A battery preparation method, back contact battery and photovoltaic module

By cleaning and setting up the sacrificial layer protection using a mixed solution of hydrogen peroxide and potassium hydroxide, the problems of poor passivation performance and short-circuit current drop caused by silicon wafer corrosion in the preparation of back contact battery are solved, and the short-circuit current and efficiency of the battery are improved.

CN118825136BActive Publication Date: 2024-12-03GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411297171.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

During the preparation of back contact batteries, the silicon wafer is susceptible to corrosion during cleaning and passivation and water washing, resulting in poor passivation performance and reduced short circuit current.

Method used

The silicon wafer is cleaned by a mixed solution of hydrogen peroxide and potassium hydroxide of a certain concentration ratio range, remove the coating layer, reduce the corrosion rate of the passivation film layer, and protect the anti-reduction layer by setting a sacrificial layer outside the anti-reduction layer to avoid It is damaged during passivation washing.

Benefits of technology

The corrosion impact on the first semiconductor layer and suede in the opening area is effectively avoided, the short circuit current and efficiency of the battery are ensured, and the overall performance of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825136B_ABST
    Figure CN118825136B_ABST
Patent Text Reader

Abstract

The invention discloses a battery preparation method, a back contact battery and a photovoltaic module, and relates to the technical field of back contact batteries. The battery preparation method removes the coating layer by a mixed solution of hydrogen peroxide and potassium hydroxide in a certain concentration ratio range, so as to greatly reduce the corrosion rate of the passivation film layer, avoid affecting the passivation performance of the first semiconductor layer, and avoid affecting the suede reflectivity in the first opening area, thereby ensuring the short-circuit current of the battery; and the anti-reflection layer is protected by a sacrificial layer arranged outside the anti-reflection layer, so as to avoid damage to the anti-reflection layer during the passivation water washing process, further ensuring the short-circuit current of the battery and improving the battery efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back-contact batteries, and in particular relates to a battery preparation method, a back-contact battery and a photovoltaic module. Background Art

[0002] At present, in the preparation process of back-contact batteries, after the first semiconductor layer with an opening area is formed on the back of the silicon wafer, and the passivation layer and anti-reflection layer are formed on the front of the silicon wafer, it is necessary to first use a low-concentration alkali solution to remove the plating, and then perform a passivation water wash to form a second semiconductor layer on the back of the silicon wafer. However, during the cleaning process, the first semiconductor layer on the back of the silicon wafer will inevitably be corroded and thinned, thereby affecting the passivation performance of the film layer, and the velvet pyramid spire in the opening area on the back of the silicon wafer will also be corroded and removed, resulting in a high reflectivity, affecting the short-circuit current of the battery; in addition, during the passivation water wash process, the anti-reflection layer on the front of the silicon wafer will be corroded and removed, resulting in a poor front anti-reflection effect, and the short-circuit current of the battery will be significantly reduced, directly affecting the battery efficiency.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art that silicon wafers are easily corroded during cleaning and passivation water washing, resulting in poor passivation performance and decreased short-circuit current. A battery preparation method, a back-contact battery and a photovoltaic module are provided. The battery preparation method cleans the silicon wafer with a mixed solution of hydrogen peroxide and potassium hydroxide in a certain concentration ratio range to remove the coating layer, so as to greatly reduce the corrosion rate of the passivation film layer, avoid affecting the passivation performance of the first semiconductor layer, and avoid affecting the suede reflectivity in the opening area, thereby ensuring the short-circuit current of the battery; and the anti-reflection layer is protected by a sacrificial layer arranged outside the anti-reflection layer to avoid damage to the anti-reflection layer during the passivation water washing process, further ensuring the short-circuit current of the battery and improving the battery efficiency.

