Antioxidant 9Cr heat-resistant steel as well as preparation method and application thereof

By heat-treating 9Cr heat-resistant steel to generate Laves phase and spinel oxide, its anti-oxidation performance in the liquid lead-bismuth eutectic environment is improved, and the problem of insufficient anti-oxidation performance of 9Cr heat-resistant steel in the existing technology is solved. Extends the service life of materials and reduces operation and maintenance costs.

CN118814079APending Publication Date: 2024-10-22SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410811714.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing 9Cr heat-resistant steel has insufficient anti-oxidation performance in the liquid lead-bismuth eutectic environment, causing liquid metal corrosion and liquid metal embrittlement, affecting the power generation efficiency and operating life of nuclear power plants.

Method used

By heat treatment of 9Cr heat-resistant steel, the Laves phase (AB2 structure, A is Mo, W, B is Fe, Cr) is generated, spinel oxide is formed, the Cr content is increased, and a dense oxide film is formed to improve the anti-oxidation performance.

Benefits of technology

It can effectively reduce liquid metal corrosion, increase the service life of materials, significantly reduce the operation and maintenance costs of lead-bismuth fast reactors, and improve the oxidation resistance of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814079A_ABST
    Figure CN118814079A_ABST
Patent Text Reader

Abstract

The invention discloses antioxidant 9Cr heat-resistant steel as well as a preparation method and application thereof, and belongs to the technical field of metal materials. The crystal phase structure of the antioxidant 9Cr heat-resistant steel provided by the invention comprises a Laves phase. It is found that an intermetallic compound Laves phase is generated in the heat treatment process of the 9Cr heat-resistant steel, the Laves phase has good oxidation resistance, the oxidation-resistant 9Cr heat-resistant steel is obtained by introducing the Laves phase into the 9Cr heat-resistant steel, the oxidation resistance of the oxidation-resistant 9Cr heat-resistant steel is good, the liquid metal corrosion phenomenon can be effectively relieved, the service life of the material is prolonged, and the service life of the material is prolonged. The antioxidant 9Cr heat-resistant steel provided by the invention has wide application in preparation of reactor structure materials, especially lead-bismuth fast reactor structure materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and in particular relates to an anti-oxidation 9Cr heat-resistant steel and a preparation method and application thereof. Background Art

[0002] In the existing nuclear energy research, the research on lead-bismuth fast reactor (LBEFR) has attracted much attention. This reactor type uses liquid lead-bismuth eutectic (LBE) as coolant and spallation target and has excellent application performance. The metal structural materials used in the reactor are immersed in LBE, which will produce two important material degradation effects: liquid metal corrosion (LMC) and liquid metal embrittlement (LME). In liquid metal corrosion (LMC), it can be divided into full liquid metal corrosion and local liquid metal corrosion according to the corrosion range, and can be divided into oxidation, dissolution, and erosion according to the type of corrosion. When liquid Pb or LBE contains enough dissolved oxygen, an oxide film will form in situ on the steel surface. When the oxide film is thin, dense, defect-free, adherent, resistant to spontaneous spallation, and has a low metal / oxygen diffusivity at reactor-related temperatures, they are expected to protect the substrate material from further LMC. However, as the thickness of the oxide increases, due to the low thermal conductivity of the oxide, the heat transfer efficiency is reduced, the heat transfer performance is inhibited, and the energy loss is increased.

[0003] Candidate structural materials for lead-bismuth fast reactors (LBEFR) must operate reliably in very harsh environments where the performance of the materials may be degraded due to radiation-induced damage, liquid metal corrosion (LMC), liquid metal embrittlement (LME), stress, transmutation, nuclear reactions producing helium atoms, and a combination of all of the above effects. When nuclear power structural materials are exposed to liquid LBE, severe LMC degradation effects often lead to reduced power generation efficiency and shortened operating life of nuclear power plants. In LMC, pipeline damage caused by oxidation effects is particularly important, so research on the oxidation resistance of pipeline metals becomes particularly important.

