Al-Mg-Si alloy profile with low critical quenching rate and high strength as well as preparation method and application of Al-Mg-Si alloy profile

By adopting low critical quenching rate and double-stage quenching treatment in Al-Mg-Si alloy profiles, the problems of insufficient mechanical properties and corrosion resistance of thin-walled structural profiles in the existing technology are solved, and high-strength and high-precision aluminum profiles are achieved. Alloy profiles, suitable for photovoltaic frame applications.

CN118814033AActive Publication Date: 2024-10-22ANHUI XINBO NEW ENERGY AUTO PARTS CO LTD

Patent Information

Application Number
CN202411300272.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-10-22
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing high-strength Al-Mg-Si alloy materials prepared by the online quenching process have poor mechanical properties and corrosion resistance in thin-walled structural profiles, and have low precision, making it difficult to meet the lightweight and high-strength requirements of photovoltaic modules.

Method used

Adopt low critical quenching rate aluminum alloy profiles, containing Si 0.70~1.00%, Cu≤0.15%, Mg 0.50~0.70%, Fe≤0.25%, Ti≤0.10%, Mn≤0.15%, Cr≤0.15%, Zr≤0.20%, the balance is Al, through double-stage quenching treatment and homogenization process, the quenching rate is controlled at 3 ~10℃/s, forming uniform grain boundary precipitation, improving toughness and corrosion resistance.

Benefits of technology

It achieves improvements in high strength, tensile strength, yield strength and corrosion resistance, ensuring the high precision of thin-walled structural profiles and the application performance of photovoltaic frames.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814033A_ABST
    Figure CN118814033A_ABST
Patent Text Reader

Abstract

The invention provides a low-critical-quenching-rate high-strength Al-Mg-Si alloy profile as well as a preparation method and application thereof, and relates to the technical field of aluminum alloy materials. The aluminum alloy profile with the low critical quenching rate comprises, by mass, 0.70%-1.00% of Si, smaller than or equal to 0.15% of Cu, 0.50%-0.70% of Mg, smaller than or equal to 0.25% of Fe, smaller than or equal to 0.10% of Ti, smaller than or equal to 0.15% of Mn, smaller than or equal to 0.15% of Cr, smaller than or equal to 0.10% of Zn, smaller than or equal to 0.20% of Zr and the balance Al, and the total amount is 100%. The critical quenching rate of the aluminum alloy profile is 3-10 DEG C / s, and the aluminum alloy profile has high tensile strength, yield strength, elongation, Vickers hardness and corrosion resistance with the intergranular corrosion level being A.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a low critical quenching rate high-strength Al-Mg-Si alloy profile and a preparation method and application thereof. Background Art

[0002] Aluminum alloy frames are widely used in the field of solar photovoltaics, covering almost all types of photovoltaic modules. Aluminum alloy frames play an important role in a variety of application scenarios such as residential buildings, commercial buildings, public facilities, industrial facilities, rural areas, desert areas, mountainous areas and grasslands. In recent years, although there have been a variety of frame alternatives such as frameless double-glass modules, rubber snap frames, steel structure frames, composite frames, etc., long-term practical applications have proved that aluminum alloy frames still have absolute advantages. With the global emphasis on renewable energy and the continuous development of photovoltaic technology, the market demand for aluminum alloy frames will continue to grow.

[0003] With the further development of photovoltaic technology and the increasing market demand for lightweight photovoltaic modules, the technology applied to aluminum alloy materials will continue to innovate and improve. For a given composition, heat-treated strengthened aluminum alloys must undergo solid solution quenching and aging heat treatment to achieve high strength, and the cooling rate is a key parameter for quenching heat treatment. If the cooling rate is lower than the critical cooling rate, grain boundary precipitation will occur during the quenching process, which is not conducive to improving corrosion resistance, toughness, and subsequent aging precipitation to improve strength. Simply increasing the content of alloying elements is an important means to increase strength and reduce wall thickness to achieve lightweight, but the precipitation problem caused by high alloying elements during the quenching process (critical cooling rate is too high) makes it impossible to use strong wind cooling online quenching to achieve high strength and reduce the corrosion resistance of the alloy; while high cooling intensity water-cooled online quenching brings about residual stress, deformation, and even cracking during the quenching process of thin-walled structures, and leads to poor toughness. These restrict the application of high-strength aluminum alloys in thin-walled photovoltaic frames. Summary of the invention

[0004] 1. Technical issues to be resolved In view of the shortcomings of the prior art, the present invention provides a high-strength Al-Mg-Si alloy profile with a low critical quenching rate and a preparation method and application thereof, which solves the technical problems that the high-strength Al-Mg-Si alloy materials prepared by the existing online quenching process have poor mechanical properties and corrosion resistance, and low precision of thin-walled structural profiles.

