Grain boundary diffusion method of light rare earth-based diffusion source based on protective atmosphere electric spark deposition
By depositing a light rare earth-based alloy coating on sintered NdFeB magnetic materials using a protective atmosphere spark, the problem of oxidation and high cost of light rare earth-based diffusion sources is solved, the coercive force and diffusion efficiency of the magnetic materials are improved, and the cost is achieved reduced effect.
Patent Information
- Application Number
- CN202411021986.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Light rare earth-based diffusion sources are easily oxidized during the pulping process, resulting in low diffusion efficiency and depth, and the existing coating process is high-cost and low-efficiency.
The grain boundary diffusion method based on the light rare earth-based diffusion source of protective atmosphere electric spark deposition is adopted. By plating the light rare earth-based alloy coating on the magnetic material substrate, and performing densification sintering and tempering treatment, inert gas protection is used to avoid oxidation. Control coating parameters such as electrode diameter, rotation speed, deposition voltage and frequency to improve coating quality and efficiency.
It effectively prevents the oxidation of light rare earth-based diffusion sources, improves the coercive force of the magnetic material matrix, improves diffusion efficiency, reduces production costs, and achieves efficient improvement of magnet performance.
Smart Images

Figure CN118824718A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth permanent magnet materials, and in particular to a grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electric spark deposition. Background Art
[0002] Sintered NdFeB permanent magnet materials have high saturation magnetization and high coercivity, and are indispensable materials for various motors and brakes. In recent years, the popularity of hybrid vehicles and electric vehicles has increased year by year, and the market demand for sintered NdFeB permanent magnet materials has also increased.
[0003] Grain boundary diffusion technology is currently a common method used to improve the coercive force of magnets in sintered NdFeB permanent magnet materials. Studies have shown that the demagnetization process of NdFeB magnets originates from the nucleation and growth of antimagnetic domains at the surface defects of NdFeB grains and in low anisotropy field areas. Through grain boundary diffusion, a shell layer with a high anisotropy field will be formed on the surface of the hard magnetic grains in the magnet, which will inhibit the nucleation of antimagnetic domains and thus improve the coercive force of the magnet. Grain boundary diffusion requires a diffusion source coating to be applied to the surface of the magnet first. Commonly used processes are magnetron sputtering, screen printing, and spraying.
[0004] As the price of heavy rare earth elements continues to rise, light rare earth-based alloy diffusion sources are gradually coming into people's view. Unlike heavy rare earth alloy diffusion sources, light rare earth-based alloy diffusion sources are very chemically active and are very easy to oxidize during the pulping process. After being coated and diffused by screen printing and spraying processes, the diffusion efficiency and diffusion depth of light rare earth elements are often low; although the coating is not easy to oxidize after coating using the magnetron sputtering process, the process is costly and the coating efficiency is low. Therefore, how to effectively inhibit the oxidation of light rare earth-based diffusion sources, improve their diffusion efficiency and diffusion depth, and reduce the use of diffusion sources has become an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electric spark deposition, which has the effects of preventing oxidation of the light rare earth-based diffusion source, effectively improving the coercive force of the magnetic material matrix, improving diffusion efficiency and reducing costs.
[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition, comprising the following steps:
[0007] S1: orienting sintered NdFeB magnetic powder with an average particle size of 2-10 μm in a magnetic field of 1.4-2 T, and pressing it into a green compact at a pressure of 10-20 MPa using an isostatic press;
[0008] S2: The green body obtained by pressing in S1 is sintered at 950-1010℃ for 1-3h to obtain a density of 6.5-7.0g / cm 3 Semi-densified magnetic material matrix;
[0009] S3: Using a light rare earth alloy as an anode electrode and a semi-densified magnetic material substrate as a cathode electrode, a light rare earth alloy coating is plated on the magnetic material substrate by electric spark deposition under the protection of an inert gas to obtain a semi-densified magnet sample containing a light rare earth alloy coating;
[0010] S4: densification sintering is performed on the semi-densified magnet sample containing the light rare earth alloy coating obtained in S3, and the sintering temperature is controlled to be 1030-1090°C and the sintering time is 2-5h;
[0011] S5: The densified magnet sample containing the light rare earth alloy coating obtained by sintering in S4 is tempered, and the tempering temperature is controlled to be 500-800° C., and the tempering time is controlled to be 3-8 hours.
