Self-adhesive tape with MOPP carrier
By optimizing the composition of the pressure-sensitive adhesive, the problem of residues during separation of the uniaxially oriented polypropylene film self-adhesive tape is solved, achieving better re-separability and applicability, and ensuring no residue at different temperatures and substrates. separation.
Patent Information
- Application Number
- CN202410474456.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-22
AI Technical Summary
Existing self-adhesive tapes easily cause the carrier film to crack and leave residue when separated, and are difficult to separate without residue after storage at different temperatures, especially when using uniaxially oriented polypropylene film (MOPP) as the carrier. , insufficient internal strength causes the adhesive tape to split in the z direction, affecting its re-detachability.
By adjusting the composition of the pressure-sensitive adhesive, using 38-65% elastomer component, 8-45% tackifier resin component and 3-22% reinforcing component, combined with polydiene block copolymer and hydrocarbon Resin and other materials, optimize the formula of pressure-sensitive adhesive to improve the re-detachability of self-adhesive tapes.
Significantly improves the re-separability of self-adhesive tapes, ensuring residue-free separation at different temperatures and substrates, improving its reliability and applicability during transportation and storage.
Smart Images

Figure BDA0004800023920000141
Abstract
Description
Technical Field
[0001] The invention relates to a self-adhesive tape, a method for producing the self-adhesive tape and its use. The self-adhesive tape comprises a carrier consisting of a uniaxially oriented polypropylene film (MOPP) and a pressure-sensitive adhesive suitable for the carrier. Background Art
[0002] Self-adhesive tapes are used in particular for fixing movable parts during transport, for example in refrigerators, and for bundling objects such as pipes, profiles or stacked cartons. The common feature of these applications is that during transport, the movable parts are firmly fixed by the tape, but the tape must be able to be removed again after transport in a manner without any residue. In addition to sufficient peel adhesion, the removability (peelability, detachability) without residue from various substrates remains a special challenge. Common substrates from which the tape must be able to be separated in a manner without residue and damage even after long-term storage at different temperatures are plastics such as PS, PP and PE, various metals, and solventborne and water-based (water-containing), solvent-free or powder-applied coatings. The common product structure of such self-adhesive tapes usually comprises a carrier and a pressure-sensitive adhesive, wherein for economic reasons, a uniaxially oriented polypropylene film (MOPP) is usually used as a carrier. However, such films have the disadvantage of low internal strength, which can lead to film splitting in the z direction when the tape is separated, which in turn leaves unwanted residues on the adhesive substrate. In the prior art, many attempts have been made to overcome these disadvantages and optimize the carrier material.
[0003] WO 2014 / 029664 discloses an adhesive tape having a carrier consisting of a film to which an adhesive is applied at least on one side, the film being a uniaxially oriented polypropylene film comprising at least 80% by weight of polypropylene, the polypropylene having previously been processed at least once, preferably extruded at least once, wherein the film has a stretch ratio of 1:4 to 1:10 in the orientation in the longitudinal direction.
[0004] DE102017203066 describes an adhesive tape having a carrier consisting of a film to which an adhesive is applied at least on one side, the film being a uniaxially oriented film consisting of at least 95 wt.-% of a polypropylene composition having different phases, comprising: (i) 80 to 99 wt.-% of a polypropylene matrix comprising a propylene homopolymer, and (ii) 1 to 20 wt.-% of an elastomer in the form of an ethylene-propylene copolymer having an ethylene content of 50 to 90 wt.-%.
[0005] DE 10 2020 214 722 provides an adhesive tape having a carrier consisting of a film to which an adhesive is applied on at least one side, the film being a film uniaxially oriented in the longitudinal direction and comprising at least 90% by weight of a polyester polymer.
[0006] MOPP films are valued for their high tensile strength in the machine direction. From an economic point of view, it is not always advantageous to implement a specific carrier system, especially for smaller batch sizes. Therefore, there is still a need for improved self-adhesive tapes with a MOPP film carrier. Summary of the invention
[0007] Against this background, the object of the present invention is to provide a self-adhesive tape with a MOPP carrier which overcomes the disadvantages of the prior art and is distinguished above all by improved redetachability. This object is achieved by a self-adhesive tape according to the concept of the invention (independent claim). Preferred developments of the self-adhesive tape of the invention are listed in the description (dependent claims).
[0008] Surprisingly, it has been found that conventional MOPP film carriers can be used advantageously if they are combined with a suitably adjusted pressure-sensitive adhesive. In this way, self-adhesive tapes can be achieved which exhibit improved re-detachability compared to conventional self-adhesive tapes.
[0009] A first subject of the present invention is therefore a self-adhesive tape comprising a carrier consisting of a uniaxially oriented polypropylene film and a pressure-sensitive adhesive comprising:
[0010] a) 38 to 65 wt. % of an elastomeric component;
[0011] b) 8 to 45 weight percent of a tackifier resin component; and
[0012] c) 3 to 22% by weight of a reinforcing component,
[0013] The weight data here relate in each case to the total weight of the pressure-sensitive adhesive, and the sum of the fractions (proportions) of elastomeric component and reinforcing component in the pressure-sensitive adhesive is at least 52% by weight, based on the total weight of the pressure-sensitive adhesive. DETAILED DESCRIPTION
[0014] i) Carrier
[0015] As the carrier of the self-adhesive tape of the present invention, common MOPP films can be used because they are commercially available. MOPP is produced by extrusion and subsequent stretching of polypropylene. The film can be composed of pure polypropylene, that is, only composed of propylene monomers. Polypropylene random copolymers or polypropylene block copolymers are also suitable. Suitable comonomers include olefins, especially ethylene and / or butene, wherein the fraction of the comonomer in polypropylene is preferably less than 50% by weight, particularly preferably less than 30% by weight, more particularly less than 20% by weight, in each case based on the total weight of the film. According to the present invention, it is also possible to use a film composed of a blend of polypropylene and at least one other polymer, wherein the fraction of the other polymer is preferably less than 15% by weight, particularly preferably less than 10% by weight, more particularly less than 5% by weight, in each case based on the total weight of the film. Polyethylene can be used in particular as a further polymer.
[0016] In the context of the present invention, a MOPP film comprising or consisting of recycled polypropylene may also be used as a carrier. Recycled polypropylene is preferably a polypropylene that has been pre-processed at least once, preferably extruded at least once. Suitable materials are, for example, edge trimmings obtained during the production of polypropylene films. Further suitable carrier films are described, for example, in WO2018 / 154106 and WO2014 / 029664.
