CN202411073731.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-22
AI Technical Summary
The problem of flammable and explosive paints poses safety hazards during production, storage and use, and it is difficult for existing technology to provide a simple, economical and widely used solution to improve the flame retardant and anti-freeze properties of paints.
By adding 10 to 30 parts of paraffin oil to the paint, stirring or ultrasonic treatment, and combining coupling agents and dispersants to form a highly flame-retardant paint mixture, the flame-retardant performance and frost resistance of the paint can be improved.
It achieves high flame retardant performance and improved frost resistance of the paint, simplifies the production process, reduces production costs, improves the adhesion effect of the paint, and enhances public safety requirements.
Smart Images

Figure CN118813084A_ABST
Abstract
Description
Technical Field
[0001] The invention specifically relates to an application of paraffin oil in flame retardancy of paint and an application method. Background Art
[0002] Paint is a very common industrial product in petroleum fine chemicals. Paint is a viscous oily pigment that is flammable when wet. This is because the main raw materials for producing paint are resin and aromatic solvents, both of which are flammable and explosive.
[0003] The resin itself is easy to burn, which is its basic characteristic. The flammability of the resin is related to its molecular structure. The molecules contain more oxygen atoms and Ruthenium atoms. These atoms cause the resin to react violently when it meets oxygen or Ruthenium atoms, leading to fire. The resin material also contains flammable additives, fillers, fillers, colorants and other ingredients that can easily increase the flammability of the resin. Therefore, the flammability of the resin is inevitable. Aromatic solvents are flammable and explosive products because their vapors can easily form explosive mixtures when in contact with air. This type of solvent also has a high boiling point and solubility. These characteristics make it extremely potential safety hazards and even explosions during storage, transportation and use. The flash point of aromatic solvents is too low, only 60°C, which means they can evaporate at a certain temperature and form flammable gases. When encountering a fire source or spark in the air, there is a possibility of combustion or explosion. Flammable and explosive aromatic solvents have a high vapor pressure and can quickly evaporate into flammable gases, easily forming flammable vapor clouds. Aromatic solvents also have a wide explosion limit range, which means they can form a flammable mixture when mixed with oxygen in the air within a certain concentration range.
[0004] In view of the problem that paint is flammable and explosive, it is necessary to provide a simple and economical method that can be widely used in actual production and has low cost. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an application of paraffin oil in flame retardancy of paint and an application method, which can improve the flame retardancy of paint through a simple method, and also improve the antifreeze performance and enhance the adhesion effect of paint.
[0006] The technical solutions adopted are:
[0007] The invention discloses an application of paraffin oil in flame retardancy of paint.
[0008] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0009] (1) weighing raw materials by weight, wherein the raw materials include 10 to 30 parts of paraffin oil and 70 to 90 parts of paint;
[0010] (2) Pour paraffin oil into the paint first and stir evenly to obtain an oil-gas mixture with high flame retardancy.
[0011] Preferably, the kinematic viscosity of the paraffin oil at 40°C is 8 to 30 mm 2 / s.
[0012] Preferably, the raw material further comprises a coupling agent, and the weight portion of the coupling agent is 1 to 3 parts.
[0013] Preferably, the coupling agent is an organic silane coupling agent.
[0014] Preferably, the raw material further comprises a dispersant, the weight portion of which is 2 to 5 parts.
[0015] Preferably, the dispersant is a mixture of one or more of polyoxyethylene alkylphenol ether, fatty amine polyoxyethylene ether or oleyl alcohol polyoxyethylene ether.
[0016] Preferably, the coupling agent is first added, and then mechanically stirred to be uniform, and then the dispersant is added, and then mechanically stirred to be uniform;
[0017] Alternatively, the paint mixture can be made uniform by ultrasonic treatment, that is, ultrasonic treatment is performed at room temperature with a frequency of 20 to 40 kHz and a power of 60 to 90 W, and finally allowed to stand for 5 to 10 minutes.