[0005] (II) Technical solution To achieve the above objectives, the present invention is implemented through the following technical solutions: On the one hand, the present invention provides a low critical quenching rate aluminum alloy profile, comprising the following components in percentage by mass: Si 0.70-1.00%, Cu≤0.15%, Mg 0.50-0.70%, Fe≤0.25%, Ti≤0.10%, Mn≤0.15%, Cr≤0.15%, Zn≤0.10%, Zr≤0.20%, the remainder is Al, and the total amount is 100%.

[0006] The critical quenching rate of the aluminum alloy profile with the above alloy content is 3-10°C / s, and it has high tensile strength, yield strength, elongation, Vickers hardness and corrosion resistance with intergranular corrosion grade A.

[0007] Preferably, the Mg / Si is 0.8 to 1.2, so as to avoid precipitation of silicon-rich phase particles at grain boundaries during quenching and aging treatment to reduce the toughness and corrosion resistance of the alloy, and achieve an alloy elongation of more than 10% and a maximum grain boundary corrosion depth of less than 30 mm.

[0008] Preferably, the sum of the mass percentages of Mg and Si is 1.35-1.53%. The sum of the mass percentages of Mg and Si is 1.35% to ...% to increase the amount of precipitation of the strengthening phase in the grain after aging and improve the strength (yield strength reaches 280 MPa or more). The sum of the mass percentages of Mg and Si is 1.35% to 1.53% to avoid the formation of Mg in the grain boundary during quenching and aging. 2 The continuous precipitation of Si phase and the formation of precipitation-free precipitation zone ensure that the alloy elongation is more than 10% and the maximum intergranular corrosion depth is less than 30mm.

[0009] Preferably, the mass percentage of Zr is 0.04-0.2%, which strengthens the ingot soaking process. 3 The formation of Zr-containing dispersed phase particles such as Zr hinders the recrystallization after extrusion and quenching and refines the grains, thereby improving the toughness and corrosion resistance of the alloy.

[0010] Preferably, the total mass percentage of Mn and Cr is 0.06-0.15%; the mass percentage of Mn is 0.03-0.07%, which solves the problem of uneven distribution of Zr-containing dispersed phase particles and improves the toughness and corrosion resistance of the alloy.

[0011] In another aspect, the present invention provides a method for preparing the low critical quenching rate aluminum alloy profile as described in the first aspect, comprising the following steps: S1. Melt the Al ingot, add Al-Si, Al-Zr, Al-Mn, Al-Cr, Al-Fe, Al-Ti and Al-Zn master alloy, Cu ingot and Mg ingot for melting treatment, stir evenly to obtain an aluminum alloy melt with uniform composition; S2, after rapid sampling and analysis of the aluminum alloy melt, adding insufficient metal elements to achieve the composition ratio of the target aluminum alloy profile, and then performing slag removal and heating to obtain aluminum alloy liquid; S3, refining the aluminum alloy liquid under an inert gas atmosphere, and then sequentially casting and homogenizing to obtain an aluminum alloy cast rod; S4, heating, heat-insulating, and extruding the aluminum alloy cast rod, and during the extrusion process, performing a double-stage quenching treatment on the aluminum alloy cast rod to obtain an aluminum alloy profile substrate; S5. The aluminum alloy profile substrate is subjected to stretching and straightening, aging treatment, sandblasting, and anodizing treatment in sequence to obtain a low critical quenching rate aluminum alloy profile.

[0012] Preferably, the two-stage quenching treatment in S4 includes first cooling to (250-300)°C by spraying quenching liquid at a cooling rate of 3-10°C / s, and then cooling to below 60°C by strong air cooling at a cooling rate of 2-3°C / s.

[0013] Preferably, the quenching liquid comprises the following components in parts by weight: 1 to 3 parts of polyalkylene glycol, 5 to 9 parts of polyethylene glycol, and 88 to 94 parts of water.