[0005] In order to achieve the above object, in a first aspect, the present invention provides a method for preparing a battery, comprising the following steps:

[0006] S1. Provide double-sided polished silicon wafers;

[0007] S2. depositing a first semiconductor layer on the back side of the silicon wafer, wherein the first semiconductor layer comprises a first tunneling oxide layer and a first doping layer disposed in sequence;

[0008] S3. Cleaning and removing the phosphosilicate glass layer produced by the deposition of S2 on the first doped layer;

[0009] S4. forming a mask layer on the first doped layer;

[0010] S5. Etching an opening on the first tunneling oxide layer, the first doping layer and the mask layer to form a first opening region;

[0011] S6. Remove the first tunneling oxide layer and the first doping layer remaining in the first opening region by texturing and cleaning, and simultaneously form a texturing surface in the first opening region and on the front side of the silicon wafer, and then completely or partially remove the mask layer outside the first opening region by cleaning;

[0012] S7. Depositing a passivation layer, an anti-reflection layer and a sacrificial layer in sequence on the front side of the silicon wafer, wherein the passivation layer comprises a second tunneling oxide layer and a second doping layer disposed in sequence;

[0013] S8. Clean and remove the winding coating produced by S7 deposition on the back of the silicon wafer, then perform alkaline washing and acid washing on the silicon wafer in sequence, and then perform passivation water washing on the silicon wafer, wherein the winding coating includes a first winding coating produced by depositing a sacrificial layer, a second winding coating produced by depositing an anti-reflection layer, and a third winding coating produced by depositing a passivation layer. The cleaning solution used to remove the third winding coating is a mixed solution of hydrogen peroxide and potassium hydroxide, and the concentration ratio of hydrogen peroxide to potassium hydroxide is 1 / 10-1 / 6. The corrosion rate of polysilicon is 0.05nm / s-0.1nm / s.

[0014] Preferably, S7 includes:

[0015] S71. Depositing a second tunneling oxide layer and a second doping layer on the front side of the silicon wafer in sequence by plasma enhanced chemical vapor deposition, wherein the thickness of the second tunneling oxide layer is 1nm-2nm, and the thickness of the second doping layer is 1nm-10nm;

[0016] S72. Depositing an anti-reflection layer on the second doped layer by plasma enhanced chemical vapor deposition, wherein the anti-reflection layer comprises a first anti-reflection layer and a second anti-reflection layer disposed in sequence, and the total thickness of the anti-reflection layer is 70nm-100nm;

[0017] S73. Depositing a sacrificial layer on the anti-reflection layer by plasma enhanced chemical vapor deposition, wherein the thickness of the sacrificial layer is 3nm-8nm.

[0018] Preferably, S72 includes:

[0019] Silane and ammonia are introduced and reacted under the condition of turning on the glow to form a first anti-reflection layer, the first anti-reflection layer is a silicon nitride layer, the nitrogen content in the first anti-reflection layer is 40%-45%, the thickness of the first anti-reflection layer is 20nm-40nm, and the refractive index of the first anti-reflection layer is 2.2-2.3;

[0020] Silane, ammonia and laughing gas are introduced and reacted under the condition of turning on the glow to form a second anti-reflection layer. The second anti-reflection layer is a silicon nitride layer. The nitrogen content in the second anti-reflection layer is 45%-50%, the thickness of the second anti-reflection layer is 50nm-70nm, and the refractive index of the second anti-reflection layer is 1.8-2.0.

[0021] Preferably, the reaction conditions for forming the first anti-reflection layer are: reaction temperature of 400° C.-450° C., silane flow rate of 800 sccm-1200 sccm, ammonia flow rate of 4000 sccm-6000 sccm, reaction time of 300 s-500 s, reaction pressure of 500 mtorr-3000 mtorr, power of 4000 W-6000 W;

[0022] And / or, the reaction conditions for forming the second anti-reflection layer are: 400℃-450℃, silane flow rate is 500sccm-900sccm, ammonia flow rate is 5000sccm-8000sccm, nitrous oxide flow rate is 500sccm-2000sccm, reaction time is 300s-500s, reaction pressure is 500mtorr-3000mtorr, and power is 4000W-6000W.