[0004] There are some solutions that can mitigate the impact of LMC, such as reactor system parameter design, oxygen control system and material innovation (making new materials or adding coatings on existing materials). Regarding how to improve the oxidation resistance of 9Cr heat-resistant steel in LBE, some of the current mainstream methods have corresponding disadvantages. For example, the design of reactor operating parameters (temperature, pressure, etc.), the temperature control in the reactor is directly opposite to the economics of NPP. Whether in terms of thermal efficiency or in exploring new markets (for example, directly using the heat released by fission reactions to produce hydrogen), it is only economically feasible above a certain temperature threshold. Using active oxygen control systems to control the oxygen content in LBE to reduce oxidation of structural materials is another method, but it is currently difficult to control the oxygen potential in any part of the reactor system because the oxygen content will naturally decrease in gaps, dirt deposits, or closed areas filled with static LBE; logically, the structural materials in these areas will be affected by LMC (and possibly LME, as the reduction in oxide film thickness can hinder compact steel / HLM contact); at the same time, the production of oxygen sensors is also a major difficulty, as their external ceramic structures may crack due to stress in the liquid LBE, causing LBE to penetrate into the sensor, thereby affecting the use and detection of electrodes. Adding corrosion-resistant elements to structural materials to improve the oxidation resistance of steel is a goal that many existing research institutes are working hard to overcome. The current problem is that after adding corrosion-resistant or antioxidant elements, other properties of the material, such as mechanical properties, cannot be guaranteed. If an oxidation-resistant coating is added to the surface of the steel in contact with the LBE, more surface engineering problems will be faced, and the selection of coating equipment is also crucial.

[0005] 9Cr heat-resistant steel is recommended as a structural material for building lead-based reactors due to its good mechanical properties and excellent resistance to neutron irradiation. At present, the research on the oxidation resistance of 9Cr heat-resistant steel mainly focuses on the affinity of different elements contained in it to oxygen, aiming to analyze how elements such as Fe and Cr combine with oxygen, what kind of oxidation products are generated, whether the oxidation resistance can be improved by changing the content of alloy elements, and how to improve the oxidation resistance. In other words, most of the current research focuses on the resistance of the chemical properties of the elements themselves to oxidation. Summary of the invention

[0006] In order to overcome at least one of the problems existing in the above-mentioned prior art, one of the objects of the present invention is to provide an oxidation-resistant 9Cr heat-resistant steel, which has good oxidation resistance and can be used to prepare reactor structural materials.

[0007] A second object of the present invention is to provide a method for preparing the above-mentioned anti-oxidation 9Cr heat-resistant steel.

[0008] The third object of the present invention is to provide an application of the above-mentioned anti-oxidation 9Cr heat-resistant steel in the preparation of reactor structural materials.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] A first aspect of the present invention provides an anti-oxidation 9Cr heat-resistant steel, wherein the crystal phase structure of the anti-oxidation 9Cr heat-resistant steel includes a Laves phase.

[0011] In some specific embodiments of the present invention, the structural formula of the Laves phase is AB2; wherein A is Mo, W or a combination thereof, and B is Fe, Cr or a combination thereof.

[0012] In some specific embodiments of the present invention, the area fraction of the Laves phase is 0.5-1.2%.

[0013] In some specific embodiments of the present invention, there is spinel oxide at the interface of the Laves phase; the spinel oxide contains Cr element.

[0014] In some specific embodiments of the present invention, the Cr content of the spinel oxide is 32-47 wt.%.

[0015] In some specific embodiments of the present invention, the Cr content in the Laves phase is 7-15 wt.%.

[0016] The second aspect of the present invention provides a method for preparing the antioxidant 9Cr heat-resistant steel described in the first aspect of the present invention, comprising the following steps: heat-treating the 9Cr heat-resistant steel to obtain the antioxidant 9Cr heat-resistant steel.

[0017] In some specific embodiments of the present invention, the Cr content of the 9Cr heat-resistant steel is 8-9.5wt.%.

[0018] In some specific embodiments of the present invention, the Mo content of the 9Cr heat-resistant steel is 0.3-1.1 wt.%.

[0019] In some specific embodiments of the present invention, the W content of the 9Cr heat-resistant steel is 0-2wt.%.

[0020] In some specific embodiments of the present invention, the heat treatment is a heat aging treatment.

[0021] In some specific embodiments of the present invention, the temperature of the thermal aging treatment is 500-700°C.

[0022] In some specific embodiments of the present invention, the thermal aging treatment time is 100 to 50,000 hours.

[0023] In some specific embodiments of the present invention, W and / or Mo elements are added to the 9Cr heat-resistant steel before the heat treatment.

[0024] In some specific embodiments of the present invention, the added amount of the W element is 1 to 10 At.%.

[0025] In some specific embodiments of the present invention, the added amount of the W element is 1 to 10 At.%.

[0026] The third aspect of the present invention provides a use of the oxidation-resistant 9Cr heat-resistant steel described in the first aspect of the present invention in the preparation of reactor structural materials.

[0027] In some specific embodiments of the present invention, the reactor is a lead-based reactor; in some more specific embodiments of the present invention, the reactor is a lead-bismuth fast reactor (LBEFR).