[0017] The thickness of the carrier film can be adjusted as desired, but after orientation, it is preferably in the range of 20 to 150 μm, particularly preferably in the range of 25 to 100 μm, more particularly in the range of 50 to 100 μm.
[0018] For the production of the carrier film, it may be appropriate to add additives and further components which improve the film-forming properties, influence the tendency to form crystalline segments and / or selectively improve or, where appropriate, impair the mechanical properties. The carrier film may contain pigments or other colorants and may thus be colored, white, gray or black. It may also contain additives, such as, in particular, stabilizers and / or fillers.
[0019] ii) Pressure sensitive adhesive
[0020] Surprisingly, it has been found that the use of the pressure-sensitive adhesive provided according to the invention makes it possible to particularly improve the re-detachability of the self-adhesive tapes according to the invention.
[0021] a) Elastomer component
[0022] In the prior art, synthetic rubber and natural rubber are used in particular as pressure-sensitive adhesives for bonding to MOPP films. In the context of the present invention, it has proven to be advantageous to use polydiene block copolymers. In a preferred embodiment, the pressure-sensitive adhesive therefore comprises at least one polydiene block copolymer, more particularly a polyvinyl aromatic compound (aromatic)-polydiene block copolymer. However, polydiene block copolymers can also be used, in which the polydiene blocks are hydrogenated.
[0023] Preferably, the fraction of the polydiene block copolymer in the elastomeric component is at least 90% by weight, based on the total weight of the elastomeric component.Preferred are polydienes derived from conjugated dienes, in particular from 1,3-dienes.
[0024] In a preferred embodiment, the elastomer component is a composition having ABA, (AB) n , (AB) n X or (ABA) n A polyvinyl aromatic compound-polydiene block copolymer of the structure X, wherein
[0025] The blocks A are independently of one another polymers formed by polymerization of at least one vinyl aromatic compound;
[0026] The blocks B are independently of one another polymers formed by polymerization of one or more conjugated dienes having 4 to 18 C atoms;
[0027] X is a group (residue) of a coupling reagent or a multifunctional initiator; and
[0028] n is an integer ≥2.
[0029] The polyvinyl aromatic compound-polydiene block copolymers preferably each comprise one or more rubbery blocks B (elastomeric blocks, soft blocks) and at least two glassy blocks A (hard blocks). In the embodiments described here, it is particularly preferred that at least one polyvinyl aromatic compound-polydiene block copolymer has an ABA, (AB)2X, (AB)3X or (AB)4X structure, wherein A, B and X meet the above definitions. Preferably, the elastomeric component comprises at least one triblock copolymer or a higher multiblock copolymer, which may be linear or multi-armed, for example radial or star-shaped.
[0030] Based on the total of all polyvinyl aromatic compounds-polydiene block copolymers of the elastomer component, preferably a polyvinyl aromatic compound-polydiene block copolymer with a peak molar mass of at least 90000 g / mol, more preferably at least 120000 g / mol. Preferably, the peak molar mass of the polyvinyl aromatic compound-polydiene block copolymer used does not exceed 250000 g / mol. Such polyvinyl aromatic compound-polydiene block copolymer is preferably present in at least 30% by weight, preferably at least 40% by weight, more preferably at least 50% by weight, and very preferably at least 60% by weight, and preferably at most 90% by weight, based on the total weight of the elastomer component. The peak molar mass can be determined by GPC (Test 1a) according to the method described in the "Test Methods" section.
[0031] The elastomeric component may also contain one or more diblock copolymers AB. However, a too high fraction of diblock copolymers is usually detrimental to the thermal shear strength. Therefore, their fraction in the pressure-sensitive adhesive should not be too high. Particularly preferably, the average diblock fraction of the polyvinyl aromatic compound-polydiene block copolymer based on all of the polyvinyl aromatic compound-polydiene block copolymers of the elastomeric component is no more than 40 wt %, particularly no more than 30 wt % and very particularly preferably no more than 25 wt %. In particular, the pressure-sensitive adhesive of the self-adhesive tape of the present invention includes a mixture of polyvinyl aromatic compound-polydiene block copolymers with AB, ABA, (AB) 3X or (AB) 4X structures, which particularly preferably includes radial block copolymers and / or triblock copolymers ABA. Also preferred are triblock copolymers and (AB) wherein n is equal to or greater than 3. n or (AB) n Mixtures of X block copolymers. The block copolymers resulting from the A and B blocks may in principle contain identical or different B blocks. The block copolymers may have a linear ABA structure, may have a radial shape, and may include star-shaped and linear multiblock copolymers.
[0032] The vinyl aromatic compounds used for the structure (construction) of block A preferably include styrene and styrene derivatives, particularly preferably styrene and α-methylstyrene. Block A can be a homopolymer or a copolymer. Particularly preferably, block A is a polystyrene block. Instead of the preferred polystyrene blocks, it is also possible to use as vinyl aromatic compounds polymer blocks based on homopolymers and copolymers containing other aromatic compounds, preferably C8 to C12 aromatic compounds, especially with a glass transition temperature of more than 75° C., for example aromatic blocks containing α-methylstyrene. For example, the glass transition temperature can be determined by DSC (test II).
[0033] The polyvinyl aromatic compound-polydiene block copolymer used according to the invention may contain identical or different A blocks. Preferably, the polyvinyl aromatic compound-polydiene block copolymer has polystyrene end blocks. The monomers for the soft block B are preferably conjugated dienes, in particular those selected from the following: butadiene, isoprene, ethylbutadiene, phenylbutadiene, piperylene, pentadiene, hexadiene, ethylhexadiene, farnesene and dimethylbutadiene, and any mixture of these monomers. Block B can also be in the form of a homopolymer or a copolymer. Particularly preferably, the monomers for the soft block B are selected from butadiene and isoprene. For example, the soft block B is a polymer block of a polyisoprene block or a polybutadiene block or a mixture of butadiene and isoprene. Very particularly preferably, block B is polyisoprene. The soft blocks B prepared from these preferred and other diene monomers may also be hydrogenated and accordingly be present in particular as poly(ethylene-co-butene) or poly(ethylene-co-propylene) blocks.
[0034] The A blocks of the polyvinylaromatic-polydiene block copolymers preferably have a glass transition temperature of at least 25° C., in particular at least 50° C. For the B blocks, preference is given to a glass transition temperature of not more than 0° C., in particular not more than −25° C. These data relate to the pure, unblended block copolymers and were determined according to the invention by DSC (test II).