[0018] Preferably, after adding paraffin oil, the method of stirring evenly is ultrasonic treatment, that is, the frequency of ultrasonic treatment at room temperature is 30-50kHz, the power is 80-100W, and the time of ultrasonic treatment is 15-30min; after sufficient mixing, it is then allowed to stand for 10-20min.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention can improve the flame retardant property and antifreeze ability of the paint by adding paraffin oil, the method is simple, easy to implement and does not require complicated equipment.
[0021] The application method of the present invention is added to the paint during production, and the preparation time is short. After completion, the ideal flame retardant performance can be achieved, and the public safety requirements can be improved. At the same time, the adhesion effect of the paint can be improved, the production cost can be reduced, and it can be widely promoted and used. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a flow chart of Example 5 of the application method of the present invention. DETAILED DESCRIPTION
[0023] The accompanying drawings are only used for exemplary description; in order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as a limitation of this patent.
[0024] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.
[0025] Example 1
[0026] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0027] (1) Weigh the raw materials by weight: 15 parts of paraffin oil and 85 parts of paint;
[0028] (2) Pour paraffin oil into the paint and stir mechanically until it is evenly mixed to obtain a paint mixture. Mechanical stirring takes a long time and the degree of uniformity is difficult to control.
[0029] Example 2
[0030] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0031] (1) Weigh the raw materials by weight: 20 parts of paraffin oil and 80 parts of paint;
[0032] (2) Pour paraffin oil into the paint and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, and the ultrasonic treatment time is 15 minutes. Let it stand for 15 minutes to obtain a paint mixture.
[0033] Example 3
[0034] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0035] (1) Weigh the raw materials by weight: 10 parts of paraffin oil and 90 parts of paint;
[0036] (2) Pour paraffin oil into the paint and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, the ultrasonic treatment time is 15 minutes, and the paint is allowed to stand for 15 minutes.
[0037] Example 4
[0038] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0039] (1) Weigh the raw materials by weight: 25 parts of paraffin oil and 75 parts of paint;
[0040] (2) Pour paraffin oil into the paint and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, the ultrasonic treatment time is 15 minutes, and the paint is allowed to stand for 15 minutes.
[0041] Example 5
[0042] like Figure 1 As shown, a method for applying paraffin oil to flame retardant paint comprises the following steps:
[0043] (1) Weigh the raw materials by weight: 15 parts of paraffin oil, 80 parts of paint, 2 parts of coupling agent, and 3 parts of dispersant;
[0044] (2) Pour paraffin oil into the paint in order, and perform ultrasonic treatment. The frequency of ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, the ultrasonic treatment time is 15 min, and the paint is left to stand for 15 min;
[0045] Then pour in the coupling agent and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 30kHz, the power is 80W, the ultrasonic temperature is room temperature, and the ultrasonic treatment time is 10 minutes. Then add the dispersant and perform ultrasonic treatment. Finally, let it stand for 10 minutes to obtain the paint mixture.
[0046] Example 6
[0047] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0048] (1) Weigh the raw materials by weight: 20 parts of paraffin oil, 75 parts of paint, 2 parts of coupling agent, and 3 parts of dispersant;
[0049] (2) Pour paraffin oil into the paint in order, and perform ultrasonic treatment. The frequency of ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, the ultrasonic treatment time is 15 min, and the paint is left to stand for 15 min;
[0050] Then pour in the coupling agent and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 30kHz, the power is 80W, the ultrasonic temperature is room temperature, and the ultrasonic treatment time is 10 minutes. Then add the dispersant and perform ultrasonic treatment. Finally, let it stand for 10 minutes to obtain the paint mixture.