[0012] The present invention is further configured as follows: the composition of the light rare earth-based alloy in S3 is LRE-M, wherein LRE is one or two of the light rare earth metal elements Nd or Pr, and the mass fraction of LRE in the LRE-M light rare earth-based alloy is 85-95wt%; M is one or more of the auxiliary metal elements Cu, Al, Mn, Ga, Co, and Fe, and the mass fraction of M in the LRE-M light rare earth-based alloy is 5-15wt%.
[0013] By adopting the above technical scheme, the present invention adopts light rare earth metal elements Nd or Pr as the main elements of the diffusion source. Compared with the method of using heavy rare earth elements as the main elements of the diffusion source in the prior art, the price of light rare earth metal elements is cheaper, which is beneficial to reducing production and processing costs; at the same time, the addition of auxiliary metal elements makes the melting point of the light rare earth diffusion source lower than the diffusion temperature, thereby allowing the light rare earth elements to penetrate into the interior of the magnet faster at high temperature, thereby improving the diffusion efficiency. In addition, the auxiliary metal elements can also optimize the grain boundaries of the magnet, thereby inhibiting the nucleation of antimagnetic domains.
[0014] The present invention is further configured as follows: the light rare earth-based alloy in S3 is used as an anode electrode, the electrode diameter is 2-10 mm, the electrode rotation speed is 1000-2000 r / min, and the electrode moving speed is 1-20 mm / s.
[0015] By adopting the above technical solution, if the electrode diameter is too small, the coating time will be too long and the coating efficiency will be low. If the electrode diameter is too large, the density of the coating and the bonding strength between the coating and the substrate will be reduced, and the coating will easily fall off. Therefore, the present invention controls the electrode diameter to 2-10mm.
[0016] The present invention is further configured as follows: the inert protective gas in S3 is nitrogen or argon, and the flow rate of the nitrogen or argon is controlled to be 5-10 L / min, and the oxygen content in the inert gas atmosphere is controlled to be below 2 ppm.
[0017] By adopting the above technical solution, if the oxygen content is too high, the diffusion source will be oxidized during the coating process, which will reduce the quality of the coating and even cause microcracks. The appearance of microcracks will make the coating easy to fall off; in addition, too high oxygen content will also make the thickness distribution of the coating uneven.
[0018] The present invention is further configured as follows: the deposition voltage of controlling the electrospark deposition in S3 is 60-90V, the deposition capacitance is 40-200μF, the deposition angle is 70-80°, the deposition pressure is 0.2-2N, the deposition frequency is 200-450HZ, and the specific deposition time is 2-6min·cm –2 .
[0019] By adopting the above technical scheme, the electrospark deposition technology mainly uses high-density electric energy to coat the metal surface. Through the spark discharge effect between the electrode material and the metal substrate surface, the electrode material is melted and infiltrated into the metal surface to form a surface alloy coating layer. The higher the deposition voltage, the faster the coating speed. However, when the voltage is too large, gaps and cracks will be generated on the coating. The size of the deposition capacitance directly determines the size of the discharge energy, which in turn affects the quality of the deposited layer. If the capacitance energy is too large, the electrode material will be vaporized and splashed, causing cracks in the coating. The selection of a suitable deposition angle can maintain a stable deposition arc, which is conducive to the deposition process and obtaining the best coating. The deposition pressure will affect the coating quality and coating speed. The deposition frequency will affect the coating thickness. Too high or too low is not good. If the deposition frequency is too low, the coating thickness will be too thin, so that the performance after diffusion cannot meet the requirements. If the frequency is too high, the cost will be too high. During deposition, increasing the specific deposition time can increase the thickness of the deposited layer. However, if the specific deposition time is too large, the thickness of the deposited layer will not only decrease, but also defects such as porosity and cracks will gradually increase.
[0020] The present invention is further configured as follows: the thickness of the light rare earth-based alloy coating in S3 is controlled to be 20-50 μm.
[0021] By adopting the above technical solution, if the coating thickness is too large, the coating weight will be large and the cost requirement will be high. The grain boundary diffusion of the present invention is mainly to control the cost and achieve the purpose of reducing costs and increasing efficiency. Therefore, the present invention controls the thickness of the light rare earth-based alloy coating to between 20-50μm.
