Method for measuring low-content titanium, molybdenum and tungsten in stainless steel

Through inductively coupled plasma mass spectrometry, combined with nitric acid-hydrochloric acid dissolution and atomization technology, the accuracy problem of detecting low-content titanium, molybdenum, and tungsten elements in stainless steel has been solved, and an accurate determination method has been realized in the metallurgical industry to meet production needs. .

CN118817818AInactive Publication Date: 2024-10-22BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202410908291.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to accurately measure the low content of titanium, molybdenum and tungsten elements in stainless steel with existing technology, and conventional inductively coupled plasma atomic emission spectrometry has poor detection results.

Method used

Inductively coupled plasma mass spectrometry is used to introduce the sample into the mass spectrometer through nitric acid-hydrochloric acid dissolution and atomization technology. Combined with the working curve of the known concentration standard material, the mass signal intensity of the element to be measured is measured. The applicable range is titanium 0.00001% ~ 0.010 %, molybdenum 0.00001% to 0.010%, tungsten 0.00001% to 0.010%.

Benefits of technology

The accurate determination of titanium, molybdenum and tungsten element content in stainless steel has been achieved. The method is accurate and practical, and is suitable for applications in the metallurgical industry and related scientific research institutions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for measuring low-content titanium, molybdenum and tungsten in stainless steel, which comprises the following steps: weighing a certain amount of sample, dissolving the sample with nitric acid-hydrochloric acid, transferring into a volumetric flask, fixing the volume, and shaking uniformly; atomizing the solution, introducing the atomized solution into an inductively coupled plasma mass spectrometer, and measuring the intensity of a mass signal of the element to be measured; and finally, outputting the concentration of the corresponding element in the substance to be detected according to the working curve of the standard substance with known concentration. The invention aims to provide a method for measuring low-content titanium, molybdenum and tungsten in stainless steel, and the method is used for production practice and is an effective, accurate and practical method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical analysis, and in particular relates to a method for determining low-content titanium, molybdenum and tungsten in stainless steel. Background Art

[0002] Stainless steel products are widely used in different fields due to their good corrosion resistance. In order to ensure that the performance of the products is qualified, the content of each element must be accurately tested. Stainless steel mainly contains elements such as iron, chromium and nickel. The main alloying element in stainless steel is chromium, which accounts for about 16-25%, and it is the main element that makes stainless steel corrosion-resistant. Another important alloying element in stainless steel is nickel, which promotes the material's higher strength, good plasticity and toughness, and improves the material's hot and cold processing. In addition, stainless steel also contains other alloying elements, such as molybdenum, titanium, tungsten, etc. Although the content is not high, it plays a decisive role in the physical properties and corrosion resistance of the corresponding stainless steel. For example, molybdenum is an indispensable element in 316L, 2205, 2507, 904L, and 317L stainless steel. Titanium is an indispensable element in the material content of 316Ti and 321 stainless steel. The role of tungsten in stainless steel is mainly to increase hardness and strength. Inductively coupled plasma emission mass spectrometry has the advantages of high sensitivity, wide linear range, multi-element analysis, high selectivity, and rapid analysis, and has been widely used in various fields of analysis and detection. The content of titanium, molybdenum, and tungsten in some varieties of stainless steel is relatively low, and conventional inductively coupled plasma atomic emission spectrometry cannot accurately determine their content. Based on the above situation, we have invented a method for determining low-content titanium, molybdenum, and tungsten in stainless steel. Summary of the invention

[0003] In order to control the quality of stainless products, the purpose of the present invention is to provide a method for determining low content of titanium, molybdenum and tungsten in stainless steel. This method has been used in production practice and is an effective, accurate and practical method.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The invention discloses a method for determining low content of titanium, molybdenum and tungsten in stainless steel. The method comprises the following steps: weighing a certain amount of sample, dissolving the sample with nitric acid-hydrochloric acid, transferring the sample to a volumetric flask, and shaking the flask after constant volume; atomizing the solution and introducing it into an inductively coupled plasma mass spectrometer to determine the intensity of the mass signal of the element to be determined; and finally outputting the concentration of the corresponding element in the substance to be determined through the working curve of a standard substance with known concentration.

[0006] Furthermore, when determining Ti:

[0007] Weigh 0.1000g sample into a 250mL quartz beaker, add 2mL HNO3 and 6mL HCL, dissolve at low temperature, add 2mL perchloric acid to continue dissolving and fuming until wet salt, remove, add 2mL HCL to dissolve the salts, transfer to a 100mL plastic volumetric flask, make up to volume, shake well, and measure using inductively coupled plasma mass spectrometry.

[0008] Furthermore, when determining Mo and W:

[0009] Weigh 0.1000g sample into a 250mL polytetrafluoroethylene beaker, add 2mL HNO3, 6mL HCL, and 2mL HF respectively, dissolve at low temperature, remove, transfer to a 100mL plastic volumetric flask, make up to volume with high-purity water, mix well, and determine by inductively coupled plasma mass spectrometry; when the mass-to-charge ratio of the element is less than 56, 6ppb Sc is used as the internal standard, and when the mass-to-charge ratio is greater than 56, 10ppb Cs and 6ppb Rh are used as internal standards.