[0028] The beneficial effects of the present invention are as follows: the present invention finds that 9Cr heat-resistant steel generates an intermetallic compound Laves phase during the heat treatment process, and the Laves phase has good anti-oxidation properties. The Laves phase is introduced into the 9Cr heat-resistant steel to obtain an anti-oxidation 9Cr heat-resistant steel, which has good anti-oxidation properties and can effectively reduce liquid metal corrosion and improve the service life of the material. The anti-oxidation 9Cr heat-resistant steel of the present invention is widely used in the preparation of reactor structural materials, especially lead-bismuth fast reactor structural materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 (a) and (b) are high-resolution TEM images of the Laves phase in the outer oxide layer of the steel sample in Example 1.

[0030] Figure 2 (a) and (b) are high-resolution TEM images of the Laves phase interface of the steel sample in Example 1.

[0031] Figure 3 The configurations of the Fe7Cr(110) surface after O atoms are adsorbed at different positions, where (a) is a top view of the adsorption site, and (b) to (d) are side views of the optimized configurations after O atoms are adsorbed on s1, s2, and s3, respectively.

[0032] Figure 4 The configurations of the Fe7CrW4 (0001) surface after O atoms are adsorbed at different positions, where (a) is a top view of the adsorption site; (b) to (d) are side views of the optimized configurations after O atoms are adsorbed on s1, s2, and s3, respectively.

[0033] Figure 5SEM images of P92 steel after heat aging treatment at 650°C for (a) 600 h, (b) 1200 h, (c) 2500 h, and (d) 5000 h.

[0034] Figure 6 This is the relationship between the Laves phase area fraction and the thermal aging treatment time.

[0035] Figure 7 This is the SEM image of P92 steel without heat aging treatment after being immersed in 550℃ liquid LBE for 1000h.

[0036] Figure 8 These are SEM images of P92 steel with a heat aging treatment time of 600 h and immersed in 550℃ liquid LBE for 1000 h. (a) and (b) are SEM images of the same sample at different positions.

[0037] Fig. 9 These are SEM images of P92 steel with a heat aging treatment time of 1200 h and immersed in 550℃ liquid LBE for 1000 h. (a) and (b) are SEM images of the same sample at different positions.

[0038] Fig.10 This is the SEM image of P92 steel with a heat aging treatment time of 2500h and immersed in 550℃ liquid LBE for 1000h.

[0039] Fig.11 These are SEM images of P92 steel with a heat aging treatment time of 5000 h and immersed in 550℃ liquid LBE for 1000 h. (a) and (b) are SEM images of the same sample at different positions.

[0040] Fig.12 This is a graph showing the relationship between the thickness of oxidation products of P92 steel at different thermal aging treatment times and the thermal aging treatment time.

[0041] Fig.13 This is the relationship between the area fraction of Laves phase and the thickness of oxidation products of P92 steel. DETAILED DESCRIPTION

[0042] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.

[0043] Regarding the terminology of the present invention, it should be noted that LBE: liquid lead bismuth eutectic (Pb 44.5 Bi 55.5 , wt.%); LBEFR: lead-bismuth fast reactor; LMC: liquid metal corrosion; LME: liquid metal embrittlement; SEM: scanning electron microscopy; EDS: energy dispersive X-ray spectroscopy; SAED: selected area electron diffraction; OOL: outer oxide layer; IOL: inner oxide layer; DO: dissolved oxygen (ppm, ppb, ppt); NPP: nuclear power plant

[0044] A first aspect of an embodiment of the present invention provides an anti-oxidation 9Cr heat-resistant steel, wherein the crystal phase structure of the anti-oxidation 9Cr heat-resistant steel includes a Laves phase.

[0045] Regarding the Laves phase, it is usually considered to be a harmful phase in steel due to its brittleness. Some studies have focused on its high temperature resistance, but there have been no reports on the effect of the precipitation of the Laves phase on the oxidation resistance of the material.

[0046] The research idea of ​​the present invention is different from the existing research that focuses on the influence of different elements in 9Cr heat-resistant steel on the affinity of oxygen. Instead, it is based on the influence of intermetallic compounds on the oxidation resistance of 9Cr heat-resistant steel. Through this new research idea, it was found that 9Cr heat-resistant steel produced an extremely strong oxidation-resistant intermetallic compound Laves phase during the heat treatment process (such as high-temperature LBE environment service process), and the Laves phase is beneficial to improving the oxidation resistance of 9Cr heat-resistant steel in high-temperature processes.