[0035] The fraction of A blocks in the polyvinyl aromatic compound-polydiene block copolymer is preferably at least 12% by weight and not more than 40% by weight, more preferably at least 15% by weight and preferably not more than 20% by weight. Preferably, the total fraction of all polyvinyl aromatic compounds-polydiene block copolymers is at least 38% by weight and not more than 65% by weight, more preferably at least 42% by weight and not more than 60% by weight, based on the total elastomer component. It has been found that too small a fraction of polyvinyl aromatic compound-polydiene block copolymer leads to a decrease in the hot shear strength of the pressure-sensitive adhesive, while too high a fraction of polyvinyl aromatic compound-polydiene block copolymer leads to a loss of too much adhesiveness of the pressure-sensitive adhesive, making the self-adhesive tape no longer suitable for certain applications.
[0036] The block copolymers derived from the A and B blocks may include the same or different B blocks, including in terms of microstructure. "Microstructure" refers to the relative proportions of the possible monomer linkage types (i.e., 1,4-cis (in polybutadiene and polyisoprene), 1,4-trans (in polybutadiene and polyisoprene), 1,2 (in polybutadiene and polyisoprene), and 3,4 (in polyisoprene)) for polybutadiene, polyisoprene, or another conjugated diene, particularly 1,3-dienes. It can be determined by 1H-NMR compares the integral of the signal to be assigned to the corresponding group. Preferably, the fraction of 1,4 (cis + trans)>80% by weight, more preferably>85% by weight, in each case based on the polydiene block, and the fraction of 1,4-cis>40% by weight, based on the polydiene block; accordingly, the total fraction of 1,2-connected and / or any 3,4-connected monomers present, the so-called vinyl fraction, is preferably less than 20% by weight, more preferably not more than 17% by weight, especially up to 13% by weight. The high fraction of 1,4-cis connections of the monomer units in the polydiene block and especially 1,4-cis connections or the low fraction of vinyl groups lead to a lower glass transition temperature, so that good impact resistance can be achieved even in a cold environment. For this reason, polybutadiene is a preferred monomer for the B block. In an alternative embodiment, the quantitative figures of the types of monomer connections, such as the quantitative figures of the vinyl fraction in particular, do not involve weight %, but instead involve mole %.
[0037] The above figures for the molar mass of the block copolymers relate to the polymer modes to which the skilled person can attribute the block copolymer structures mentioned in the respective context. In this case, the figures for the molar mass are to be understood as the peak molar mass. GPC generally allows the determination of the molar masses of the individual polymer modes in a mixture of different block copolymers.
[0038] In a particularly preferred embodiment, the elastomer component is a styrene-butadiene-styrene block copolymer (SBS) or a styrene-isoprene-styrene block copolymer (SIS), in particular a SIS block copolymer. In addition, hydrogenated block copolymers such as styrene-(ethylene-to-butylene)-styrene block copolymer (SEBS) and styrene-(ethyl-to-propylene)-styrene block copolymer (SEPS) can be used.
[0039] b) Tackifier resin component
[0040] According to the present invention, the pressure-sensitive adhesive comprises a tackifier resin component in addition to the elastomer component. The tackifier resin component is particularly used to set the adhesion in a desired manner. According to the general understanding of those skilled in the art, "tackifier resin" is understood to refer to an oligomeric or polymeric resin that improves the adhesion (i.e., inherent adhesion) of the pressure-sensitive adhesive compared to an otherwise identical pressure-sensitive adhesive without any tackifier resin. Tackifier resins are specific compounds with low molar mass compared to elastomers, typically having a weight average molecular weight M of less than 5000 g / mol. w Typically, the tackifier resin component used in the context of the present invention has a weight average molecular weight of 400 to 5000 g / mol, preferably 500 to 2000 g / mol, determined by GPC (Test 1b).
[0041] In the context of the present invention, the tackifier resin component is not to be understood as a reinforcing component, ie the tackifier resin component is preferably substantially incompatible with the hard blocks of the polydiene block copolymer.
[0042] The tackifier resin component is particularly compatible with the elastomer component and in particular with the polydiene block. Hydrocarbon resins or polyterpene resins have proven to be suitable, in particular in the case where polyvinyl aromatic compound-polydiene block copolymers are used. Therefore, it is preferred to use a tackifier resin in which at least 75% by weight, based on the total weight of the tackifier resin component, is a hydrocarbon resin or a polyterpene resin or a mixture thereof.
[0043] Preferably, the tackifier resin component of the pressure-sensitive adhesive comprises at least 75% by weight, based on the tackifier resin component, of at least one tackifier resin having a DACP (diacetone alcohol cloud point, test IIIa) of at least -20°C, preferably at least 0°C, very preferably at least +20°C. In addition, the tackifier resin component preferably has a softening temperature (ring & ball, test IV) of at least +85°C, preferably at least +100°C and at most +140°C. Methods for determining DACP and softening temperature are given in the "Test Methods" section.
[0044] Preferably, the tackifier resin component is selected from non-polar hydrocarbon resins, preferably hydrogenated and non-hydrogenated polymers of dicyclopentadiene (DCPD); non-hydrogenated, partially, selectively or fully hydrogenated hydrocarbon resins based on C5 or C5 / C9 monomer streams, or partially, selectively or fully hydrogenated hydrocarbon resins based on C9 monomer streams. Other tackifier resins that can be used for the tackifier resin component are polyterpene resins based on α-pinene and / or β-pinene and / or δ-limonene, which can also be hydrogenated.
[0045] The above-mentioned tackifier resins can be used alone or in the form of a mixture. Hydrogenated hydrocarbon resins such as hydrogenated C5 resins, hydrogenated C9 resins and / or hydrogenated DCPD resins are preferably suitable for combination with the polyisoprene block copolymer.
[0046] However, oxygen-containing tackifier resins such as terpene-phenol resins or rosin-containing resins, in particular rosin esters, are also conceivable. Rosin resins and rosin ester resins may be hydrogenated or non-hydrogenated or disproportionated or otherwise stabilized.
[0047] The fraction of the tackifier resin component in the pressure-sensitive adhesive has a positive effect on the bond strength. Therefore, the fraction of the tackifier resin should not be too low. However, it has been shown that the fraction of the tackifier resin is too high to the thermal shear strength, and particularly has a negative impact on re-separability. Therefore, the fraction of the tackifier resin component used for the purpose of the present invention is at least 8 wt % and is no more than 45 wt %, preferably no more than 40 wt %, very preferably no more than 35 wt %, all based on the gross weight of the pressure-sensitive adhesive in each case. It is also very advantageous to be no more than 30 wt % or even no more than 20 wt % of the resin fraction.