[0022] The present invention is further configured as follows: the light rare earth-based alloy used as the anode electrode in S3 is plated by a selective diffusion coating method, so that a light rare earth-based alloy coating of a predetermined shape is formed on the surface of the semi-densified magnet sample.
[0023] By adopting the above technical solution, the present invention can use the selective diffusion method to selectively coat the magnetic material substrate, and reduce the usage of diffusion sources through the selective diffusion, thereby achieving the purpose of cost saving.
[0024] In summary, the present invention has the following beneficial effects:
[0025] The present invention provides a grain boundary diffusion method of a light rare earth-based diffusion source based on electrospark deposition, comprising the following steps: first, semi-densified sintering of magnetic powder to obtain a magnetic material matrix; second, electrospark deposition is used as a coating method to plate a light rare earth-based alloy diffusion source onto the surface of the magnetic material matrix under gas protection; and finally, densification sintering and tempering are performed. Electrospark deposition has little effect on the performance of the matrix, can accurately control the coating amount and coating area, and has simple equipment; at the same time, gas protection can effectively inhibit the oxidation of the light rare earth-based diffusion source during the coating process. The present invention effectively increases the utilization efficiency and diffusion depth of the light rare earth-based diffusion source, significantly reduces the production cost, and has the effects of preventing the oxidation of the light rare earth diffusion source, effectively improving the coercivity of the magnetic material matrix, improving the diffusion efficiency and reducing the cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a structural schematic diagram of the present invention.
[0027] Figure 2 It is a cross-sectional view of the sample after electrospark deposition coating of the present invention, and the sample has not been diffused.
[0028] Figure 3 This is a metallographic photograph taken at a depth of 50 μm from the magnet surface after diffusion in Example 1 of the present invention.
[0029] Figure 4 This is a metallographic photograph of the comparative example 2 of the present invention after diffusion at a depth of 50 μm from the magnet surface.
[0030] Figure 5 It is a schematic diagram of the sample after selective coating by electrospark deposition on a sintered NdFeB magnetic material substrate in the present invention.
[0031] In the figure: 1. Magnetic material substrate; 2. Light rare earth-based alloy coating; 3. Electrode gun; 4. Light rare earth-based alloy electrode; 5. Plasma arc; 6. Protective gas; 7. Coating area; 8. Non-coating area. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with the accompanying drawings.
[0033] A grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition, such as Figure 1-2As shown, the grain boundary diffusion device of the present invention includes an electrode gun 3 and a shielding gas pipe, the shielding gas pipe is used to continuously purge an inert shielding gas 6 around the welding position of the electrode gun 3 at a fan-shaped angle, the material for electric spark deposition includes a light rare earth alloy electrode 4 and a NdFeB magnetic material substrate 1, and the light rare earth alloy electrode 4 is melted and welded to the magnetic material substrate 1 by a high-temperature plasma arc 5 generated by the electrode gun 3 to form a light rare earth alloy coating 2, and the steps are as follows:
[0034] S1: orienting sintered NdFeB magnetic powder with an average particle size of 2-10 μm in a magnetic field of 1.4-2 T, and pressing it into a green compact at a pressure of 10-20 MPa using an isostatic press;
[0035] S2: The green body obtained by pressing in S1 is sintered at 950-1010℃ for 1-3h to obtain a density of 6.5-7.0g / cm 3 Semi-densified magnetic material matrix;
[0036] S3: Using a light rare earth alloy as an anode electrode and a semi-densified magnetic material substrate as a cathode electrode, a light rare earth alloy coating is plated on the magnetic material substrate by electric spark deposition under the protection of an inert protective gas to obtain a semi-densified magnet sample containing a light rare earth alloy coating;
[0037] S4: densification sintering is performed on the semi-densified magnet sample containing the light rare earth alloy coating obtained in S3, and the sintering temperature is controlled to be 1030-1090°C and the sintering time is 2-5h;
[0038] S5: The densified magnet sample containing the light rare earth alloy coating obtained by sintering in S4 is tempered, and the tempering temperature is controlled to be 500-800° C., and the tempering time is controlled to be 3-8 hours.