[0023] Preferably, S73 includes:

[0024] Silane and ammonia are introduced and reacted under the condition of turning on the glow to form a sacrificial layer. The sacrificial layer is a silicon nitride layer. The nitrogen content in the sacrificial layer is 35%-40%, and the refractive index of the sacrificial layer is 2.3-2.5.

[0025] Preferably, the reaction conditions for forming the sacrificial layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1800sccm, ammonia flow rate of 3000sccm-5000sccm, reaction time of 40s-100s, reaction pressure of 500mtorr-3000mtorr, and power of 4000W-6000W.

[0026] Preferably, S8 includes:

[0027] The first winding coating and the second winding coating are sequentially cleaned and removed by a chain cleaning machine, wherein the cleaning solution used is an aqueous solution containing hydrofluoric acid, and the concentration of hydrofluoric acid is 5%-15%;

[0028] The third winding coating is removed by cleaning in a tank cleaning machine, wherein the cleaning solution used has a hydrogen peroxide concentration of 0.2%-1% and a potassium hydroxide concentration of 2%-5%;

[0029] The silicon wafer is alkaline washed, wherein the alkaline washing solution used is a mixed solution of ammonia water or potassium hydroxide and hydrogen peroxide, the concentration of ammonia water or potassium hydroxide is 2%-5%, and the concentration of hydrogen peroxide is 3%-5%;

[0030] The silicon wafer is pickled, wherein the pickling solution used is a mixed solution of hydrochloric acid and hydrogen peroxide, the concentration of hydrochloric acid is 2%-5%, and the concentration of hydrogen peroxide is 3%-5%;

[0031] The silicon wafer is passivated and washed with water, wherein the washing solution used is an aqueous solution containing hydrofluoric acid, and the concentration of hydrofluoric acid is 1%-5%.

[0032] Preferably, the cleaning conditions for removing the first winding coating and the second winding coating are: the reaction temperature is 20°C-35°C, the reaction time is 30s-120s, and the transmission roller speed of the chain cleaning machine is 1.2m / min-3.0m / min;

[0033] And / or, the cleaning conditions for removing the third winding coating are: reaction temperature is 25°C-35°C, reaction time is 60s-240s;

[0034] And / or, the alkaline washing conditions are: reaction temperature is 60°C-80°C, reaction time is 120s-240s;

[0035] And / or, the pickling conditions are: reaction temperature is 60°C-80°C, reaction time is 120s-240s;

[0036] And / or, the passivation water washing conditions are: reaction temperature is 10°C-20°C, and reaction time is 60s-180s.

[0037] Preferably, after S8, the battery preparation method further comprises:

[0038] S9. depositing a second semiconductor layer on the back side of the silicon wafer so that a portion of the second semiconductor layer covers a side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer, wherein the second semiconductor layer includes an intrinsic amorphous silicon layer and a third doped layer disposed in sequence;

[0039] S10. Etching openings on the second semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;

[0040] S11. forming a conductive film layer on the back side of the silicon wafer;

[0041] S12. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the second semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0042] S13. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0043] In a second aspect, the present invention provides a back-contact battery, which is prepared by the above-mentioned battery preparation method.

[0044] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0045] Beneficial effects:

[0046] Through research, it is found that during the de-coating and cleaning process after the front coating, the first semiconductor layer on the back of the silicon wafer will inevitably be corroded and thinned, thereby affecting the passivation performance of the film layer, and the velvet pyramid tip in the opening area on the back of the silicon wafer will also be corroded and removed, resulting in a high reflectivity, affecting the short-circuit current of the battery; in addition, during the passivation water washing process, the anti-reflection layer on the front of the silicon wafer will be corroded and removed, resulting in poor anti-reflection effect on the front, and the short-circuit current of the battery will be significantly reduced, directly affecting the battery efficiency. Based on this, further research is conducted and the present invention is proposed.