[0047] In some embodiments of the present invention, the structural formula of the Laves phase is AB2; wherein A is Mo, W or a combination thereof, and B is Fe, Cr or a combination thereof.

[0048] In some specific embodiments of the present invention, the structural formula of the Laves phase is expressed as (Fe, Cr) 2 (Mo, W).

[0049] It should be noted that in AB2 or (Fe,Cr)2(Mo,W), the sum of the amounts of Fe and Cr: the sum of the amounts of Mo and W = 2:1, and as long as the sum of the amounts of the substances satisfies this relationship, some elements may not exist. Taking Fe7CrW4 as an example, it satisfies the Laves phase structural formula AB2. Specifically, A is W, the number is 4, and B is a combination of Fe and Cr, the sum of the two is 8.

[0050] In some embodiments of the present invention, the area fraction of the Laves phase is 0.5-1.2%, with non-limiting examples being 0.6%, 0.8%, 1% or 1.1%.

[0051] The area fraction of the Laves phase refers to the area percentage occupied by the Laves phase on the cross section of the steel material. The present invention has found that the area fraction of the Laves phase in the LBEFR environment is strongly negatively correlated with the thickness of the oxide layer of 9Cr heat-resistant steel (such as P92 steel), that is, the larger the area fraction of the Laves phase, the thinner the surface oxide layer of 9Cr heat-resistant steel (such as P92 steel). This feature also reflects that the Laves phase can inhibit the oxidation of 9Cr heat-resistant steel under the operating conditions of the lead-bismuth fast reactor, thereby increasing the service life of the material and significantly reducing the operation and maintenance costs of the lead-bismuth fast reactor.

[0052] In some embodiments of the present invention, there is spinel oxide at the interface of the Laves phase; the spinel oxide contains Cr element; in some specific embodiments of the present invention, the spinel oxide is iron-chromium oxide.

[0053] In some embodiments of the present invention, the spinel oxide has a structural formula of Fe 3-x Cr x O4, x is 1 or 2.

[0054] In some embodiments of the present invention, the Cr content of the spinel oxide is 32-47 wt.%, with non-limiting examples being 35, 41 wt.%, or 44 wt.%.

[0055] Since O atoms are more likely to combine stably with Cr atoms, the spinel oxide at the interface of the Laves phase has a high Cr content, thereby forming a dense and more protective Cr-rich oxide film on the surface of the Laves phase interface, isolating the oxidation of the interior by O elements.

[0056] In some embodiments of the present invention, the Cr content in the Laves phase is 7-15 wt.%, with non-limiting examples being 8, 10 wt.% or 12 wt.%.

[0057] The second aspect of the embodiment of the present invention provides a method for preparing the anti-oxidation 9Cr heat-resistant steel described in the first aspect of the present invention, comprising the following steps: heat-treating the 9Cr heat-resistant steel to obtain the anti-oxidation 9Cr heat-resistant steel.

[0058] In the present invention, 9Cr heat-resistant steel refers to a heat-resistant F / M steel with a Cr content of about 9wt.% (e.g., 8-9.5wt.%), having a body-centered cubic (bcc) crystal structure, and exhibiting good ductility and fracture toughness, high thermal conductivity, low thermal expansion, and excellent resistance to radiation embrittlement and void expansion at high temperatures (usually up to 550-610°C).

[0059] In some embodiments of the present invention, the Cr content of the 9Cr heat-resistant steel is 8-9.5wt.%, non-limiting examples being 8.2wt.%, 8.5wt.%, 8.8wt.%, 9wt.% or 9.2wt.%.

[0060] In some embodiments of the present invention, the Mo content of the 9Cr heat-resistant steel is 0.3-1.1 wt.%, with non-limiting examples being 0.5 wt.%, 0.7 wt.%, 0.9 wt.% or 1 wt.%.

[0061] In some embodiments of the present invention, the W content of the 9Cr heat-resistant steel is 0-2wt.%, with non-limiting examples being 0wt.%, 0.5wt.%, 1wt.%, and 1.5wt.%.

[0062] In some specific embodiments of the present invention, the 9Cr heat-resistant steel is selected from P91 steel, P92 steel or a combination thereof.

[0063] In some embodiments of the present invention, the heat treatment is a heat aging treatment.

[0064] In some embodiments of the present invention, the temperature of the thermal aging treatment is 500-700°C; in some specific embodiments of the present invention, the temperature of the thermal aging treatment is 500-690°C; non-limiting examples are 550°C, 600°C or 650°C.

[0065] In some embodiments of the present invention, the heat aging treatment is performed in air.