[0014] The preparation method of the aluminum alloy profile of the present application includes using the above-mentioned quenching liquid to perform a double-stage quenching treatment on the aluminum alloy extruded profile, first using the above-mentioned quenching liquid to cool the temperature of the aluminum alloy extruded profile with a higher temperature to (250-300)°C at a cooling rate of 3-10°C / s, and then using strong air cooling to cool it to below 60°C at a cooling rate of 2-3°C / s. This double quenching process ensures that the aluminum alloy profile undergoes obvious uniform (along grain boundaries / phase boundaries) precipitation, thereby improving the corrosion resistance of the aluminum material, and can also promote subsequent uniform aging precipitation to improve the mechanical properties of the alloy.

[0015] Preferably, the mass percentage concentration of the quenching liquid is (5-11)%.

[0016] Preferably, in S1, an electromagnetic stirring device is used for stirring during the melting process to make the temperature and composition of the aluminum alloy melt more uniform. After all the metals are melted, the temperature of the aluminum alloy melt is 700-760°C.

[0017] Preferably, S2 satisfies at least one of the following conditions: The temperature of the aluminum alloy melt is not less than 700℃ when sampling; After the slag removal is completed, the temperature of the aluminum alloy liquid is heated to 715-730°C.

[0018] Preferably, S3 satisfies at least one of the following conditions: The temperature of the aluminum alloy liquid before refining is (720-740)°C, and the refining time is (0.5-0.6)h; Casting speed is (110-120) mm / min; The homogenization treatment includes: firstly heating to (470-490)℃ at (20-100)℃ / h and keeping at (3-3.5)h, in which a large number of small, uniformly distributed and coherent Al (Mn, Cr, Zr) dispersed phase particles are formed, thereby providing conditions for controlling the formation of grain boundaries after extrusion and uniform precipitation (along grain boundaries / phase boundaries) during interphase quenching; then heating to 570℃ at 200-300℃ / h and keeping at (1-3)h, in which the heat preservation can achieve β-AlFe The MnSi phase transforms to the α-AlFeMnSi phase with less influence. The rapid heating is to avoid the transformation of the coherent Al (Mn, Cr, Zr) dispersed phase particles formed in the early stage to incoherent; then strong wind is used to cool to (200-300) ° C, and finally cooling to room temperature is carried out by cooling water spray. The rapid cooling at this stage is to avoid the precipitation of coarse Mg2Si phase during the cooling process, thereby inducing the re-transformation and uneven precipitation of Al (Mn, Cr, Zr) dispersed phase particles during the subsequent extrusion heating and deformation process.

[0019] Preferably, in S4, the heating temperature is 440-510° C., the holding time is 3-4 hours, and the extrusion process is forward extrusion.

[0020] Preferably, S5 satisfies at least one of the following conditions: The elongation rate of tensile straightening is (0.5~1.2)%; The aging treatment includes: heating to (175-195)°C at a rate of 100°C / h, then keeping warm for (3-6) hours, and after being taken out of the furnace, cooling with strong wind at a rate of 120°C / h to below 40°C.

[0021] In the third aspect, the present invention provides an application of a low critical quenching rate aluminum alloy profile described in the first aspect and / or prepared by the preparation method described in the second aspect in the manufacture of a high-precision, thin-walled solar photovoltaic frame, wherein the low critical quenching rate aluminum alloy profile has a critical quenching rate of (3-10) °C / s, a tensile strength of (310-340) N / mm2, a yield strength of (280-310) N / mm2, an elongation of (10-16)%, a Vickers hardness of (16-19) HW, and a maximum intergranular corrosion depth of (19-29) um. The wall thickness of the thin-walled structure is (0.5-1.0) mm, which is suitable for the field of solar photovoltaic frames. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is a scanning electron microscope photograph of the aluminum alloy profile prepared in Example 1.