[0039] Among them, the composition of the light rare earth-based alloy in S3 is LRE-M, wherein LRE is one or two of the light rare earth metal elements Nd or Pr, and the mass fraction of LRE in the LRE-M light rare earth-based alloy is 85-95wt%; M is one or more of the auxiliary metal elements Cu, Al, Mn, Ga, Co, and Fe, and the mass fraction of M in the LRE-M light rare earth-based alloy is 5-15wt%. The present invention adopts light rare earth metal elements Nd or Pr as the main elements of the diffusion source. Compared with the method of using heavy rare earth elements as the main elements of the diffusion source in the prior art, the price of light rare earth metal elements is cheaper, which is conducive to reducing production and processing costs; at the same time, the addition of auxiliary metal elements makes the melting point of the light rare earth diffusion source lower than the diffusion temperature, thereby enabling the light rare earth elements to penetrate into the interior of the magnet faster at high temperature, thereby improving the diffusion efficiency. In addition, the auxiliary metal elements can also optimize the grain boundaries of the magnet, thereby inhibiting the nucleation of the antimagnetic domain; the light rare earth-based alloy in S3 is used as an anode electrode, and its electrode diameter is 2-10mm, and the electrode rotation speed is 1 000-2000r / min, the electrode moving speed is 1-20mm / s. If the electrode diameter is too small, the coating time will be too long and the coating efficiency will be low. If the electrode diameter is too large, the density of the coating and the bonding strength between the coating and the substrate will be reduced, and the coating will easily fall off. Therefore, the electrode diameter is controlled to be 2-10mm in the present invention; the inert protective gas in S3 is nitrogen or argon, and the flow rate of nitrogen or argon is controlled to be 5-10L / min, and the oxygen content in the inert gas atmosphere is controlled to be below 2ppm. If the oxygen content is too high, it will cause The diffusion source is oxidized during the coating process, which reduces the quality of the coating and even causes microcracks. The appearance of microcracks will cause the coating to fall off easily. In addition, excessive oxygen content will also make the thickness distribution of the coating uneven. In S3, the deposition voltage of the electrospark deposition is controlled to be 60-90V, the deposition capacitance is 40-200μF, and a light rare earth-based alloy is installed on the electrode gun as the anode electrode. During the deposition process, the deposition angle between the anode electrode and the magnetic material substrate is controlled to be 70-80°, and the deposition pressure applied by the anode electrode on the magnetic material substrate is controlled to be 0.2-2N, deposition frequency is 200-450HZ, specific deposition time is 2-6min·cm–2, where specific deposition time is the ratio of the time used for electrospark deposition to the deposition area, which indicates the residence time of the electrode on the substrate. The higher the deposition voltage, the faster the coating speed. However, when the voltage is too high, gaps and cracks will be generated in the coating. The size of the deposition capacitance directly determines the size of the discharge energy, which in turn affects the quality of the deposited layer. If the capacitance energy is too high, the electrode material will be vaporized and splashed, causing cracks in the coating. Choosing a suitable deposition angle can maintain a stable deposition arc, which is conducive to the deposition process and obtaining the best coating. The deposition pressure will affect the coating quality and coating speed. Degree; deposition frequency will affect the coating thickness, too high or too low is not good, too low deposition frequency will lead to too thin coating thickness, so that the performance after diffusion cannot meet the requirements, too high frequency will lead to too high cost; during deposition, increasing the specific deposition time can increase the deposition layer thickness; but if the specific deposition time is too large, the deposition layer thickness will not only decrease but also defects such as porosity and cracks will gradually increase; the thickness of the light rare earth-based alloy coating in S3 is controlled at 20-50μm. If the coating thickness is too large, the weight of the coating will be large and the cost requirement will be high. The grain boundary diffusion of the present invention is mainly to control the cost and achieve the purpose of reducing costs and increasing efficiency. Therefore, the thickness of the light rare earth-based alloy coating is controlled between 20-50μm in the present invention. .