[0048] C) Reinforcement Component
[0049] Without being bound to any particular theory, it is assumed that especially the presence of the reinforcing component in combination with the MOPP film as carrier provides for the improved re-detachability of the self-adhesive tapes according to the invention.
[0050] Within the scope of the present invention, the reinforcing component should not be understood as a tackifier resin component, ie the reinforcing component is preferably substantially incompatible with the soft block (ie the polydiene block).
[0051] In particular, so-called end-block reinforcing agents are used as reinforcing components according to the invention.
[0052] End block reinforcing agents are those materials that are substantially compatible with the hard blocks of the polydiene block copolymer.
[0053] According to the present invention, the reinforcing component is at least one resin.
[0054] If the hard block type is a polyvinyl aromatic block, the reinforcing component is preferably at least one resin based on at least one hydrocarbon compound, in particular an aromatic hydrocarbon compound, preferably obtained from a C8 and / or C9 stream and preferably selected from styrene, α-methylstyrene, p-methylstyrene, indene, methylindene and copolymers thereof. For the reinforcing component, oxygen-containing resins such as terpene-phenol resins, indene-coumarone resins or phenol-modified aromatic resins may also be selected.
[0055] The at least one resin of the reinforcing component has a weight average molecular weight M of at least 800 g / mol, preferably 1000 g / mol to 15000 g / mol, more preferably 2000 g / mol to 10000 g / mol, as determined by GPC (test 1b). w .
[0056] At least one resin of the reinforcing component has a mixed methylcyclohexane aniline cloud point (MMAP; test IIIb) of not more than 30° C., preferably not more than 20° C.
[0057] The softening point of the at least one resin of the reinforcing component is preferably at least 130° C., more preferably at least 140° C., particularly preferably at least 150° C., determined according to Test IV.
[0058] The fraction of the reinforcing component is at least 3% by weight and at most 22% by weight, preferably at least 8% by weight and at most 18% by weight, based on the total weight of the pressure-sensitive adhesive.
[0059] It has been found that the fraction of the elastomeric component and the fraction of the reinforcing component have a beneficial effect on the properties of the self-adhesive tape containing MOPP. In this case, it has been shown that if the pressure-sensitive adhesive is largely (mainly) composed of an elastomeric component and a reinforcing component, it is particularly advantageous in terms of re-separability. Therefore, the sum of the fractions of the elastomeric component and the reinforcing component in the pressure-sensitive adhesive is at least 52% by weight, based on the total weight of the pressure-sensitive adhesive. In addition, the following embodiment is preferred, in which the sum of the elastomeric component and the reinforcing component is at least 55% by weight, in particular at least 60% by weight, based on the total weight of the pressure-sensitive adhesive.
[0060] In the context of the present invention, the expressions “substantially incompatible” or “substantially incompatible” are understood in particular to mean that the ingredients or components mentioned are miscible with one another to an extent of at most 10% by weight, preferably at most 5% by weight.
[0061] In the context of the present invention, the expression “substantially compatible” is understood in particular to mean that the ingredients or components mentioned are miscible with one another to an extent of at least 90% by weight, preferably at least 95% by weight.
[0062] d) Additional components
[0063] The pressure-sensitive adhesive of the self-adhesive tape of the present invention may contain additional components in addition to the above-mentioned components. Particularly preferably, the pressure-sensitive adhesive further includes a plasticizer component.
[0064] The plasticizer component is used primarily for the final fine-tuning of the cohesion / adhesion (cohesion / adhesion) balance. Preferably, the plasticizer component comprises one or more plasticizer resins and / or one or more mineral oils having a softening temperature of less than 30° C., determined according to test IV. Plasticizer resins or plasticizer-resin mixtures are preferred, and very preferably plasticizer resins or plasticizer-resin mixtures having a melt viscosity (test V) of at least 20 Pa*s, preferably at least 50 Pa*s at 25° C. and 1 Hz. The plasticizer resin is very preferably a plasticizer resin based on hydrocarbons or polyterpenes.
[0065] The plasticizer component is preferably present in the pressure-sensitive adhesive in an amount of at least 3 and / or at most 25 % by weight, more preferably at least 8 % by weight and at most 18 % by weight, based on the gross weight of the pressure-sensitive adhesive. Surprisingly found that by using a plasticizer component, particularly a plasticizer resin, the re-separability of the self-adhesive tape can be further improved. On the other hand, the presence of mineral oil or a mineral oil mixture (which is also commonly used as a plasticizer) has been found to be disadvantageous for re-separability. Therefore, preferred following embodiment, wherein the fraction of the mineral oil and / or the mineral oil mixture in the pressure-sensitive adhesive is no more than 3 % by weight, more preferably no more than 1.5 % by weight.
[0066] Despite their negative effects, higher contents of mineral oils and / or mineral oil mixtures may be preferred. For those embodiments in which the fraction of mineral oil and / or mineral oil mixture relative to the total weight of the pressure-sensitive adhesive exceeds 3% by weight, a fraction of reinforcing component of preferably at least 10% by weight is selected, also relative to the total weight of the pressure-sensitive adhesive.
[0067] In order to adjust further properties, the pressure-sensitive adhesive may comprise further additives. Preferably, however, their fraction does not exceed 18% by weight, preferably not more than 10% by weight, of the pressure-sensitive adhesive.
[0068] These additives are mainly protective agents. These include primary and secondary (primary and secondary) types of aging inhibitors, light stabilizers and UV protectants, as well as flame retardants, in addition to fillers, dyes and pigments. The pressure-sensitive adhesive layer can be colored as required, or white, gray or black. Typically, this or other additional additives that can be used are:
[0069] primary antioxidants such as sterically hindered phenols, for example preferably in a fraction of 0.2 to 1% by weight, based on the total weight of the pressure-sensitive adhesive;
[0070] - secondary antioxidants such as phosphites or thioethers, for example preferably in a fraction of 0.2 to 1% by weight, based on the total weight of the pressure-sensitive adhesive;
[0071] process stabilizers such as C free radical scavengers, for example preferably in a fraction of 0.2 to 1% by weight, based on the total weight of the pressure-sensitive adhesive,
[0072] Light stabilizers such as UV absorbers or sterically hindered amines, for example preferably in a fraction of 0.2 to 1% by weight, based on the total weight of the pressure-sensitive adhesive;
[0073] Processing aids, preferably in a fraction of 0.2 to 1% by weight, based on the total weight of the pressure-sensitive adhesive;
[0074] Optionally further polymers, preferably further polymers having elastomeric properties; elastomers which can thus be used include, inter alia: those based on pure hydrocarbons, for example unsaturated polydienes such as naturally or synthetically produced polyisoprene or polybutadiene; chemically essentially saturated elastomers, for example saturated ethylene-propylene copolymers, olefin copolymers, polyisobutylene, butyl rubber, ethylene-propylene rubber; and chemically functionalized hydrocarbons, for example halogen-containing, acrylate-containing, allyl- or vinyl ether-containing polyolefins, preferably in a fraction of 0.2 to 10% by weight, based on the total weight of the pressure-sensitive adhesive.