[0010] Furthermore, drawing the working curve includes:

[0011] In 7 100mL plastic volumetric flasks, 10mL (1+1+3) HCL, HNO3 mixed acid, 2mL HF, and different amounts of Ti, Mo, and W element standard solutions were added respectively to prepare a series of standard solutions, which were equivalent to 0.00%, 0.00002%, 0.00005%, 0.0001%, 0.0005%, 0.001%, 0.005, and 0.01% Ti, Mo, and W element mass fractions in 0.1000g of the sample; the working curve was plotted using plasma mass spectrometry with mass fraction as the abscissa and intensity as the ordinate; when the mass-to-charge ratio of the element was less than 56, 6ppb Sc was used as the internal standard, and when the mass-to-charge ratio was greater than 56, 10ppb Cs and 6ppb Rh could be used as the internal standard.

[0012] Furthermore, the measurement range is: Ti: 0.00001% to 0.010%; Mo: 0.00001% to 0.010%; W: 0.00001% to 0.010%.

[0013] Compared with the prior art, the beneficial technical effects of the present invention are:

[0014] The method of the present invention has been used in production practice, and the measurement result is accurate. It is an effective and practical method and can be promoted and applied in the metallurgical industry and related scientific research institutes. DETAILED DESCRIPTION

[0015] A method for determining low content of titanium, molybdenum and tungsten in stainless steel, comprising: 1. Range

[0016] This method specifies the determination of titanium, molybdenum and tungsten content in stainless steel by inductively coupled plasma mass spectrometry. Determination range: Ti: 0.00001% to 0.010%; Mo: 0.00001% to 0.010%; W: 0.00001% to 0.010%.

[0017] 2 Method Summary

[0018] Weigh a certain amount of sample, dissolve it with nitric acid-hydrochloric acid, transfer it to a 100mL volumetric flask, and shake it to volume. Atomize the solution and introduce it into the inductively coupled plasma mass spectrometer to measure the intensity of the mass signal of the element to be measured. Finally, output the concentration of the corresponding element in the substance to be measured through the working curve of the known concentration standard substance.

[0019] 3 Reagents and materials

[0020] 3.1 Hydrochloric acid, ρ about 1.19 g / mL

[0021] 3.2 Nitric acid, ρ about 1.42 g / mL

[0022] 3.3 Perchloric acid, ρ1.67 g / mL

[0023] 3.4 Hydrofluoric acid, ρ1.15 g / mL

[0024] 3.5 Titanium, molybdenum, and tungsten standard solutions, 1000 μg / mL

[0025] 4. Main instruments

[0026] 4.1 Thermo Fisher Scientific Inc., i CP RQ plasma mass spectrometer.

[0027] 4.2 The mass numbers of the elements to be measured are: titanium 46; molybdenum 96; tungsten 184.

[0028] 5 Analysis steps

[0029] 5.1 Sample quantity

[0030] Weigh 0.1000g of the sample, accurate to 0.0002g.

[0031] 5.2 Determination steps

[0032] 5.2.1Ti

[0033] Weigh 0.1000g sample into a 250mL quartz beaker, add 2mL HNO3 and 6mL HCL, dissolve at low temperature, add 2mL perchloric acid to continue dissolving and fuming until wet salt, remove, add 2mL HCL to dissolve the salts, transfer to a 100mL plastic volumetric flask, make up to volume, shake well, and measure using inductively coupled plasma mass spectrometry.

[0034] 5.2.2Mo, W

[0035] Weigh 0.1000g of sample into a 250mL polytetrafluoroethylene beaker, add 2mL HNO3, 6mL HCL, and 2mL HF respectively, dissolve at low temperature, remove, transfer to a 100mL plastic volumetric flask, make up to volume with high-purity water, mix well, and measure using an inductively coupled plasma mass spectrometer. When the mass-to-charge ratio of the element is less than 56, 6ppb Sc is used as the internal standard, and when the mass-to-charge ratio is greater than 56, 10ppb Cs and 6ppb Rh can be used as internal standards.

[0036] 5.3 Curve drawing

[0037] In 7 100mL plastic volumetric flasks, add 10mL (1+1+3) HCL, HNO3 mixed acid, 2mL HF, and different amounts of Ti, Mo, and W element standard solutions to prepare a series of standard solutions, which are equivalent to 0.00%, 0.00002%, 0.00005%, 0.0001%, 0.0005%, 0.001%, 0.005, and 0.01% of the mass fraction of Ti, Mo, and W in 0.1000g of the sample. The plasma mass spectrometry method is used to determine the mass fraction as the horizontal axis and the intensity as the vertical axis to draw the working curve. When the mass-to-charge ratio of the element is less than 56, 6ppb Sc is used as the internal standard. When the mass-to-charge ratio is greater than 56, 10ppb Cs and 6ppb Rh can be used as the internal standard.

