Finishing finish paint and preparation method thereof

The photoinitiator promotes the cross-linking of the modified acrylic resin and the monomer to form a three-dimensional network structure, which solves the problems of low hardness and poor anti-slip performance of the varnish, achieves high mechanical strength and good anti-slip effect, and ensures Coating smoothness and adhesion.

CN118813104AActive Publication Date: 2024-10-22ZHEJIANG DARUI PAINT TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411085708.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-22
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing topcoat has problems such as low hardness and poor anti-skid performance.

Method used

The photoinitiator is used to cross-link the modified acrylic resin and the monomer to form a stable three-dimensional network structure. By limiting the proportion and type of components, the mechanical strength and anti-slip properties of the coating are improved.

Benefits of technology

It achieves good anti-slip effect and physical strength of the coating film, avoids the formation of uneven layer structure after curing, and improves the smoothness and adhesion of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985124360000041
    Figure BDA0004985124360000041
  • Figure BDA0004985124360000051
    Figure BDA0004985124360000051
Patent Text Reader

Abstract

The invention relates to finishing paint and a preparation method thereof, and relates to the technical field of paint. The invention discloses finishing paint which is prepared from the following raw materials in parts by mass: 3-5 parts of a photoinitiator, 0.5-1.5 parts of an auxiliary agent, 20-35 parts of acrylic resin, 15-35 parts of a monomer and 45-65 parts of a solvent, the preparation method of the finishing paint comprises the following step: mixing the photoinitiator, the assistant, the acrylic resin, the monomer and the solvent to obtain the finishing paint. The modified acrylic resin and the monomer are crosslinked and interspersed through the photoinitiator to form a stable three-dimensional network structure, the mechanical strength of a film formed by the coating is improved, and it is guaranteed that the coating has a good anti-skid effect after being formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coating technology, and in particular to a finishing paint and a preparation method thereof. Background Art

[0002] Finishing paint is commonly known as varnish and is frequently used in model making. It is usually used for civilian models to improve the brightness of the finished product. Finishing paint can be mainly divided into automotive finishing paint, exterior wall transparent finishing paint, metal finishing paint, high hardness glass finishing paint, etc. An ideal finishing paint should have the properties of transparency, non-yellowing, UV resistance, wear resistance, chemical corrosion resistance, high gloss and high light retention, and can be used for various wear surfaces for decoration and protection. However, the existing finishing paint itself, as a commonly used topcoat with a fast curing rate, high surface hardness and large shrinkage rate, has the problems of low hardness and poor anti-slip performance. Summary of the invention

[0003] In order to solve the problem of low hardness and poor anti-slip performance of the topcoat in the prior art, the present application provides a topcoat and a preparation method thereof.

[0004] In a first aspect, the present application provides a finishing paint.

[0005] A finishing paint comprises raw materials including 3-5 parts of a photoinitiator, 0.5-1.5 parts of an auxiliary agent, 20-35 parts of an acrylic resin, 15-35 parts of a monomer and 45-65 parts of a solvent, calculated by weight.

[0006] The present application uses a photoinitiator to cause cross-linking and interlacing between the modified acrylic resin and the monomer to form a stable three-dimensional network structure, thereby improving the mechanical strength of the coating film and ensuring that the coating has a good anti-slip effect after forming.

[0007] Preferably, the raw materials for preparation include 4 parts of photoinitiator, 1 part of auxiliary agent, 28 parts of acrylic resin, 22 parts of monomer and 55 parts of solvent, calculated by mass.

[0008] The present application further defines the component ratio of the finishing paint, so that the finishing paint can have good physical strength and anti-slip performance.

[0009] Preferably, the photoinitiator is 184-photoinitiator.

[0010] The present application limits the types of the photoinitiators, thereby ensuring that the raw materials form a better connection structure during the photocuring process.

[0011] Preferably, the additives include BYK-333 additive and a leveling agent.