[0075] The at least one pressure-sensitive adhesive layer typically has a layer thickness of about at least 10 μm and not more than 150 μm, more often at least 20 μm and not more than 100 μm. A layer thickness in the range of at least 25 μm and not more than 60 μm is particularly preferred.
[0076] Depending on the embodiment, the pressure-sensitive adhesive can be arranged on one side or on both sides relative to the carrier to give a single-sided or double-sided tape.
[0077] For the purposes of the present invention, the general expressions "adhesive tape" or "self-adhesive tape" include all flat structures, such as films or film portions (segments) extending in two dimensions, tapes, tape portions (segments) etc. with an extended length and a limited width, and finally also die-cut parts or labels.
[0078] The adhesive tape can be produced in roll form, ie wound on itself in the form of an Archimedean spiral, or covered on its adhesive side with a release material, such as siliconized paper or siliconized film.
[0079] Suitable release materials are preferably lint-free materials, such as plastic film or thoroughly sized long-fiber paper.
[0080] The adhesive tapes have in particular a running length of 25 to 100 m in the form of customary adhesive tape rolls and a running length of 1000 to 30000 m in the form of reels.
[0081] In order to advantageously affect the unfolding properties of the adhesive tape wound into an Archimedean spiral, the reverse side varnish can be applied to the back side of the adhesive tape. For this reason, the reverse side varnish can be provided with (be provided with) silicone or fluorosilicone compound, or be provided with polyvinyl stearyl carbamate, polyethyleneimine stearyl urea or organic fluorine compound as anti-adhesive (anti-adhesive) material. Suitable stripping agent includes a surfactant stripping system based on a long-chain alkyl group, such as stearyl sulfosuccinate or stearyl sulfosuccinamate (stearyl sulfosuccinamate), but also includes a chromium complex that can be selected from the following polymer: polyvinyl stearyl carbamate, polyethyleneimine stearyl urea, C14 to C28 fatty acid and stearyl copolymer, as described in DE2845541A for example. Based on acrylic polymers, silicone or fluorosilicone compounds with perfluoroalkyl, for example, a stripping agent based on poly (dimethylsiloxane) is also suitable. Particularly preferably, the release layer comprises a silicone-based polymer. Particularly preferred examples of such silicone-based release polymers include polyurethane-modified and / or polyurea-modified silicones, preferably organopolysiloxane / polyurea / polyurethane block copolymers, particularly preferably as described in Example 19 of EP1336683B1, very particularly preferably anionically stabilized polyurethane-modified and urea-modified silicones having a silicone weight fraction of 70% and an acid value of 30 mg KOH / g. The use of polyurethane- and / or urea-modified silicones has the following effect: the product according to the invention has an optimized separation behavior together with optimized aging resistance and universal writability. In a preferred embodiment of the present invention, the release layer comprises 10 to 20% by weight, particularly preferably 13 to 18% by weight of release components.
[0082] In addition to the release layer, an antistatic coating may be present on top of the film, for example in the form of an amine or amide wax, such as Atmer (Croda) or Arquad T50. Such a coating is advantageous because it prevents electrostatic adhesion of the tape to fingers and objects.
[0083] In order to adjust the anchoring of at least one pressure-sensitive adhesive layer to at least one carrier layer to the desired extent, the carrier layer is preferably chemically and / or physically pretreated. The chemical pretreatment is carried out by applying a functional layer, in particular by a primer layer according to the prior art. The physical pretreatment can be carried out online or offline by corona treatment (especially in air or nitrogen atmosphere) and / or flame and / or plasma treatment and / or other surface activation methods.
[0084] The adhesive tape according to the invention is preferably used in a width of 9 to 50 mm, in particular 19 to 25 mm, and has a preferred thickness of 40 to 200 μm, preferably 50 to 180 μm, more preferably 60 to 130 μm. The selected width of the roll is usually 10, 15, 19, 25, 30 and 50 mm.
[0085] The self-adhesive tape according to the invention preferably has a peel adhesion (steel) in the range of 2.5 to 8.5 N / cm, particularly preferably 3.5 to 7.0 N / cm. The peel adhesion can be determined according to the method described in the "Test Methods" section (Test VI). Adhesion strengths in the specified range allow for secure fixing of movable objects during transport and at the same time allow for easy and residue-free re-detachment of the self-adhesive tape.
[0086] The self-adhesive tapes according to the invention further have a thermal shear strength (SAFT) of preferably greater than or equal to 95° C., particularly preferably greater than or equal to 115° C. The method for determining the thermal shear strength is also described in the “Test Methods” section (Test VII).
[0087] For the present invention, it is essential that the self-adhesive tape has good releasability, which is at least "+" according to test method VIII. For this purpose, the self-adhesive tape does not necessarily have to show peel adhesion and / or hot shear strength within the above-mentioned preferred property ranges.
[0088] In addition to good re-separability, the self-adhesive tape of the present invention is also distinguished by its sustainable manufacturability. It has been found that the use of solvents is unnecessary. Therefore, preferred embodiments are those in which the pressure-sensitive adhesive is produced by solvent-free mixing. This is preferably carried out continuously in a compounding extruder, wherein a twin-screw extruder is particularly preferred.
[0089] Another subject of the present invention is a method for producing the self-adhesive tape according to the invention. In the context of the production method according to the invention, the pressure-sensitive adhesive is applied to the carrier in a solvent-free manner by extrusion or contact nozzle coating. The pressure-sensitive adhesive can be applied to the carrier both on one side and on both sides.
[0090] Although solvent-free processing is preferred, it is likewise possible to produce and coat the pressure-sensitive adhesive in organic solvents or combinations of organic solvents. A self-adhesive tape is then obtained after drying of the coating.
[0091] In addition to the method for producing the self-adhesive tape according to the invention, the present invention also relates to the use of the self-adhesive tape according to the invention. Therefore, another subject of the present invention is the use of the self-adhesive tape according to the invention as an adhesive fixing tape for transport fixing, for bundling, packaging, palletizing and / or for edge reinforcement.