[0066] Since the reactor of a lead-bismuth fast reactor is operated under a saturated oxygen concentration, and the normal atmospheric environment is a saturated oxygen environment, the thermal aging treatment carried out in air can simulate the saturated oxygen concentration required by the reactor of a lead-bismuth fast reactor.

[0067] After heat treatment, 9Cr heat-resistant steel (such as P92 steel) will produce a surface oxide layer. The surface oxide layer is generally a double-layer oxide layer, namely the outer oxide layer (OOL) and the inner oxide layer (IOL). There are some differences in the elements and structures of these two oxide layers.

[0068] In some embodiments of the present invention, the heat aging treatment time is 100 to 50,000 hours, non-limiting examples being 200 hours, 600 hours, 1,200 hours, 2,500 hours, 5,000 hours, 10,000 hours, 20,000 hours, 30,000 hours or 40,000 hours.

[0069] With the extension of thermal aging treatment time, the number and particle size of Laves phase increase accordingly. The area fraction of Laves phase is positively correlated with the thermal aging treatment time, and the thickness of oxidation product is negatively correlated with the thermal aging treatment time. It can be concluded that the area fraction of Laves phase is negatively correlated with the thickness of oxidation product. Therefore, with the extension of thermal aging treatment time, the area fraction of Laves phase increases, the thickness of oxidation product decreases, the oxidation resistance of material improves, and promoting the formation of Laves phase can improve the oxidation resistance of 9Cr heat-resistant steel.

[0070] In some embodiments of the present invention, W and / or Mo elements are added to the 9Cr heat-resistant steel before heat treatment.

[0071] The Laves phase is a brittle phase that will increase the yield strength and reduce the toughness of the alloy, but the elements such as W and Mo in the alloy can effectively improve the creep resistance of the alloy. High W and Mo elements are conducive to making the obtained oxidation-resistant 9Cr heat-resistant steel easier to generate Laves phase during service, thereby improving the oxidation resistance of the oxidation-resistant 9Cr heat-resistant steel and making it have a longer service life when used as a LBEFR structural material.

[0072] In some embodiments of the present invention, the added amount of the W element is 1 to 10 At.%, and non-limiting examples include 3 At.%, 5 At.%, 7 At.% or 9 At.%.

[0073] In some embodiments of the present invention, the added amount of the W element is 1 to 10 At.%, and non-limiting examples include 3 At.%, 5 At.%, 7 At.% or 9 At.%.

[0074] A third aspect of an embodiment of the present invention provides a use of the oxidation-resistant 9Cr heat-resistant steel described in the first aspect of the present invention in the preparation of reactor structural materials.

[0075] In some embodiments of the present invention, the reactor is a lead-based reactor; in some more specific embodiments of the present invention, the reactor is a lead-bismuth fast reactor (LBEFR).

[0076] The present invention is further described below in conjunction with specific embodiments.

[0077] Example 1

[0078] The high temperature and long heat aging treatment of 9Cr heat-resistant steel specifically includes the following steps:

[0079] A high-temperature autoclave was designed and built independently to simulate the temperature (480-570℃) and saturated oxygen concentration of liquid lead-bismuth environment in a lead-bismuth fast reactor. The P92 steel sample after high-temperature long heat aging treatment (650℃ heat aging treatment for 10,000 hours) was placed in the lead-bismuth fast reactor for 1,000 hours of immersion treatment. After the sample was soaked, it was taken out and washed with a solution of alcohol, hydrogen peroxide and acetic acid to remove the surface lead and bismuth, and then embedded in metal inlay powder or epoxy resin, and then polished to obtain the treated steel sample. The morphology of the treated steel sample was characterized and analyzed.

[0080] Figure 1 High-resolution TEM image (a) and SAED image (b) of the Laves phase in the inner oxide layer (IOL) of the steel sample in Example 1, wherein the area in (b) is selected from the circle in (a). Figure 2 The high-resolution TEM image (a) and SAED image (b) of the Laves phase interface of the steel sample in Example 1, wherein the dotted line in (a) is the boundary between the Laves phase and the inner oxide layer (IOL), and the area in (b) is selected from the box in (a). After heat treatment in the range of 500-690°C, an intermetallic compound Laves phase will precipitate in the 9Cr heat-resistant steel. Figures 1-2 It can be seen that the bright particles (i.e. Laves phase) precipitated during the long heat aging treatment of 9Cr heat-resistant steel are scattered in the inner oxide layer (IOL) and the matrix. When SAED is performed on the interior of the Laves phase in the inner oxide layer, it is found that it still maintains a close-packed hexagonal (Fe, Cr) 2 (Mo, W) intermetallic compound structure, proving that it is not oxidized inside. EDS energy spectrum detection and electron diffraction analysis at the Laves phase boundary show that there is a layer of Fe with a thickness of about 10 to 20 nm at the boundary. 3-x Cr x The oxide film with O4 spinel structure is consistent with the structure of the inner oxide layer.