[0047] The battery preparation method provided by the present invention adopts the above-mentioned technical scheme, especially uses a mixed solution of hydrogen peroxide and potassium hydroxide in a certain concentration ratio range to clean the silicon wafer and remove the coating layer, so as to greatly reduce the corrosion rate of the passivation film layer, avoid affecting the passivation performance of the first semiconductor layer, and avoid affecting the suede reflectivity in the first opening area, thereby ensuring the short-circuit current of the battery; and the anti-reflection layer is protected by a sacrificial layer arranged outside the anti-reflection layer to avoid damage to the anti-reflection layer during the passivation water washing process, thereby further ensuring the short-circuit current of the battery and improving the battery efficiency.

[0048] The back contact battery provided by the present invention is produced by the above-mentioned battery preparation method, and has better passivation performance, higher short-circuit current and higher battery efficiency.

[0049] The photovoltaic module provided by the present invention includes the above-mentioned back contact cell, has better photoelectric conversion efficiency and high photovoltaic power generation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0051] Figure 1 This is a schematic diagram of the structure of a silicon wafer after double-sided polishing and cleaning according to an embodiment of the present invention;

[0052] Figure 2 This is a schematic diagram of the structure of forming a first semiconductor layer and a mask layer on the back side of a silicon wafer according to an embodiment of the present invention;

[0053] Figure 3 This is a schematic diagram of a structure in which a first opening area is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0054] Figure 4 This is a schematic diagram of the structure of forming a passivation layer, an anti-reflection layer and a sacrificial layer on the front side of a silicon wafer according to an embodiment of the present invention;

[0055] Figure 5 This is a schematic diagram of the structure of removing the sacrificial layer from the front side of the silicon wafer according to an embodiment of the present invention;

[0056] Figure 6 This is a schematic diagram of a structure in which a second semiconductor layer is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0057] Figure 7 This is a schematic diagram of a structure in which a second opening area is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0058] Figure 8 This is a schematic diagram of a structure in which a conductive film layer is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0059] Fig. 9 This is a schematic diagram of a structure in which an isolation groove is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0060] Fig.10 It is a schematic diagram of the structure of forming a first electrode and a second electrode on the back side of a silicon wafer according to an embodiment of the present invention.

[0061] Description of reference numerals:

[0062] 1-silicon wafer; 2-first tunneling oxide layer; 3-first doping layer; 4-mask layer; 5-second tunneling oxide layer; 6-second doping layer; 7-first anti-reflection layer; 8-second anti-reflection layer; 9-sacrificial layer; 10-intrinsic amorphous silicon layer; 11-third doping layer; 12-conductive film layer; 13-first electrode; 14-second electrode. DETAILED DESCRIPTION

[0063] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0064] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0065] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0066] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0067] In the first aspect, the present invention provides a battery preparation method, which cleans silicon wafers with a mixed solution of hydrogen peroxide and potassium hydroxide in a certain concentration ratio range to remove the coating layer, thereby greatly reducing the corrosion rate of the passivation film layer, avoiding affecting the passivation performance of the first semiconductor layer, and avoiding affecting the suede reflectivity in the first opening area, thereby ensuring the short-circuit current of the battery; and protecting the anti-reflection layer by a sacrificial layer arranged outside the anti-reflection layer to avoid damage to the anti-reflection layer during the passivation water washing process, thereby further ensuring the short-circuit current of the battery and improving the battery efficiency.

[0068] The battery preparation method comprises the following steps:

[0069] S1. Provide double-sided polished silicon wafers;

[0070] S2. depositing a first semiconductor layer on the back side of the silicon wafer, wherein the first semiconductor layer comprises a first tunneling oxide layer and a first doping layer disposed in sequence;

[0071] S3. Cleaning and removing the phosphosilicate glass layer produced by the deposition of S2 on the first doped layer;

[0072] S4. forming a mask layer on the first doped layer;

[0073] S5. Etching an opening on the first tunneling oxide layer, the first doping layer and the mask layer to form a first opening region;

[0074] S6. Remove the first tunneling oxide layer and the first doping layer remaining in the first opening region by texturing and cleaning, and simultaneously form a texturing surface in the first opening region and on the front side of the silicon wafer, and then completely or partially remove the mask layer outside the first opening region by cleaning;