[0092] In addition, the tape can be used to excellently secure movable parts such as doors, flaps, etc. on printers or refrigerators during transportation from the manufacturer to the seller or buyer.
[0093] The adhesive tapes of the invention can also be advantageously used in the following applications by virtue of the properties described:
[0094] a) Used to temporarily fix larger parts such as car windshields after insertion into the frame (frame) until the PU liquid adhesive cures to prevent slippage during the curing process.
[0095] b) For end-joining of metal coils requiring re-separability without residue (end-ply bonding).
[0096] c) For temporary closure of containers requiring re-detachability without residue or general bonding to surfaces.
[0097] The present invention is illustrated by the following examples, which should in no way be understood as limiting the concept of the invention.
[0098] Example
[0099] The specimens were prepared from solution or in a solvent-free manner by extrusion. The selected production method is described accordingly in each individual example.
[0100] The expected raw material based on solvent was weighed into a glass sample container and provided with a solvent mixture consisting of acetone, special boiling point spirit and toluene (weight fraction based on the total amount of solvent was 16:54:30), and left on a rolling bench for 48 hours to obtain a 40 wt % solution. The solution was coated on a plate heated at 60 W min / m with a doctor blade. 2 On a 85 μm thick MOPP film pretreated with N2 corona, in order to obtain a 30 g / m 2 The dried pressure sensitive adhesive layer was covered with a layer of siliconized release paper until further testing.
[0101] The samples were also prepared by extrusion. Compounding was carried out at 180°C in a twin-screw extruder which fed the hot melt nozzle in-line. Coating was carried out in a contact process at 180°C, where the MOPP film to be coated was fed through a counter-roller (cooling roll). The cooling roll temperature was 15°C. The MOPP film was coated within 24 hours after a corona pretreatment at 100 W min / m under nitrogen. 2 conduct.
[0102] Chemicals used
[0103]
[0104] The following self-adhesive tapes (I) according to the invention were produced and their properties were analyzed and compared with those of a comparative adhesive tape (C) (the percentages in each case are in % by weight).
[0105] I1 I2 I3 Preparation method Solvents Solvents Extrusion Elastomer 1 59.0% 59.0% 51.0% Resin 1 15.0% 10.0% Resin 2 15.0% Plasticizer 1 15.0% 15.0% 18.0% Plasticizer 2 Enhancer 1 10.0% 10.0% 20.0% Additive 1 0.5% 0.5% 0.5% Additive 2 0.5% 0.5% 0.5% The sum of elastomer component + reinforcing component 69.0% 69.0% 71.0% Peel Adhesion 5.0N / cm 3.1N / cm 3.1N / cm SAFT 123℃ 125℃ 106℃ Re-separability ++ ++ ++
[0106] C1 C2 C3 C4 Preparation method Solvents Solvents Solvents Extrusion Elastomer 1 45.4% 43.5% 41.6% 52.0% Resin 1 47.0% Resin 2 50.0% 47.8% 45.8% Plasticizer 1 Plasticizer 2 4.5% 4.3% 4.2% Enhancer 1 4.3% 8.3% Additive 1 0.1% 0.1% 0.1% 0.5% Additive 2 0.5% The sum of elastomer component + reinforcing component 45.4% 47.8% 49.9% 52.0% Peel Adhesion 5.9N / cm 5.9N / cm 5.8N / cm 7.2N / cm SAFT 110℃ 113℃ 122℃ 103℃ Re-separability - - -- --
[0107] I4 I5 I6 I7 Preparation method Extrusion Extrusion Extrusion Solvents Elastomer 1 56.0% 41.0% 45.0% Elastomer 2 59.0% Resin 1 10.0% 29.0% 18.0% Resin 2 15.0% Plasticizer 1 18.0% 16.0% 18.0% 15.0% Plasticizer 2 Enhancer 1 15.0% 13.0% 18.0% 10.0% Additive 1 0.5% 0.5% 0.5% 0.5% Additive 2 0.5% 0.5% 0.5% 0.5% The sum of elastomer component + reinforcing component 71.0% 54.0% 63.0% 69.0% Peel Adhesion 3.5N / cm 6.9N / cm 4.5N / cm 1.8N / cm SAFT 113℃ 106℃ 107℃ 129℃ Re-separability ++ ++ ++ ++
[0108] C5 C6 C7 C8 Preparation method Extrusion Extrusion Extrusion Solvents Elastomer 1 40.0% 34.0% 66.0% 59.0% Resin 1 43.0% 37.0% 26.0% Resin 2 15.0% Plasticizer 1 16.0% 14.0% 7.0% 15.0% Plasticizer 2 Enhancer 1 14.0% Enhancer 2 10.0% Additive 1 0.5% 0.5% 0.5% 0.5% Additive 2 0.5% 0.5% 0.5% 0.5% The sum of elastomer component + reinforcing component 40.0% 48.0% 66.0% 69.0% Peel Adhesion 6.2N / cm 8.2N / cm 1.2N / cm 5.8N / cm SAFT 86℃ 94℃ 106℃ 110℃ Re-separability - -- -- -
[0109] I8 I9 I10 I11 Preparation method Extrusion Extrusion Extrusion Extrusion Elastomer 1 45.0% 39.0% 51.0% 57.0% Resin 1 34.0% 15.0% 35.0% Resin 2 Resin 3 25.0% Plasticizer 1 11.0% 18.0% 18.0% Plasticizer 2 Enhancer 1 9.0% 17.0% 15.0% 7.0% Additive 1 0.5% 0.5% 0.5% 0.5% Additive 2 0.5% 0.5% 0.5% 0.5% The sum of elastomer component + reinforcing component 54.0% 56.0% 66.0% 64.0% Peel Adhesion 6.7N / cm 7.1N / cm 7.2N / cm 5.0N / cm SAFT 105℃ 105℃ 104℃ 113℃ Re-separability ++ + ++ ++
[0110] Compared to the comparative adhesive tapes C1 to C8, the self-adhesive tapes I1 to I11 according to the invention have satisfactory (+) to very good (++) re-separability. It can also be seen from the data that the limitation of the fraction of mineral oil and the fraction of the elastomer component and the reinforcing component in the pressure-sensitive adhesive of at least 52% by weight has a favorable effect on the re-separability.