[0012] The present application defines that the additives include BYK-333 additive and leveling agent, which can ensure that the topcoat has good fluidity and can avoid forming an uneven layer structure after curing.

[0013] Preferably, the resin includes modified acrylic resin and nonafunctional aliphatic resin.

[0014] The present application can ensure that the topcoat has good physical properties by limiting the type of the resin.

[0015] Preferably, the monomers include dipentaerythritol hexaacrylate, pentaerythritol triacrylate and tripropylene glycol diacrylate.

[0016] The present application limits the types of the monomers so that they can cooperate with the photoinitiator to form a better connection structure during the photocuring process.

[0017] Preferably, the solvent includes propylene glycol methyl ether acetate, acetic acid, n-butyl acetate and propylene glycol methyl ether.

[0018] The present application can ensure that the prepared topcoat has a good solid-to-liquid ratio by limiting the type of the solvent.

[0019] In a second aspect, the present application provides a method for preparing the aforementioned topcoat.

[0020] A method for preparing a finishing paint comprises the following steps: mixing a photoinitiator, an auxiliary agent, an acrylic resin, a monomer and a solvent to obtain the finishing paint.

[0021] The present application combines various raw materials by mixing, and the paint can be formed without heating.

[0022] Preferably, the mixing is carried out under stirring conditions, the stirring speed is 600-800 r / min, and the stirring time is 20-40 min.

[0023] The present application can ensure that the components of the topcoat are fully and evenly mixed by limiting the mixing conditions.

[0024] In summary, this application has the following beneficial effects: 1. The present application uses a photoinitiator to cause cross-linking and interlacing between the modified acrylic resin and the monomer to form a stable three-dimensional network structure, thereby improving the mechanical strength of the coating film and ensuring that the coating has a good anti-slip effect after forming.

[0025] 2. By limiting the content of each component, the present application can ensure that the coating has a good solid-liquid ratio, avoid the appearance of protruding layer structures during subsequent use, and ensure the smoothness of the coating. DETAILED DESCRIPTION

[0026] The present application is further described in detail below with reference to the embodiments.

[0027] Example 1 A method for preparing a finishing paint comprises the following steps: 3 parts of 184-photoinitiator, 0.2 parts of BYK-333 auxiliary agent, 0.3 parts of leveling agent, 10 parts of modified acrylic resin, 10 parts of nonagent aliphatic acrylic resin, 5 parts of dipentaerythritol hexaacrylate, 5 parts of pentaerythritol triacrylate, 5 parts of tripropylene glycol diacrylate and 45 parts of propylene glycol methyl ether acetate are mixed in a container, and stirred at 700r / min for 30min to obtain a topcoat; the leveling agent is acrylate-modified polysiloxane with the brand name: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd. with the brand name: 10230; the nonagent aliphatic acrylic resin is purchased from Changzhou Houding Chemical Co., Ltd. with the brand name: HD-1209.

[0028] Example 2 5 parts of 184-photoinitiator, 0.7 parts of BYK-333 auxiliary agent, 0.8 parts of leveling agent, 17 parts of modified acrylic resin, 18 parts of nonagent aliphatic acrylic resin, 12 parts of dipentaerythritol hexaacrylate, 12 parts of pentaerythritol triacrylate, 11 parts of tripropylene glycol diacrylate and 65 parts of propylene glycol methyl ether acetate are mixed in a container, and stirred at 700 r / min for 30 minutes to obtain a topcoat; the leveling agent is acrylate-modified polysiloxane with the brand name: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd. with the brand name: 10230; the nonagent aliphatic acrylic resin is purchased from Changzhou Houding Chemical Co., Ltd. with the brand name: HD-1209.