[0081] In addition, oxidation experiments were carried out on the single metals for the relevant elements in the Laves phase. Except for the samples being converted into four single metals, Fe, Cr, W, and Mo, the rest of the experimental steps were the same. In the SEM images, it can be observed that the pure metals Fe, W, and Mo have poor oxidation resistance in the LBE solution, and a thicker oxide layer appears on the surface. Pure Cr has stronger oxidation resistance, with an oxide layer of only about 100 nm thick on the surface, but the thickness is still about 5 times higher than the oxide layer on the surface of the Laves phase, and oxygen will still penetrate deeper into the matrix along the dislocation channel. Therefore, it can be concluded that the oxidation resistance of the Laves phase is not caused by the element itself.

[0082] Example 2

[0083] In order to explore the reasons why the Laves phase has extremely strong antioxidant properties, a computational simulation analysis was carried out, as follows:

[0084] The exchange-correlation energy is calculated based on the projected augmented wave (PAW) algorithm of Vienna Ab initio Simulation Package (VASP) and the generalized gradient approximation (GGA). In order to reduce the number of plane waves required for the calculation, the PAW calculation method is introduced with a cutoff energy of 500 eV. The integral of the Brillouin zone is generated using the Gamma method on the k-point grid. The convergence criteria for force and energy are and 10 -5 eV. The Methfessel-Paxton method was used to determine the Fermi level broadening, and the broadening width was 0.05 eV. The adsorption of oxygen atoms on the surface was calculated using the following formula.

[0085]

[0086] Where E ad represents the adsorption energy, is the total energy of the surface of the adsorbed atom, E slab is the total energy of a clean surface without any atoms adsorbed, and E adatom is in a The energy of the isolated atom calculated in the box. E ad The lower (more negative), the more stable the adsorption system is and the easier it is for adsorbed atoms to be attached to its surface.

[0087] Firstly, the Fe-Cr binary alloy of FCC was constructed. Its surface model consists of 4 atomic layers, including 4 Cr atoms and 28 Fe atoms, and the vacuum layer is The doping of Cr atoms was achieved by using MS disorder spectrum method, and the structure with the lowest energy was selected as the calculation object. The close-packed plane (110) was selected as the exposed surface to calculate the adsorption of oxygen atoms on it. Figure 3That is, the configuration of the Fe7Cr(110) surface after O atoms are adsorbed at different positions, where (a) is the top view of the adsorption site, and (b) to (d) are the side views of the optimized configuration after O atoms are adsorbed on s1, s2, and s3, respectively. Figure 3 As shown in (a), three adsorption sites s1, s2, and s3 are selected on the Fe7Cr(110) surface. The adsorption energy and bond length data are shown in Table 1. Figure 3 As can be seen in (b) and Table 1, O atoms pull the bonded Cr atoms away from the surface, which may indicate that the bond between Cr atoms and O atoms is stronger; Figure 3 Middle (c), Figure 3 It can be seen from (d) and Table 1 that when adsorbed at the s2 and s3 sites, the O atoms that were originally only located above the Fe atoms are all combined with the Cr atoms after optimization, which also shows that O atoms tend to combine with Cr atoms.

[0088] Table 1 Adsorption energies and corresponding bond lengths of O atoms at different positions on the Fe7Cr(110) surface

[0089] Secondly, the HCP Fe7CrW4 was constructed to match the Laves phase element ratio ((Fe,Cr)2W), which contains 4 Cr atoms, 28 Fe atoms, and 16 W atoms. The vacuum layer was then formed, and the close-packed surface (0001) terminated with Cr atoms was selected as the exposed surface. Figure 4 The configurations of the Fe7CrW4(0001) surface after O atoms are adsorbed at different positions, where (a) is a top view of the adsorption site; (b) to (d) are side views of the optimized configurations after O atoms are adsorbed on s1, s2, and s3, respectively. Figure 4 It can be seen that, similar to the adsorption of O atoms on the Fe7Cr surface, O atoms that are initially higher than Fe atoms are combined with Cr atoms after adsorption, which further reflects that O has a stronger affinity for Cr. The adsorption energy and bond length are shown in Table 2. It can be found that the absolute value of the adsorption energy of O atoms on the Fe7CrW4 (0001) surface has reached 10 eV, which is much larger than the adsorption energy on the Fe7Cr (110) surface. From an energy point of view, O atoms are easily adsorbed on the Fe7CrW4 surface, and O atoms are more stable when adsorbed on the Laves phase surface, making it difficult for them to diffuse along the Laves interface.