[0040] like Figure 5 As shown, the light rare earth-based alloy used as the anode electrode in S3 is plated by a selective diffusion coating method, forming a coating area 7 and a non-coating area 8 on the magnetic material substrate 1, so that a light rare earth-based alloy coating of a predetermined shape is formed on the surface of the semi-densified magnet sample. The present invention can plate the light rare earth-based alloy by selective diffusion, and reduce the use of diffusion sources by selective diffusion, thereby achieving the purpose of cost saving. Specific embodiment 1
[0042] A grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition comprises the following steps:
[0043] S1: Sintering NdFeB magnetic powder with an average particle size of 2.8 μm and a grade of N38 is pressed under a magnetic field of 2 T and a pressure of 14 MPa to obtain a compact;
[0044] S2: The compact was sintered at 950 °C for 3 h to obtain a density of 6.8 g / cm 3 Semi-densified blank;
[0045] S3: The composition is Pr 85 Al 10Cu5 (wt%) light rare earth alloy is used as the anode electrode, the electrode diameter is 6mm, the electrode rotation speed is 1200r / min, and the semi-densified blank is used as the cathode electrode. Under the protection of high-purity argon gas with a flow rate of 5L / min, the anode electrode coats the entire surface of the blank with a coating thickness of 30μm. During coating, the moving speed of the anode electrode is 10mm / s, the deposition voltage of the electrospark deposition is 80V, the deposition angle is 78.8°, the deposition pressure is 1N, the deposition frequency is 300HZ, and the specific deposition time is 4min·cm –2 , a semi-densified magnet sample containing a light rare earth alloy coating was obtained, and the mass of the sample after coating increased by 1% compared with that before coating;
[0046] S4: The sample is subjected to densification sintering at a temperature of 1060°C for 4 hours; then directly subjected to tempering treatment at 620°C for 5 hours.
[0047] Figure 3 This is a surface morphology photograph of the sample obtained by the method of specific embodiment 1 observed under an electron microscope. The white area in the figure is the grain boundary phase, and the gray area is Nd2Fe 14 B main phase, from the figure can be observed that a large number of continuous network distribution of grain boundary phase makes Nd2Fe 14 The B main phases are isolated from each other, which weakens the exchange coupling between adjacent main phase grains. This structure is beneficial to the improvement of coercivity.
[0048] Comparative Example 1
[0049] A grain boundary diffusion method of a light rare earth-based diffusion source based on electric spark deposition. The difference between comparative example 1 and specific embodiment 1 is that during electric spark deposition, the electrode is not protected by high-purity argon gas and is directly exposed to the air.
[0050] Comparative Example 2
[0051] A grain boundary diffusion method of a light rare earth-based diffusion source based on screen printing, comprising the following steps;
[0052] S1: Sintering NdFeB magnetic powder with an average particle size of 2.8 μm and a grade of N38 is pressed under a magnetic field of 2 T and a pressure of 14 MPa to obtain a compact;
[0053] S2: The compact was sintered at 1060°C for 5 h to obtain a density of 7.6 g / cm 3 Densified blank;
[0054] S3: The composition is Pr 85 Al 10 Cu5 (wt%) light rare earth alloy powder and alcohol and PVB were mixed in a ratio of 1:1:1 to prepare a slurry, wherein Pr 85Al 10 The average particle size of Cu5 alloy powder is 7.6 μm;
[0055] S4: The slurry is plated onto the surface of the blank, and then dried in an oven at 100°C. The mass of the blank after coating increases by 1% compared with that before coating;
[0056] S5: The sample is subjected to an optimal diffusion treatment at 900°C for 10 h, followed by a direct tempering treatment at 620°C for 5 h.
[0057] Figure 4 This is a surface morphology photograph of a sample obtained by using the existing technology of screen printing grain boundary diffusion method observed under an electron microscope in Comparative Example 2. The white area in the figure is the grain boundary phase, and the gray area is Nd2Fe 14 B main phase, and Figure 3 different, Figure 4 There is a lack of continuous network-like grain boundary phases between adjacent main phase grains, and the main phase grains are directly bonded together, which makes the adjacent main phase grains connected into a large grain group. The remagnetization of one main phase grain will drive the remagnetization of the adjacent grains in a chain reaction, which makes the magnet prepared by the comparative example 2 have a lower coercive force than the magnet prepared by the specific embodiment 1.