[0075] S7. Depositing a passivation layer, an anti-reflection layer and a sacrificial layer in sequence on the front side of the silicon wafer, wherein the passivation layer comprises a second tunneling oxide layer and a second doping layer disposed in sequence;

[0076] S8. Clean and remove the winding coating produced by S7 deposition on the back of the silicon wafer, then perform alkaline washing and acid washing on the silicon wafer in sequence, and then perform passivation water washing on the silicon wafer, wherein the winding coating includes a first winding coating produced by depositing a sacrificial layer, a second winding coating produced by depositing an anti-reflection layer, and a third winding coating produced by depositing a passivation layer. The cleaning solution used to remove the third winding coating is a mixed solution of hydrogen peroxide and potassium hydroxide, and the concentration ratio of hydrogen peroxide to potassium hydroxide is 1 / 10-1 / 6. The corrosion rate of polysilicon is 0.05nm / s-0.1nm / s.

[0077] It should be noted that, in S1, the silicon wafer is preferably an N-type single crystal silicon wafer, and the silicon wafer can be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.

[0078] In S2, a first tunneling oxide layer is first formed by low pressure chemical vapor deposition (LPCVD). The thickness of the first tunneling oxide layer is 1nm-2nm. The deposition conditions are oxygen permeation, the deposition temperature is 550℃-700℃, and the deposition time is 5min-60min. Then, a first doping layer is formed by low pressure chemical vapor deposition (LPCVD) and high temperature diffusion annealing method. The first doping layer is an N-type doped polysilicon layer with a thickness of 70nm-300nm.

[0079] In S3, the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 1%-5%, the cleaning time is 1min-3min, and the cleaning temperature is 25°C.

[0080] In S4, a mask layer is formed by plasma enhanced chemical vapor deposition (PECVD), the mask layer is a silicon nitride layer, and the thickness of the mask layer is 50nm-90nm.

[0081] In S5, laser or mask etching is used to etch openings on the first tunneling oxide layer, the first doping layer and the mask layer on the back of the silicon wafer to form a first opening area, and the mask layer and the first semiconductor layer in the first opening area are etched away. The width of the first opening area W1 is 0.4 mm-0.8 mm. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser, and the pulse width is less than 100 ns.

[0082] In S6, a texturing liquid is first used for texturing cleaning. The texturing liquid is a mixed solution of potassium hydroxide or sodium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide or sodium hydroxide is 1%-5%, and the mass percentage of the texturing additive is 0.5%-1%. The texturing time is 8min-12min, the texturing temperature is 75℃-85℃, and the texturing additive contains at least one of benzoic acid, aminotrimethylphosphoric acid, polyepoxysuccinic acid, and polyaspartic acid, that is, the texturing additive contains a certain film-forming protective agent; then a cleaning liquid is used to completely or partially remove the mask layer outside the first opening area. The cleaning liquid is a mixed solution of hydrofluoric acid and water, wherein the hydrofluoric acid concentration is 5%-10%, the cleaning temperature is 20℃-30℃, and the cleaning time is 60s-200s.

[0083] S7 includes three steps:

[0084] S71. A second tunneling oxide layer and a second doping layer are sequentially deposited on the front side of the silicon wafer by plasma enhanced chemical vapor deposition, wherein the second tunneling oxide layer has a thickness of 1nm-2nm, the second doping layer is an N-type doped polysilicon layer, and the thickness of the second doping layer is 1nm-10nm.

[0085] S72. Depositing an anti-reflection layer on the second doped layer by plasma enhanced chemical vapor deposition, wherein the anti-reflection layer comprises a first anti-reflection layer and a second anti-reflection layer disposed in sequence, and the total thickness of the anti-reflection layer is 70nm-100nm.