[0051] Example 7
[0052] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0053] (1) Weigh the raw materials by weight: 10 parts of paraffin oil, 85 parts of paint, 2 parts of coupling agent, and 3 parts of dispersant;
[0054] (2) Pour paraffin oil into the paint in order, and perform ultrasonic treatment. The frequency of ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, the ultrasonic treatment time is 15 min, and the paint is left to stand for 15 min;
[0055] Then pour in the coupling agent and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 30kHz, the power is 80W, the ultrasonic temperature is room temperature, and the ultrasonic treatment time is 10 minutes. Then add the dispersant, perform ultrasonic treatment, and finally let it stand for 10 minutes.
[0056] Example 8
[0057] A method for applying paraffin oil to flame retardant paint comprises the following steps:
[0058] (1) Weigh the raw materials by weight: 10 parts of paraffin oil, 85 parts of paint, 2 parts of coupling agent, and 3 parts of dispersant;
[0059] (2) Pour paraffin oil into the paint in order, and perform ultrasonic treatment. The frequency of ultrasonic treatment is 40 kHz, the power is 100 W, the ultrasonic temperature is room temperature, the ultrasonic treatment time is 15 min, and the paint is left to stand for 15 min;
[0060] Then pour in the coupling agent and perform ultrasonic treatment. The frequency of the ultrasonic treatment is 30kHz, the power is 80W, the ultrasonic temperature is room temperature, and the ultrasonic treatment time is 10 minutes. Then add the dispersant, perform ultrasonic treatment, and finally let it stand for 10 minutes.
[0061] In Comparative Example 1, the paint used in Examples 1-6 was directly used.
[0062] Test experiment 1: The paint mixtures prepared in Examples 1, 2, 5, and 6 were placed in transparent containers, respectively, and placed in a freezer. The freezer was adjusted to a freezing temperature of minus 30°C to minus 40°C, and the mixtures were taken out after being frozen for 12 hours. It was observed that the paint mixtures in each container had good fluidity and would not freeze even if they were viscous, indicating that the paint mixtures prepared by the method of the present invention had a good antifreeze effect.
[0063] Test experiment 2: flame retardancy test of the paint mixture prepared in Example 2 and the paint of Comparative Example 1. In a closed laboratory, two 200 ml beakers A and B were taken, 50 ml of the paint of Comparative Example 1 was poured into A, and 50 ml of the paint prepared in Example 4 was poured into B, and they were placed on a lit alcohol lamp for slow fire roasting and carefully observed under a microscope.
[0064] Beaker B: After 2 minutes, it was found that there was a slow melting phenomenon during the heating process. The temperature gradually increased from 20 degrees to 40 degrees at a rate of 0.167 degrees per second, and about 0.1 grams of white odorless steam began to appear per second. After 3 minutes, the temperature was raised to 50 degrees, and water droplets of about 100 microns began to appear on the inner wall of the beaker. The temperature rise slowed down significantly. After 4 minutes, the temperature was raised to 55 degrees Celsius at a rate of 0.0833 per second. After 5 minutes, the water droplets became larger than 500 microns and began to flow. At this time, the steam reached about 0.01g / second. The temperature dropped to 50 degrees Celsius. After 6 minutes, the temperature was raised to 55 degrees Celsius and 60 degrees Celsius at a rate of 0.167 degrees per second. At this time, the mixture was reduced at a rate of 2ml per second, 3ml per second, and 5ml per second. After 7 minutes, the paint mixture prepared in Example 4 disappeared with the steam, and the paint residue left in the beaker was completely unburned.
[0065] Beaker A: Place a beaker with 50ml of paint on a burning alcohol lamp. There is no change in 10 seconds. After 15 seconds, the temperature in the beaker rises from 20℃ to 30℃, and there are obvious signs of hot melting, accompanied by a pungent odor of aromatic solvents. After 20 seconds, about 0.1 grams of gray smoke appears in the beaker per second, which quickly turns into black smoke after 22 seconds. After 25 seconds, the temperature has risen to 50℃, and the black smoke has reached 0.5 grams per second. At 40 seconds, the temperature has reached 60℃. With thick smoke billowing from the beaker mouth, various data can no longer be seen clearly. The beaker has exploded with a sound of 30 decibels, and paint is scattered all over the floor and burning. The laboratory is filled with the pungent smell of solvents.