[0029] Example 3 4 parts of 184-photoinitiator, 0.5 parts of BYK-333 auxiliary agent, 0.5 parts of leveling agent, 14 parts of modified acrylic resin, 14 parts of nonagent aliphatic acrylic resin, 7 parts of dipentaerythritol hexaacrylate, 8 parts of pentaerythritol triacrylate, 8 parts of tripropylene glycol diacrylate and 55 parts of propylene glycol methyl ether acetate are mixed in a container, and stirred at 600r / min for 20min to obtain a topcoat; the leveling agent is acrylate-modified polysiloxane with the brand name: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd. with the brand name: 10230; the nonagent aliphatic acrylic resin is purchased from Changzhou Houding Chemical Co., Ltd. with the brand name: HD-1209.

[0030] Example 4 3.5 parts of 184-photoinitiator, 0.2 parts of BYK-333 auxiliary agent, 0.8 parts of leveling agent, 10 parts of modified acrylic resin, 18 parts of nonagent aliphatic acrylic resin, 5 parts of dipentaerythritol hexaacrylate, 5 parts of pentaerythritol triacrylate, 10 parts of tripropylene glycol diacrylate and 55 parts of propylene glycol methyl ether acetate are mixed in a container, and stirred at 800 r / min for 40 minutes to obtain a topcoat; the leveling agent is acrylate-modified polysiloxane with the brand name: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd. with the brand name: 10230; the nonagent aliphatic acrylic resin is purchased from Changzhou Houding Chemical Co., Ltd. with the brand name: HD-1209.

[0031] Example 5 4.5 parts of 184-photoinitiator, 0.5 parts of BYK-333 auxiliary agent, 0.7 parts of leveling agent, 15 parts of modified acrylic resin, 13 parts of nonagent aliphatic acrylic resin, 10 parts of dipentaerythritol hexaacrylate, 5 parts of pentaerythritol triacrylate, 5 parts of tripropylene glycol diacrylate and 65 parts of propylene glycol methyl ether acetate are mixed in a container, and stirred at 700 r / min for 30 minutes to obtain a topcoat; the leveling agent is acrylate-modified polysiloxane with the brand name: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd. with the brand name: 10230; the nonagent aliphatic acrylic resin is purchased from Changzhou Houding Chemical Co., Ltd. with the brand name: HD-1209.

[0032] Comparative Example 1 3.9 parts of photoinitiator, 0.1 parts of leveling agent, 34 parts of modified acrylate, 5 parts of ethyl ester, 5 parts of butyl ester and 40 parts of monomer are mixed in a container, and stirred at 700r / min for 30 minutes to obtain a topcoat; wherein the photoinitiator is 2-hydroxy-2methyl-1-phenyl-1-propanone, purchased from Tianjin Jiuri Chemical Co., Ltd., item number: 1173; the leveling agent is acrylate-modified polysiloxane, brand: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd., brand number 10230; the monomer is trimethylolpropane triacrylate, purchased from Sanmu Group, brand number TMPTA.

[0033] Comparative Example 2 3.9 parts of photoinitiator, 0.1 parts of leveling agent, 15 parts of modified acrylate, 5 parts of ethyl ester, 5 parts of butyl ester and 10 parts of monomer are mixed in a container, and stirred at 700r / min for 30 minutes to obtain a topcoat; wherein the photoinitiator is 2-hydroxy-2methyl-1-phenyl-1-propanone, purchased from Tianjin Jiuri Chemical Co., Ltd., item number: 1173; the leveling agent is acrylate-modified polysiloxane, brand: Digao 2100; the modified acrylate is purchased from Foshan Gaoming Tongde Chemical Co., Ltd., brand number 10230; the monomer is trimethylolpropane triacrylate, purchased from Sanmu Group, brand number TMPTA.

[0034] Performance Testing Performance test 1: Viscosity test: refer to the test standard of GB / T1723-93, at 25°C, take the coatings prepared in Examples 1 to 5, prepare a 4# viscosity cup, block the cup mouth with your left hand, and fill the viscosity cup with the coating with your right hand, then release the left and right hands and use a stopwatch to time, and stop the stopwatch when the coating has flowed out of the cup. The seconds displayed on the stopwatch are the paint viscosity.