[0024] Figure 2 It is a schematic diagram of the cross section of an extruded profile. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0027] Examples 1 to 6 and Comparative Examples 1 to 8 The method for preparing the aluminum alloy profiles in Examples 1 to 6 and Comparative Examples 1 to 8 of the present invention comprises the following steps: S1. Clean the smelting furnace and add Al ingots into the smelting furnace for heating and melting. Place Al-Si, Al-Zr, Al-Mn, Al-Cr, Al-Fe, Al-Ti and Al-Zn master alloys, Cu ingots and Mg ingots into the smelting furnace, perform melting treatment and stir evenly to obtain an aluminum alloy melt; S2, the aluminum alloy melt of S1 is sampled for rapid detection and analysis. When sampling, the temperature of the aluminum liquid mixture must be higher than 700°C. The chemical composition of the target aluminum alloy profile is adjusted by adding metal elements (see Table 1 for details). After slag removal and heating, the aluminum alloy liquid is obtained, and its temperature is controlled at 730°C. S3, spraying and refining the S2 aluminum alloy liquid in a static furnace with nitrogen, the temperature of the aluminum alloy liquid is controlled at 735°C, and the spraying and refining time is 0.5h; the aluminum alloy liquid is flowed into a mold, and the aluminum alloy liquid is cast by a hot top method, at a casting speed of 120mm / min and a cooling water flow rate of 100m3 / h. After the casting is completed, it is homogenized, and the homogenization treatment includes: first heating from 50℃ / h to 470℃ and keeping it for 3h, then heating to 570℃ at 200℃ / h and keeping it for 1h, then cooling to 200℃ with strong wind, and finally cooling to room temperature by cooling water spray to obtain aluminum alloy cast rods; S4. Keep the aluminum alloy casting rod at 460℃ for 4h, then take it out of the furnace and put it into the extrusion cylinder for forward extrusion. The cross section of the extruded profile is as follows Figure 2 As shown, after extrusion, it is immediately subjected to a double-stage quenching method through an online quenching device. First, 6% quenching liquid is sprayed and cooled at 5°C / s to 260°C, and then strong air cooling is used at 3°C / s to cool to below 60°C.

[0028] The quenching liquid includes 1 part of polyalkylene glycol, 5 parts of polyethylene glycol and 94 parts of water. The polyalkylene glycol and polyethylene glycol are first mixed evenly, and the mixture is added into water at room temperature, stirred evenly, and then heated to 70°C and dissolved under stirring to obtain the quenching liquid.

[0029] S5. Cool the aluminum alloy profile substrate to below 60°C, then stretch and straighten it, and control the stretching rate at 0.6%; saw and pack it into baskets according to the fixed length, and then send it to the aging furnace for aging treatment: heat it to 185°C at a rate of 100°C / h, keep it warm for 5h, take it out and cool it to below 40°C at a rate of 120°C / h; then sandblast and anodize it to obtain the aluminum alloy profile.

[0030] Comparative Example 9 The difference between this comparative example and Example 1 is that the two-stage quenching method in S5 is different. Specifically, the two-stage quenching method is carried out by an online quenching device. First, pure water spray cooling is adopted to cool to 260°C at 80°C / s, and then strong air cooling is adopted to cool to below 60°C at 3°C / s. The rest is the same as Example 1.

[0031] Comparative Example 10 The difference between this comparative example and Example 1 is that no homogenization treatment is performed after the casting is completed in S3, and the rest is the same as Example 1.

[0032] The chemical compositions of the aluminum alloy profiles in Examples 1 to 6 and Comparative Examples 1 to 8 of the present invention are shown in Table 1.

[0033] The aluminum alloy profiles prepared in the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 10 were tested for tensile strength, yield strength, and elongation according to GB / T 16865-2013 Specimens and methods for tensile testing of deformed aluminum, magnesium, and their alloy products; their Vickers hardness was tested according to the standard YS / T 420 Vickers hardness test method for aluminum alloys; and their maximum intergranular corrosion depth was tested according to the ISO 11846-2008 standard. The critical quenching rate was tested according to the method described in the patent "Device and method for measuring the hardening depth of aluminum alloy materials" (ZL200710034410.8). The test results are shown in Table 2.

[0034] Table 1 Chemical composition of target aluminum alloy profiles prepared in Examples 1 to 6 and Comparative Examples 1 to 8

[0035] The preparation method of Comparative Example 9 includes a homogenization treatment after the casting is completed, and bipolar quenching is first performed by pure water spray cooling and then by strong air cooling; in S3 of Comparative Example 10, no homogenization treatment is performed after the casting is completed. From Table 2, it can be seen from the comparison of the data of Comparative Examples 9 and 10 with that of Example 1 that the corrosion resistance of the aluminum alloy profiles of Comparative Examples 9 and 10 is significantly worse than that of Example 1. This is because a large number of small, uniformly distributed and coherent Al (Mn, Cr, Zr) dispersed phase particles can be formed after the homogenization treatment of the preparation method of the present application, and the dispersed phase particles can be precipitated uniformly (along the grain boundaries / phase boundaries) at the phase interface in the two-stage quenching process of the present application using polyalkylene glycol and polyethylene glycol as the quenching liquid, because the dispersed phase particles can improve the corrosion resistance of the aluminum material after the phase interface is uniformly precipitated (along the grain boundaries / phase boundaries). The surface morphology of the aluminum alloy profile prepared in the above Example 1 was observed using a scanning electron microscope (see Figure 1 ), it can be seen that the alloy profile of Example 1 forms a large number of fine-sized coherent Al (Mn, Cr, Zr) particles. Therefore, the preparation method of the present application includes a homogenization treatment and a two-stage quenching process. Under the synergistic effect of the two, the corrosion resistance of the aluminum material is improved, and the intergranular corrosion grade is A.