[0090] Table 2 Adsorption energy and corresponding bond length of O atoms at different sites on the Fe7CrW4(0001) surface

[0091]

[0092]

[0093] At the same time, O atoms are more likely to combine stably with Cr atoms, thus forming a dense and more protective Cr-rich oxide film on the surface of the Laves phase, isolating the oxidation of the interior by O elements. This also explains why the spinel oxide film at the Laves phase interface has a higher Cr content (the Cr content inside the Laves phase is about 7wt.%, while the Cr content at its surface oxide film can reach 47wt.%). In addition, there are relatively few dislocations inside the Laves phase crystal, and it is difficult for O atoms to diffuse through the preferential oxidation channel. It is precisely because of the above reasons that the interior of the Laves phase exhibits extremely strong oxidation resistance.

[0094] Example 3

[0095] In view of the anti-oxidation characteristics of Laves phase, we further explored how to reduce the intrusion of 9Cr heat-resistant steel matrix. After reading the literature and analyzing the existing materials, it was found that long-term high-temperature (500-690℃) heat aging treatment can promote the generation of Laves phase. The P92 sample was made into several metal blocks with a size of 10×10×5mm by wire cutting, divided into 5 parts by quantity, and placed in a muffle furnace for heat aging treatment at 600℃. The first sample was taken out after 600h of heat aging treatment, the second sample was taken out after 1200h, the third sample was taken out after 2500h, and the last sample was taken out after 5000h.

[0096] The four samples were observed by SEM. Figure 5 As shown in the figure, firstly, it was observed that the amount and particle size of Laves phase increased with the extension of thermal aging treatment time. Secondly, through comparison, it was found that the formation position of Laves phase also changed with the thermal aging treatment time. In the SEM images of 600h and 1200h, it was observed that Laves phase precipitated and grew along the original austenite grain boundary. However, in the samples of 2500h and 5000h, it was observed that in addition to the Laves phase at the original austenite grain boundary, a large amount of Laves phase was also precipitated in the martensite lath in the matrix.

[0097] The area fraction of the Laves phase of different samples was tested. The specific test process was as follows: 3 parallel samples were set for each sample, all of which were polished, and dozens of photos were taken under SEM. The area fraction of the Laves phase was calculated for each photo using ImageJ software. Finally, the data obtained were averaged after removing the maximum and minimum values ​​to obtain the area fraction of the Laves phase of each sample. The relationship between the ratio of the Laves phase area to the total area (area fraction) and the heat aging treatment time was made as follows: Figure 6 , which more intuitively shows that during the entire thermal aging treatment process, the area fraction of the Laves phase is always positively correlated with the thermal aging treatment time.

[0098] Subsequently, the above four samples plus one sample without thermal aging treatment were placed in a high-temperature autoclave simulating the environment of a lead-bismuth fast reactor and immersed in a 550℃ LBE environment for 1000h. After being taken out, the surface morphology was observed. The SEM image of the sample with thermal aging treatment for 0h (without thermal aging treatment) is as follows: Figure 7 , SEM images of samples treated with heat for 600h are as follows: Figure 8 , SEM of the sample treated with heat for 1200h is Fig. 9 , SEM of the sample treated with heat for 2500h is Fig.10 , SEM of the sample treated with heat for 5000h is Fig.11 Through comparative observation, it was found that as the thermal aging treatment time increased from 0h to 5000h, the thickness of the oxidation product on the surface of P92 steel also decreased from 24μm to 10.6μm.

[0099] Establish the relationship between thermal aging treatment time and oxide film thickness, such as Fig.12 It is found that the thickness of the oxidation product is negatively correlated with the thermal aging treatment time. Since the Laves phase area fraction is positively correlated with the thermal aging treatment time, it can be concluded that the Laves phase area fraction is negatively correlated with the thickness of the oxidation product. In order to draw a more intuitive conclusion, a relationship diagram between the oxide film thickness and the Laves phase area fraction is made, as shown in Fig.13 As shown in the figure, the coefficient of determination (R 2 =0.951) intuitively illustrates that the larger the area fraction of the Laves phase, the stronger the oxidation resistance of 9Cr heat-resistant steel. Through literature review, it is concluded that the diffusion of oxygen is generally not uniform, and it will preferentially diffuse along grain boundaries, dislocations and nanocavities. These diffusion areas are often preferentially oxidized, causing serious corrosion to the metal. Combined with SEM observation, it is found that the precipitated Laves phase is mainly distributed on the preferential diffusion path of oxygen. Because of the super oxidation resistance of the Laves phase, it hinders the diffusion of oxygen along the grain boundaries. It is further concluded that the Laves phase can improve the oxidation resistance of 9Cr heat-resistant steel.