[0058] The effects of the methods of specific embodiment 1, comparative example 1 and comparative example 2 on the performance of N38 magnet are shown in Table 1 below:
[0059] Table 1: Effects of Specific Example 1, Comparative Example 1 and Comparative Example 2 on the Performance of N38 Magnets
[0060]
[0061] It can be seen from Table 1 that, by comparing Specific Example 1, Comparative Example 1 and Comparative Example 2, the remanence and squareness of the three change little relative to the N38 magnetic material matrix, but compared with the grain boundary diffusion methods of Comparative Examples 1 and 2, the intrinsic coercive force of the sample obtained by the grain boundary diffusion method based on protective atmosphere electrospark deposition in Specific Example 1 is more improved. Specific embodiment 2
[0063] A grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition comprises the following steps:
[0064] S1: Sintering NdFeB magnetic powder with an average particle size of 2.8 μm and a grade of N38 is pressed under a magnetic field of 2 T and a pressure of 14 MPa to obtain a compact;
[0065] S2: The compact was sintered at 950 °C for 3 h to obtain a density of 6.8 g / cm 3 Semi-densified blank;
[0066] S3: The composition is Pr 85 Nd 10 Fe5 (wt%) light rare earth alloy is used as the anode electrode, the electrode diameter is 6mm, the electrode rotation speed is 1200r / min, and the semi-densified blank is used as the cathode electrode. Under the protection of high-purity argon gas with a flow rate of 5L / min, the anode electrode coats the entire surface of the blank with a coating thickness of 25μm. During coating, the moving speed of the anode electrode is 10mm / s, the deposition voltage of the electrospark deposition is 80V, the deposition angle is 78.8°, the deposition pressure is 1N, the deposition frequency is 300HZ, and the specific deposition time is 4min·cm –2 , a semi-densified magnet sample containing a light rare earth alloy coating was obtained, and the mass of the sample after coating increased by 0.8% compared with that before coating;
[0067] S4: The sample is subjected to densification sintering at a temperature of 1060°C for 4 hours; then directly subjected to tempering treatment at 620°C for 5 hours.
[0068] The difference between the specific embodiment 2 and the specific embodiment 1 is that: first, the diffusion source components of the embodiment 2 and the embodiment 1 are different. The component of the diffusion source in the embodiment 1 is Pr 85 Al 10 Cu5, the composition of the diffusion source in Example 2 is Pr 85 Nd 10 Fe 5; Secondly, the mass increase after coating is different for both films. In Example 1, the mass increase after coating is 1% compared with that before coating, and in Example 2, the mass increase after coating is 0.8% compared with that before coating.
[0069] Comparative Example 3
[0070] A grain boundary diffusion method of a light rare earth-based diffusion source based on electrospark deposition. The difference between comparative example 3 and specific embodiment 2 is that during electrospark deposition, the electrode is not protected by high-purity argon gas and is directly exposed to the air.
[0071] Comparative Example 4
[0072] A method for grain boundary diffusion of a light rare earth-based diffusion source based on screen printing comprises the following steps:
[0073] S1: Sintering NdFeB magnetic powder with an average particle size of 2.8 μm and a grade of N38 is pressed under a magnetic field of 2 T and a pressure of 14 MPa to obtain a compact;
[0074] S2: The compact was sintered at 1060°C for 5 h to obtain a density of 7.6 g / cm 3 Densified blank;
[0075] S3: The composition is Pr 85 Nd 10 Fe5 (wt%) light rare earth alloy powder and alcohol and PVB were mixed in a ratio of 1:1:1 to prepare a slurry, wherein Pr 85 Nd 10 The average particle size of Fe5 alloy powder is 7.3 μm;
[0076] S4: The slurry is plated onto the surface of the blank, and then dried in an oven at 100°C. The mass of the blank after coating increases by 1% compared with that before coating;
[0077] S5: The sample is subjected to an optimal diffusion treatment at 890°C for 10 h, followed by a direct tempering treatment at 620°C for 5 h.
[0078] The screen printing grain boundary diffusion method of comparative example 4 is a prior art, and one difference between comparative example 4 and specific embodiment 2 is that the mass of comparative example 4 increases by 1% after coating than before coating.