[0038] 6 Results and discussion

[0039] 6.1 Accuracy Experiment

[0040] Weigh the stainless steel standard samples respectively and carry out the test experiment according to this method. The results are shown in Table 1:

[0041] Table 1 Accuracy of measurement results (%)

[0042] Elements to be measured 304 detection value 304 value 304SQ test value 304SQ standard value Ti 0.0022 0.0022 0.0016 0.0016 Mo 0.00098 0.0010 0.00097 0.0010 W 0.00051 0.0005 0.00076 0.0008

[0043] From the data in the table, we can see that the detection method has a very high accuracy.

[0044] 6.2 Precision experiment

[0045] Weigh 11 portions of 304 stainless steel standard samples and perform precision tests according to the above experimental method. The test results are shown in Table 2:

[0046] Table 2 Determination results precision table (%)

[0047] Elements to be measured average value Standard Deviation RSD Ti 0.0022 0.0031% 1.38% Mo 0.00098 0.0004% 0.41% W 0.00050 0.0004% 0.86%

[0048] The above data show that the detection method has good precision.

[0049] 7 Conclusion

[0050] The method can accurately determine the content of titanium, molybdenum and tungsten in stainless steel. The method is simple to operate and easy to master, and can meet production needs.

[0051] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for determining low content of titanium, molybdenum and tungsten in stainless steel, characterized by: Weigh a certain amount of sample, dissolve it with nitric acid-hydrochloric acid, transfer it to a volumetric flask, and shake it evenly after adjusting the volume; atomize the solution and introduce it into the inductively coupled plasma mass spectrometer to measure the intensity of the mass signal of the element to be measured; finally, output the concentration of the corresponding element in the substance to be measured through the working curve of the known concentration standard substance.

2. The method for determining low content of titanium, molybdenum and tungsten in stainless steel according to claim 1, characterized in that: When measuring Ti: Weigh 0.1000g sample into a 250mL quartz beaker, add 2mL HNO3 and 6mL HCL, dissolve at low temperature, add 2mL perchloric acid to continue dissolving and fuming until wet salt, remove, add 2mL HCL to dissolve the salts, transfer to a 100mL plastic volumetric flask, make up to volume, shake well, and measure using inductively coupled plasma mass spectrometry.

3. The method for determining low content of titanium, molybdenum and tungsten in stainless steel according to claim 1, characterized in that: When measuring Mo and W: Weigh 0.1000g sample into a 250mL polytetrafluoroethylene beaker, add 2mL HNO3, 6mL HCL, and 2mL HF respectively, dissolve at low temperature, remove, transfer to a 100mL plastic volumetric flask, make up to volume with high-purity water, mix well, and determine by inductively coupled plasma mass spectrometry; when the mass-to-charge ratio of the element is less than 56, 6ppb Sc is used as the internal standard, and when the mass-to-charge ratio is greater than 56, 10ppb Cs and 6ppb Rh are used as internal standards.

4. The method for determining low content of titanium, molybdenum and tungsten in stainless steel according to claim 1, characterized in that: Drawing a working curve includes: In 7 100mL plastic volumetric flasks, 10mL (1+1+3) HCL, HNO3 mixed acid, 2mL HF, and different amounts of Ti, Mo, and W element standard solutions were added respectively to prepare a series of standard solutions, which were equivalent to 0.00%, 0.00002%, 0.00005%, 0.0001%, 0.0005%, 0.001%, 0.005, and 0.01% Ti, Mo, and W element mass fractions in 0.1000g of the sample; the working curve was plotted using plasma mass spectrometry with mass fraction as the abscissa and intensity as the ordinate; when the mass-to-charge ratio of the element was less than 56, 6ppb Sc was used as the internal standard, and when the mass-to-charge ratio was greater than 56, 10ppb Cs and 6ppb Rh could be used as the internal standard.

5. The method for determining low content of titanium, molybdenum and tungsten in stainless steel according to claim 1, characterized in that: Measurement range: Ti: 0.00001%~0.010%; Mo: 0.00001%~0.010%; W:0.00001%~0.010%。

Citation Information

Patent Citations

  • Method for measuring Ti content in low-carbon ferrophosphorus

    CN101750406A

  • Method for measuring content of Al, Ti and Ca in low-carbon silicon iron

    CN101750407A

  • Inductively coupled plasma mass spectrometry used for determining trace aluminum molybdenum vanadium titanium niobium in silicon steel

    CN104614434A

  • Method for measuring content of tungsten and molybdenum in ore

    CN106018384A

  • Method for detecting migration of 11 elements in stainless steel food container

    CN109613103A

Cited By

  • Method for detecting content of tungsten element in stainless steel

    CN120890965A

  • Method for measuring yttrium in medium-low alloy steel

    CN122238461A