[0066] It can be seen from this that the paint prepared by the method of the present invention can decompose temperature and accumulate conductive heat by itself, thereby reducing the temperature of the material surface, and is a rare and efficient flame retardant paint.
[0067] According to existing indicators, the paint mixtures prepared in the above Examples 1-8 were tested for physical properties and flame retardancy. The data comparison is shown in Table 1.
[0068] Table 1 Comparison of physical properties of the paint mixtures prepared in Examples 1-8 and Comparative Example 1
[0069]
[0070] As shown in Table 1, the paint mixture prepared by the present invention has a higher limiting oxygen index than the paint in Comparative Example 1, and has good flame retardant properties. It also has good bonding effect and quick drying time. After the configuration of the method of the present invention, the color and UV protection of the obtained paint mixture are better than those of Comparative Example 1, and the production cost is also reduced, which can be widely promoted.
[0071] Paraffin oil can be used in wire and cable products, waterproof coating (paint) products, plastic products (including plastic pipes), tire products, foam products, and plastic additives products. Adding 10-30% of it will help improve the flame retardancy of the mixture and the mechanical properties of the product, and reduce production costs.
[0072] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. Application of paraffin oil in flame retardant paint.
2. A method for applying paraffin oil in flame retardant paint, characterized in that: The steps include: (1) weighing raw materials by weight, wherein the raw materials include 10 to 30 parts of paraffin oil and 70 to 90 parts of paint; (2) Pour paraffin oil into the paint and stir well.
3. The method for applying paraffin oil in flame retardant paint according to claim 2, characterized in that: The kinematic viscosity of the paraffin oil at 40°C is 8 to 30 mm 2 / s.
4. The method for applying paraffin oil in flame retardant paint according to claim 2, characterized in that: The raw materials also include a coupling agent, and the weight portion of the coupling agent is 1 to 3 parts.
5. The method for applying paraffin oil in flame retardant paint according to claim 4, characterized in that: The coupling agent is an organic silane coupling agent.
6. The method for applying paraffin oil in flame retardant paint according to claim 5, characterized in that: The raw materials also include a dispersant, the weight portion of which is 2 to 5 parts.
7. The method for applying paraffin oil in flame retardant paint according to claim 6, characterized in that: The dispersant is a mixture of one or more of polyoxyethylene alkylphenol ether, fatty amine polyoxyethylene ether or oleyl alcohol polyoxyethylene ether.
8. The method for applying paraffin oil in flame retardant paint according to claim 7, characterized in that: First add the coupling agent, stir mechanically to make it uniform, then add the dispersant, stir mechanically to make it uniform; Alternatively, the paint mixture can be made uniform by ultrasonic treatment, that is, ultrasonic treatment is performed at room temperature with a frequency of 20 to 40 kHz and a power of 60 to 90 W, and finally allowed to stand for 5 to 10 minutes.
9. The method for applying paraffin oil in flame retardant paint according to claim 2, characterized in that: After adding paraffin oil, the method of stirring evenly is ultrasonic treatment, that is, the frequency of ultrasonic treatment at room temperature is 30-50kHz, the power is 80-100W, and the time of ultrasonic treatment is 15-30min; after fully mixing, it is then left to stand for 10-20min.
Citation Information
Patent Citations
Flame-retardant and smoke-inhibition type non-cured rubber asphalt waterproof coating material
CN105238270A
Burnthrough-resistant water-based fire retardant glue for spinning
CN106366723A
Ultrathin flame-retardant can-making water-based paint and preparation method thereof
CN113999583A
Incombustible coating material for styrofoam, method for preparing the same, and flameproof process using the same
KR1020080086293A