[0111] Test method:
[0112] Test I - Molar Mass (GPC)
[0113] (a) Peak molar masses of individual block copolymer modes
[0114] In terms of molar mass distribution, polymers are multimodal systems. A mixture of different polymers can be understood as a multimodal system, in which each polymer contributes its own molar mass distribution. A mixture of block copolymers with structures having different molar mass distributions can also be understood as a multimodal system. Thus, each block copolymer contributes its own molar mass distribution. For simplicity, these are referred to as block copolymer modes here.
[0115] GPC (gel permeation chromatography) is a metrological method for determining the molar masses of individual polymer modes in a mixture of different polymers. For block copolymers prepared by living anionic polymerization which can be used in the sense of the present invention, the molar mass distribution is generally narrow enough to allow the polymer modes that can be assigned to triblock copolymers, diblock copolymers or multiblock copolymers to appear with sufficient resolution from one another in the elution spectrum (elugram). The peak molar masses of the individual polymer modes can then be read off from the elution spectrum.
[0116] The peak molar mass of the elastomer (peak M W ) was determined by GPC. The eluent used was THF. The measurement was carried out at 23°C. The pre-column used was PSS-SDV, 5μ, ID 8.0mmx50mm. For separation, the column used was PSS-SDV, 5μ, as well as and Each had an ID of 8.0 mm x 300 mm. The sample concentration was 4 g / l and the flow rate was 1.0 ml / min. Calibration was performed using the ReadyCal kit Poly(styrene) high commercially available from PSS Polymer Standard Service GmbH, Mainz (μ = μm; ).
[0117] (b) Weight average molar mass
[0118] The weight average molecular weight M of the tackifier resin, plasticizer and reinforcing agent w Determined by GPC. The eluent used was THF. The measurement was carried out at 23°C. The pre-column used was PSS-SDV, 5μ, ID 8.0mmx50mm. For separation, the column used was PSS-SDV, 5μ, as well as and Each had an ID 8.0 mm x 300 mm. The sample concentration was 4 g / l and the flow rate was 1.0 ml / min. The calibration was performed using the ReadyCal kit Poly(styrene) high commercially available from PSS Polymer Standard Service GmbH, Mainz.
[0119] Test II-DSC
[0120] In particular, the glass transition point of a polymer or polymer block, synonymously referred to as glass transition temperature, is reported as the result of measurement by differential scanning calorimetry (DSC) according to DIN 53 765, in particular Sections 7.1 and 8.1, but with a uniform heating and cooling rate of 10 K / min in all heating and cooling steps (see DIN 53 765; Section 7.1; Note 1). The sample weight is 20 mg. The melting temperature or softening temperature of a polymer or polymer block is also determined in this way.
[0121] Test IIIa-DACP
[0122] 5.0 g of the test substance (tackifier resin sample to be checked) are weighed into a dry sample glass and 5.0 g of xylene (isomer mixture, CAS [1330-20-7], ≥98.5%, Sigma-Aldrich #320579 or equivalent) are added. The test substance is dissolved at 130° C. and then cooled to 80° C. Any xylene that escapes is made up with further xylene so that 5.0 g of xylene are present again. Subsequently, 5.0 g of diacetone alcohol (4-hydroxy-4-methyl-2-pentanone, CAS [123-42-2], 99%, Aldrich #H41544 or equivalent) are added. The sample tube is shaken until the test substance has completely dissolved. To this end, the solution is heated to 100° C. The sample tube containing the resin solution is then introduced into a Novomatics Chemotronic Cool turbidity meter and heated to 110° C. therein. It is cooled at a cooling rate of 1.0 K / min. The cloud point is detected optically. For this purpose, the temperature at which the turbidity of the solution is 70% is recorded. The results are reported in ° C. The lower the DACP value, the more polar the test substance.
[0123] Test IIIb-MMAP
[0124] 5.0 g of the test substance (tackifier resin sample to be investigated) are weighed into a dry sample tube and 10 ml of dry aniline (CAS [62-53-3], ≥99.5%, Sigma-Aldrich #51788 or equivalent) and 5 ml of dry methylcyclohexane (CAS [108-87-2], ≥99%, Sigma-Aldrich #300306 or equivalent) are added. The sample tube is shaken until the test substance has completely dissolved. To this end, the solution is heated to 100° C. The sample tube containing the resin solution is then introduced into a Novomatics Chemotronic Cool turbidity point measuring instrument and heated therein to 110° C. It is cooled at a cooling rate of 1.0 K / min. The turbidity point is detected optically. To this end, the temperature at which the solution has a turbidity of 70% is recorded. The results are reported in ° C. The lower the MMAP, the higher the aromaticity of the test substance.
[0125] Test IV - (Tackifier Resin) Softening Temperature
[0126] For the individual substances: (Tackifier) The resin softening temperature (softening point; soft point) is determined according to the method known as the ring & ball method and is standardized according to ASTM E28.
[0127] Test V - Melt Viscosity
[0128] To determine the melt viscosity of the plasticizer resin, a shear stress scan was performed in a rotational manner in a shear stress regulated DSR 200N rheometer from Rheometrics Scientific. A cone / plate measuring system with a diameter of 25 mm (cone angle 0.1002 rad) was used; the measuring head was air-mounted and suitable for standard force measurements. The gap was 0.053 mm and the measuring temperature was 25° C. The frequency was varied from 0.002 Hz to 200 Hz and the melt viscosity was recorded at 1 Hz.
[0129] Test VI - Peel Adhesion, Steel
[0130] The peel adhesion was determined as follows. A polished steel plate with a thickness of 2 mm (ASTM D3330; three times cleaning with acetone using a cellulose cloth and evaporation for 10 minutes) was used as a given adhesive substrate. The bondable sheet element to be investigated (30 g / m on 85 μm MOPP film) was placed on a 10-mm thick sheet of 10-mm thick steel plate. 2The pressure-sensitive adhesive layer) was cut into a width of 20 mm and a length of about 25 cm, equipped with a handle (unless otherwise specified), and immediately thereafter pressed against the adhesive substrate with a 4 kg steel roller at a speed of 10 m / min for five times. Immediately thereafter, the bondable sheet-like element was pulled away from the adhesive substrate at an angle of 180 ° with a tensile tester (from Zwick) at a speed of v = 300 mm / min, and the force required for this at room temperature was measured. The measured values (in N / cm) were obtained as the average value from two individual measurements.
[0131] Test VII-SAFT
[0132] This test is used to quickly test the shear strength of adhesive formulations under temperature load. To this end, the test specimens to be investigated are adhered to a temperature-controlled steel plate and loaded with a weight (50 g), and the shear distance is recorded.