[0036] Secondly, it can be seen from the data in Table 2 that the aluminum alloy profile prepared by the present invention has high tensile strength, yield strength, elongation and Vickers hardness. It can be seen from the data in Examples 1 to 3 that when the Mg+Si (i.e., the total mass percentage of Mg and Si) changes slightly, as the Zr content increases, the tensile strength, yield strength and elongation increase accordingly.

[0037] It can be seen from the data of Examples 4 to 6 that, when the Zr content is constant, the performance is basically maintained at a high level when Mg+Si fluctuates between 1.35 and 1.41% and Mg / Si fluctuates between 0.88 and 0.93.

[0038] From the twisting degree of the 6m long aluminum alloy profiles prepared in Examples 1 to 6, it can be seen that the aluminum alloy profiles of the present invention have high precision.

[0039] It can be seen from the data of Comparative Example 1 and the embodiment that the tensile strength, yield strength, elongation and Vickers hardness of the aluminum alloy profile prepared without Zr are reduced, the maximum intergranular corrosion depth is higher, and the intergranular corrosion grade is B, indicating that the mechanical properties and corrosion resistance of the aluminum alloy profile prepared without Zr in Comparative Example 1 are greatly reduced.

[0040] It can be seen from the data of Comparative Example 2 and the embodiment that even when the Mg+Si and Zr contents are relatively high, the mechanical properties of the aluminum alloy profile prepared in Comparative Example 2 are reduced due to the small Mg / Si value.

[0041] From the data comparison between Comparative Example 3 and the embodiment, it can be seen that the mechanical properties of Comparative Example 3 are reduced due to the lack of addition of Cu, that is, the strength of the alloy is improved by adding a trace amount of Cu in the present invention.

[0042] From the comparison between the comparative example 4 and the embodiment data, it can be seen that in the comparative example 4, the Mg+Si content exceeds 1.53%. Even though the tensile strength and yield strength are increased, the elongation is decreased and the intergranular corrosion performance is also decreased.

[0043] Table 2 Performance test data of aluminum alloy profiles

[0044] From the comparison between the comparative example 5 and the example data, it can be seen that the Mg+Si in the comparative example 5 is lower than 1.35%, resulting in a decrease in both the yield strength and the tensile strength.

[0045] From the comparison between the comparative example 6 and the example data, it can be seen that since the Mg / Si ratio of the comparative example 6 is greater than 1.2, the yield strength and tensile strength of the comparative example 6 decrease significantly even though the Mg+Si ratio is in the range of 1.35-1.53%.

[0046] From the comparison between the comparative example 7 and the example data, it can be seen that the comparative example 7 has a Zr content exceeding 0.20%, resulting in a significant decrease in its strength, elongation and intergranular corrosion performance.

[0047] From the data comparison between Comparative Example 8 and the embodiment, it can be seen that since the Cr and Mn contents of Comparative Example 8 are 0, although the Mg+Si content is in the range of 1.35-1.53%, its intergranular corrosion performance and elongation are significantly reduced.

[0048] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0049] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low critical quenching rate aluminum alloy profile, characterized in that: The invention comprises the following components in mass percentage: Si 0.70-1.00%, Cu ≤ 0.15%, Mg 0.50-0.70%, Fe ≤ 0.25%, Ti ≤ 0.10%, Mn ≤ 0.15%, Cr ≤ 0.15%, Zn ≤ 0.10%, Zr ≤ 0.20%, the balance is Al, and the total amount is 100%; The ingot homogenization treatment of the low critical quenching rate aluminum alloy profile includes: first heating to 470-490°C at 20-100°C / h and keeping warm for 3-3.5h, then heating to 570°C at 200-300°C / h and keeping warm for 1-3h, then cooling to 200-300°C by strong wind, and finally cooling to room temperature by spraying cooling water; after the homogenization treatment, a two-stage quenching treatment is adopted, and the two-stage quenching treatment includes first cooling to (250-300)°C by spraying quenching liquid at a cooling rate of 3-10°C / s, and then cooling to below 60°C by strong wind at a cooling rate of 2-3°C / s.