[0100] Because the operating temperature of LBEFR is between 480 and 570°C, its structural material 9Cr heat-resistant steel is also equivalent to undergoing thermal aging treatment during the operation of the nuclear power plant. Because this temperature is just within the temperature range of the Laves phase, the service life of 9Cr heat-resistant steel may be longer than the predicted service life. This discovery increases the replacement cycle of 9Cr heat-resistant steel in nuclear power plants, which can reduce the number of replacements and reduce maintenance costs over a long period of time.

[0101] At the same time, adding an appropriate amount (1-10 At.%) of W and / or Mo alloy elements to 9Cr heat-resistant steel makes it easier to generate Laves phase during service, and the service life of LBEFR structural materials is further improved.

[0102] The present invention breaks through the idea of ​​using oxidation-resistant elements to improve the oxidation resistance of the matrix, and pioneers a method of improving the oxidation resistance by improving the lattice structure. It also conducts a more in-depth study on the oxidation corrosion behavior of 9Cr heat-resistant steel in the LBE environment, and at the same time finds a kind of intermetallic compound with high oxidation resistance in the matrix: Laves phase. It is also verified that the Laves phase can reduce the oxidation of 9Cr heat-resistant steel. At the same time, it is proposed to add W and Mo to make the material generate Laves phase, and improve the oxidation resistance of the material through the Laves phase. The method of the present invention has many advantages. In addition to not changing the intrinsic structure and performance, the addition of W and Mo can also improve the creep resistance of steel. At the same time, compared with the existing coating processing technology, it is simpler and suitable for large-scale production.

[0103] In summary, the present invention finds that 9Cr heat-resistant steel generates an intermetallic compound Laves phase during the heat treatment process, and the Laves phase has good anti-oxidation properties. The Laves phase is introduced into the 9Cr heat-resistant steel to obtain an anti-oxidation 9Cr heat-resistant steel with good anti-oxidation properties. The steel can effectively reduce liquid metal corrosion and improve the service life of the material. The anti-oxidation 9Cr heat-resistant steel of the present invention is widely used in the preparation of reactor structural materials, especially lead-bismuth fast reactor structural materials.

Claims

1. An anti-oxidation 9Cr heat-resistant steel, characterized in that: The crystalline phase structure of the anti-oxidation 9Cr heat-resistant steel includes Laves phase.

2. The oxidation-resistant 9Cr heat-resistant steel according to claim 1, characterized in that: The structural formula of the Laves phase is AB2; Wherein, A is Mo, W or a combination thereof, and B is Fe, Cr or a combination thereof.

3. The oxidation-resistant 9Cr heat-resistant steel according to claim 1, characterized in that: The area fraction of the Laves phase is 0.5-1.2%.

4. The oxidation-resistant 9Cr heat-resistant steel according to claim 1, characterized in that: There is spinel oxide at the interface of the Laves phase; the spinel oxide contains Cr element; preferably, the Cr content of the spinel oxide is 32-47wt.%; And / or, the Cr content in the Laves phase is 7-15wt.%.

5. The method for preparing the oxidation-resistant 9Cr heat-resistant steel according to any one of claims 1 to 4, characterized in that: The following steps are involved: The 9Cr heat-resistant steel is heat-treated to obtain the anti-oxidation 9Cr heat-resistant steel.

6. The preparation method according to claim 5, characterized in that: The Cr content of the 9Cr heat-resistant steel is 8-9.5wt.%; And / or, the Mo content of the 9Cr heat-resistant steel is 0.3-1.1wt.%; And / or, the W content of the 9Cr heat-resistant steel is 0-2wt.%.

7. The preparation method according to claim 5, characterized in that: The heat treatment is a heat aging treatment; preferably, the temperature of the heat aging treatment is 500-700° C.; and / or the time of the heat aging treatment is 100-50000 h.

8. The preparation method according to claim 5, characterized in that: Before the heat treatment, W and / or Mo elements are added to the 9Cr heat-resistant steel.

9. The preparation method according to claim 8, characterized in that: The added amount of the W element is 1 to 10 At.%; And / or, the added amount of the W element is 1 to 10 At.%.

10. Use of the oxidation-resistant 9Cr heat-resistant steel according to any one of claims 1 to 4 in the preparation of reactor structural materials.