[0133] Test sample preparation:
[0134] The test samples (30 g / m 2 , on 85μm MOPP carrier) cut into a size of 10mm*50mm.
[0135] The cut-to-size tape samples were bonded with the other adhesive side to a polished test panel cleaned with acetone (material 1.4301, DIN EN 10088-2, surface 2R, surface roughness R a =30 to 60 nm, size 50 mm * 13 mm * 1.5 mm), so that the bonding area of the sample is 13 mm * 10 mm in height * width, and the test plate protrudes 2 mm from the top edge. Subsequently, a 2 kg steel roller is rolled 6 times at a speed of 10 m / min to fix the bond. The sample is reinforced flush with a stable adhesive strip on the top, which serves as the base of the distance sensor. The sample is then suspended by means of the plate so that the longer protruding end of the test sample points vertically downward.
[0136] Measurement:
[0137] The sample to be measured is loaded with a weight of 50 g at the lower end. The test plate with the bonded sample is heated starting at 25°C at a rate of 9 K / min to a final temperature of 200°C.
[0138] The sliding distance of the sample as a function of temperature and time is observed by a distance sensor. The maximum sliding distance is set to 1000 μm (1 mm); if exceeded, the test is terminated and the failure temperature is recorded. Test conditions: room temperature 23+ / -3°C, relative humidity 50+ / -5%. The results are reported as the average value from two separate measurements and in °C.
[0139] Test VIII - Re-separability
[0140] The test strip (width 20 mm) was cut into a length of 250 mm and laminated to a steel plate with a thickness of 2 mm (according to ASTM D3330; washed three times with acetone using a cellulose cloth and evaporated for 10 minutes) using a rubber roller and rolled back and forth once using a 2 kg steel roller. The assembly was stored at 60° C. and 95% relative humidity for 7 days. It was then equilibrated at 23° C. and 50% relative humidity for 24 hours and removed at a speed of 10 m / min at an angle of about 170°. Subsequently, the substrate was visually inspected for any tape residue.
[0141] A dual assessment was performed using the following rating scale:
[0142] ++ ≤1% adhesive residue (by area), no carrier splitting Passed very well + ≤5% adhesive residue (by area), no carrier splitting Pass well - >5% adhesive residue (by area), no carrier splitting fail -- Vector Splitting fail
Claims
1. A self-adhesive tape comprising a carrier consisting of a uniaxially oriented polypropylene film and a pressure-sensitive adhesive comprising: a) 38 to 65 wt. % of an elastomeric component; b) 8 to 45 weight percent of a tackifier resin component; and c) 2 to 22% by weight of reinforcing components, In each case based on the total weight of the pressure-sensitive adhesive, The pressure-sensitive adhesive is characterized in that the sum of the fractions of the elastomeric component and the reinforcing component in the pressure-sensitive adhesive is at least 52% by weight, based on the total weight of the pressure-sensitive adhesive, and wherein the reinforcing component has a weight average molecular weight M of at least 800 g / mol. w at least one resin. 2 . The self-adhesive tape according to claim 1 , characterized in that the thickness of the carrier film after orientation is 20 to 150 μm, preferably 25 to 100 μm. 3 . The self-adhesive tape according to claim 1 , wherein the elastomeric component is a polydiene block copolymer, more particularly a polyvinylaromatic-polydiene block copolymer.
4. The self-adhesive tape according to claim 1 , wherein the tackifier resin component is selected from nonpolar hydrocarbon resins, preferably hydrogenated and nonhydrogenated polymers of dicyclopentadiene; nonhydrogenated, partially, selectively or fully hydrogenated hydrocarbon resins based on C5 or C5 / C9 monomer streams, or partially, selectively or fully hydrogenated hydrocarbon resins based on C9 monomer streams, and polyterpene resins based on α-pinene and / or β-pinene and / or δ-limonene.
5. The self-adhesive tape according to claim 1, characterized in that the fraction of the tackifier resin component in the pressure-sensitive adhesive is up to 40% by weight, particularly preferably up to 35% by weight, in each case based on the total weight of the pressure-sensitive adhesive.
6. The self-adhesive tape according to claim 1 , wherein the reinforcing component is at least one resin based on at least one hydrocarbon compound, in particular an aromatic hydrocarbon compound, preferably obtained from a C8 and / or C9 stream and preferably selected from styrene, α-methylstyrene, p-methylstyrene, indene, methylindene and copolymers thereof, wherein the at least one resin of the reinforcing component preferably has a weight average molecular weight M of 1000 g / mol to 15000 g / mol, preferably 2000 g / mol to 10000 g / mol, as determined by GPC. w .
7. The self-adhesive tape according to claim 1, characterized in that the reinforcing component is present in the pressure-sensitive adhesive in an amount of 8 to 18% by weight, in each case based on the total weight of the pressure-sensitive adhesive.
8. Self-adhesive tape according to at least one of the preceding claims, characterised in that at least one resin of the reinforcing component has a softening point of at least 130°C, preferably at least 140°C, measured according to ASTM E28.
9. Self-adhesive tape according to at least one of the preceding claims, characterised in that the sum of the fractions of elastomeric component and reinforcing component in the pressure-sensitive adhesive is at least 55% by weight, preferably at least 60% by weight, based on the total weight of the pressure-sensitive adhesive.
10. The self-adhesive tape according to claim 1, characterized in that the pressure-sensitive adhesive further comprises a plasticizer component, preferably in an amount of 3 to 25% by weight, preferably 8 to 18% by weight, based on the total weight of the pressure-sensitive adhesive.
11. The self-adhesive tape according to claim 1, characterized in that the fraction of mineral oil and / or mineral oil mixture in the pressure-sensitive adhesive is not more than 3% by weight, preferably not more than 1.5% by weight, based on the total weight of the pressure-sensitive adhesive.
12. The self-adhesive tape according to claim 1, characterized in that the pressure-sensitive adhesive comprises further additives, preferably in an amount of not more than 18% by weight, particularly preferably not more than 10% by weight, based on the total weight of the pressure-sensitive adhesive. 13 . The self-adhesive tape according to claim 1 , wherein the pressure-sensitive adhesive is produced by solvent-free mixing.
14. Method for producing a self-adhesive tape according to at least one of the preceding claims, characterized in that the pressure-sensitive adhesive is applied to the carrier in a solvent-free manner by extrusion or contact nozzle coating.
15. Use of the self-adhesive tape according to at least one of claims 1 to 13 as a fixing tape for transport fixing, for bundling, packaging, palletizing and / or for edge reinforcement.