[0079] The effects of the methods of specific embodiment 2, comparative example 3 and comparative example 4 on the performance of N38 magnet are shown in Table 2 below:
[0080] Table 2: Effects of Specific Example 2, Comparative Example 3 and Comparative Example 4 on the Performance of N38 Magnets
[0081]
[0082] As shown in Table 2, compared with Example 4 with a coating weight increase of 1wt%, Example 2 with a coating weight increase of 0.8wt% has a higher coercivity, and the remanence and squareness are basically the same; compared with Example 2 with the same weight increase and Comparative Example 3, the coercivity is greatly improved, and the remanence is basically the same. It can be seen that the electrospark deposition based on the protective atmosphere can improve the utilization efficiency of the light rare earth diffusion source and reduce the usage amount.
[0083] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.
Claims
1. A grain boundary diffusion method of light rare earth-based diffusion source based on protective atmosphere electrospark deposition, It is characterized in that The following steps are involved: S1: orienting sintered NdFeB magnetic powder with an average particle size of 2-10 μm in a magnetic field of 1.4-2 T, and pressing it into a green compact at a pressure of 10-20 MPa using an isostatic press; S2: The green body obtained by pressing in S1 is sintered at 950-1010℃ for 1-3h to obtain a density of 6.5-7.0g / cm 3 Semi-densified magnetic material matrix; S3: Using a light rare earth alloy as an anode electrode and a semi-densified magnetic material substrate as a cathode electrode, a light rare earth alloy coating is plated on the magnetic material substrate by electric spark deposition under the protection of an inert protective gas to obtain a semi-densified magnet sample containing a light rare earth alloy coating; S4: densification sintering is performed on the semi-densified magnet sample containing the light rare earth alloy coating obtained in S3, and the sintering temperature is controlled to be 1030-1090°C and the sintering time is 2-5h; S5: The densified magnet sample containing the light rare earth alloy coating obtained by sintering in S4 is tempered, and the tempering temperature is controlled to be 500-800° C., and the tempering time is controlled to be 3-8 hours.
2. The grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition according to claim 1, Features: The composition of the light rare earth-based alloy in S3 is LRE-M, wherein LRE is one or two of the light rare earth metal elements Nd or Pr, and the mass fraction of LRE in the LRE-M light rare earth-based alloy is 85-95wt%; M is one or more of the auxiliary metal elements Cu, Al, Mn, Ga, Co, and Fe, and the mass fraction of M in the LRE-M light rare earth-based alloy is 5-15wt%.
3. The grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition according to claim 1, Features: The light rare earth-based alloy in S3 is used as the anode electrode, the electrode diameter is 2-10 mm, the electrode rotation speed is 1000-2000 r / min, and the electrode movement speed is 1-20 mm / s.
4. The grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition according to claim 1, Features: The inert protective gas in S3 is nitrogen or argon, and the flow rate of nitrogen or argon is controlled to be 5-10L / min, and the oxygen content in the inert gas atmosphere is controlled to be below 2ppm.
5. The grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition according to claim 1, Features: The deposition voltage of S3 controlled by the electrospark deposition was 60-90 V, the deposition capacitance was 40-200 μF, the deposition angle was 70-80°, the deposition pressure was 0.2-2 N, the deposition frequency was 200-450 Hz, and the specific deposition time was 2-6 min·cm – 2 .
6. The grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition according to claim 1, Features: The thickness of the light rare earth-based alloy coating in S3 is controlled at 20-50μm.
7. The grain boundary diffusion method of a light rare earth-based diffusion source based on protective atmosphere electrospark deposition according to claim 1, Features: The light rare earth-based alloy used as the anode electrode in S3 is plated by a selective diffusion coating method, so that a light rare earth-based alloy coating of a predetermined shape is formed on the surface of the semi-densified magnet sample.
Citation Information
Patent Citations
R-Fe-B rare-earth sintered magnet and process for producing the same
CN101375352A
Hybrid film coating method of neodymium iron boron rare earth permanent magnet device
CN103854819A
WC / amorphous composite coating and preparation method thereof
CN106757008A
Laser-cleaning-based electrospark hardening treatment method for surfaces of neodymium iron boron magnets
CN108866547A
Method for enhancing coercive force of neodymium-iron-boron magnet through evaporation grain boundary diffusion
CN109360728A