2. The low critical quenching rate aluminum alloy profile according to claim 1, characterized in that: The Mg / Si is 0.8 to 1.

2.

3. The low critical quenching rate aluminum alloy profile according to claim 1, characterized in that: The total mass percentage of Mg and Si is 1.35-1.53%.

4. A method for preparing a low critical quenching rate aluminum alloy profile according to any one of claims 1 to 3, characterized in that: The steps include: S1. Melt the Al ingot, add Al-Si, Al-Zr, Al-Mn, Al-Cr, Al-Fe, Al-Ti and Al-Zn master alloy, Cu ingot and Mg ingot for melting treatment, and stir evenly to obtain an aluminum alloy melt; S2, after rapid sampling and analysis of the aluminum alloy melt, adding insufficient metal elements to achieve the composition ratio of the target aluminum alloy profile, and then performing slag removal and heating to obtain aluminum alloy liquid; S3, refining the aluminum alloy liquid under an inert gas atmosphere, and then sequentially casting and homogenizing to obtain an aluminum alloy cast rod; S4, heating, heat-insulating, and extruding the aluminum alloy cast rod, and during the extrusion process, performing a double-stage quenching treatment on the aluminum alloy cast rod to obtain an aluminum alloy profile substrate; S5. The aluminum alloy profile substrate is subjected to stretching and straightening, aging treatment, sandblasting, and anodizing treatment in sequence to obtain a low critical quenching rate aluminum alloy profile.

5. The preparation method according to claim 4, characterized in that: The quenching liquid comprises the following components in parts by weight: 1 to 3 parts of polyalkylene glycol, 5 to 9 parts of polyethylene glycol, and 88 to 94 parts of water.

6. The preparation method according to claim 4, characterized in that: The mass percentage concentration of the quenching liquid is (5-11)%.

7. The preparation method according to claim 4, characterized in that: S3 satisfies at least one of the following conditions: The temperature of the aluminum alloy liquid before refining is 720-740°C, and the refining time is 0.5-0.6h; The casting speed is 110-120 mm / min.

8. The preparation method according to claim 4, characterized in that: S5 satisfies at least one of the following conditions: The stretching rate of stretch straightening is 0.5-1.2%; The aging treatment includes: heating to 175-195°C at a rate of 100°C / h, then keeping the temperature for 3-6 hours, and cooling to below 40°C at a rate of 120°C / h after being taken out of the furnace.

9. An application of the low critical quenching rate aluminum alloy profile according to any one of claims 1 to 3 in manufacturing high-precision, thin-walled solar photovoltaic frames, characterized in that: The low critical quenching rate aluminum alloy profile has a critical quenching rate of 3 to 10°C / s and a tensile strength of 310 to 340 N / mm 2 , yield strength is 280~310N / mm 2 , elongation is 10-16%, Vickers hardness is 16-19HW, maximum intergranular corrosion depth is 19-29um, and the wall thickness of the thin-walled structure is 0.5-1.0mm.

Citation Information

Patent Citations

  • Ultrahigh-strength alloy steel and preparation method thereof

    CN116695026A

  • High-strength aluminum alloy profile for solar photovoltaic frame and preparation method of high-strength aluminum alloy profile

    CN118028665A

  • High strength aluminum alloy extruded material excellent in fatigue strength and motorcycle front fork outer tube material

    JP1996295977A

  • Production of al-mg-si alloy extruded material excellent in surface roughness

    JP1998298724A

  • Continuous solution quenching treatment method for aluminum alloy sheet for forming

    JP2003089860A

Cited By

  • High-strength aluminum alloy profile for automobile threshold beam and preparation method of high-strength aluminum alloy profile

    CN119194187A

  • Photovoltaic module frame, preparation method thereof and solar photovoltaic module

    CN119464857A

  • Aluminum alloy material suitable for photovoltaics and preparation method thereof

    CN119899963A

  • High-strength corrosion-resistant easy-to-process aluminum alloy profile for photovoltaic frame and preparation method thereof

    CN120290945A