[0035] Performance Test 2: Adhesion test method: Spray the topcoat prepared in Example 1 to Example 5 on 7 groups of ABS plastic plates respectively, bake in a 60°C oven for 1 minute, place under a 400-800mj / cm2 ultraviolet lamp for curing for 5 seconds, vacuum electroplate aluminum on the plates, and then apply the topcoat on the electroplated aluminum film. Use a knife to scratch the paint film on the prepared ABS plastic plate, use 3M tape to pull the paint film three times, observe the paint film falling off at the paint film, and divide the adhesion level according to the test standard of GB / T1720-1979.

[0036] Performance Test 3: Coating property test: Spray the topcoat prepared in Examples 1-5 and Comparative Examples 1-2 on 7 groups of ABS plastic plates respectively, bake in a 60°C oven for 1 min, cure under a 400-800mj / cm2 ultraviolet lamp for 5 seconds, then vacuum electroplate aluminum on the plates, spray the topcoat on the electroplated aluminum film, and then boil in 100°C water for 2 hours. Then check whether there are cracks on the coating layer and the ABS plastic plate layer. If there are cracks, the coating property is recorded as poor, and if there are no cracks, the coating property is recorded as good.

[0037] Performance Test 4: According to GB / T 6739-2006, Examples 1-5 and Comparative Examples 1-2 were sprayed on the surfaces of 7 groups of polished tinplate sheets, respectively, and cured at 180° C. for 10 min. Then, the hardness of the coating was tested using a surface hardness tester.

[0038] Table 1 Test results In combination with Examples 1-5, Comparative Examples 1-2 and Table 1, it can be seen that the coating provided in the present application has good viscosity and adhesion, and has good cross-linking performance. At the same time, the coating provided in the present application has a high hardness. Taking all factors into consideration, Example 3 of the present application has the best performance.

[0039] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A finishing paint, It is characterized in that The raw materials include the following by weight: 3-5 parts of photoinitiator, 0.5-1.5 parts of auxiliary agent, 20-35 parts of acrylic resin, 15-35 parts of monomer and 45-65 parts of solvent.

2. The finishing paint according to claim 1, It is characterized in that The following raw materials are included in parts by mass: 4 parts of photoinitiator, 1 part of auxiliary agent, 28 parts of acrylic resin, 22 parts of monomer and 55 parts of solvent.

3. The finishing paint according to claim 1 or 2, It is characterized in that The photoinitiator is 184-photoinitiator.

4. The finishing paint according to claim 1 or 2, It is characterized in that The additives include BYK-333 additive and a leveling agent.

5. The finishing paint according to claim 1 or 2, It is characterized in that The resin includes modified acrylic resin and nonafunctional aliphatic acrylic resin.

6. The finishing paint according to claim 1 or 2, It is characterized in that The monomers include dipentaerythritol hexaacrylate, pentaerythritol triacrylate and tripropylene glycol diacrylate.

7. The finishing paint according to claim 1 or 2, It is characterized in that The solvent includes propylene glycol methyl ether acetate, acetic acid, n-butyl acetate and propylene glycol methyl ether.

8. A method for preparing a finishing paint according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The photoinitiator, the auxiliary agent, the acrylic resin, the monomer and the solvent are mixed to obtain the finishing paint.

9. The preparation method according to claim 7, It is characterized in that The mixing is carried out under stirring conditions, the stirring speed is 600-800r / min, and the stirring time is 20-40min.

Citation Information

Patent Citations

  • Top coat for vacuum coating and method of forming coating on vacuum coating layer surface

    CN103374245A

  • High-performance vacuum plating UV coating finish paint and preparation method thereof

    CN108977046A

  • Finishing varnish and preparation method thereof

    CN111892862A

  • Acrylic acid modified UV (ultraviolet) finishing coating easy to recoat and preparation method of acrylic acid modified UV finishing coating

    CN115572527A