[0086] Specifically, S72 includes two stages:

[0087] The first stage: silane and ammonia are introduced, and react under the condition of turning on the glow to form the first anti-reflection layer, the first anti-reflection layer is a silicon nitride layer, the nitrogen content in the first anti-reflection layer is 40%-45%, the thickness of the first anti-reflection layer is 20nm-40nm, and the refractive index of the first anti-reflection layer is 2.2-2.3. Preferably, in the first stage, the reaction conditions for forming the first anti-reflection layer are: reaction temperature of 400°C-450°C, silane flow rate of 800sccm-1200sccm, ammonia flow rate of 4000sccm-6000sccm, reaction time of 300s-500s, reaction pressure of 500mtorr-3000mtorr, power of 4000W-6000W.

[0088] The second stage: silane, ammonia and laughing gas are introduced, and reacted under the condition of turning on the glow to form a second anti-reflection layer, the second anti-reflection layer is a silicon nitride layer, the nitrogen content in the second anti-reflection layer is 45%-50%, the thickness of the second anti-reflection layer is 50nm-70nm, and the refractive index of the second anti-reflection layer is 1.8-2.0. Preferably, in the second stage, the reaction conditions for forming the second anti-reflection layer are: reaction temperature is 400℃-450℃, silane flow rate is 500sccm-900sccm, ammonia flow rate is 5000sccm-8000sccm, laughing gas flow rate is 500sccm-2000sccm, reaction time is 300s-500s, reaction pressure is 500mtorr-3000mtorr, power is 4000W-6000W.

[0089] S73. Depositing a sacrificial layer on the anti-reflection layer by plasma enhanced chemical vapor deposition, wherein the thickness of the sacrificial layer is 3nm-8nm.

[0090] In S73, silane and ammonia are introduced, and reacted under the condition of turning on the glow to form a sacrificial layer, the sacrificial layer is a silicon nitride layer (the higher the nitrogen content in the silicon nitride layer, the easier it is to be corroded), the nitrogen content in the sacrificial layer is 35%-40%, and the refractive index of the sacrificial layer is 2.3-2.5. Since the nitrogen content of the sacrificial layer is low (lower than the nitrogen content of the first anti-reflection layer and lower than the nitrogen content of the second anti-reflection layer), the deposition rate is slow, so the density of the sacrificial layer is high, and it is not easy to be corroded during the subsequent hydrofluoric acid solution cleaning process, and the anti-reflection layer can be effectively protected. Preferably, the reaction conditions for forming the sacrificial layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1800sccm, ammonia flow rate of 3000sccm-5000sccm, reaction time of 40s-100s, reaction pressure of 500mtorr-3000mtorr, and power of 4000W-6000W.

[0091] S8 consists of five stages:

[0092] The first stage: the first winding coating and the second winding coating are sequentially cleaned and removed by a chain cleaning machine, wherein the cleaning solution used is an aqueous solution containing hydrofluoric acid, and the concentration of hydrofluoric acid is 5%-15%. Preferably, in the first stage, the cleaning conditions for removing the first winding coating and the second winding coating are: the reaction temperature is 20°C-35°C, the reaction time is 30s-120s, and the transmission roller speed of the chain cleaning machine is 1.2m / min-3.0m / min.

[0093] The second stage: remove the third winding coating by cleaning with a tank cleaning machine, wherein the concentration of hydrogen peroxide in the cleaning solution is 0.2%-1%, and the concentration of potassium hydroxide is 2%-5%. Preferably, in the second stage, the cleaning conditions for removing the third winding coating are: the reaction temperature is 25°C-35°C, and the reaction time is 60s-240s.

[0094] Furthermore, in the cleaning solution, the concentration ratio of hydrogen peroxide to potassium hydroxide is 1 / 10-1 / 6. At this concentration ratio, the corrosion rate of the cleaning solution on polysilicon is 0.05nm / s-0.1nm / s. Compared with the technology of removing polysilicon with pure alkali solution in the prior art, the corrosion rate is greatly reduced, and the thickness of the first doped layer on the back of the silicon wafer is reduced, ensuring that its passivation performance is not affected, and the velvet pyramid morphology of the opening area will not change, ensuring that its reflectivity and anti-reflection effect are not affected, thereby improving the short-circuit current of the battery.

[0095] The third stage: alkaline washing the silicon wafer, wherein the alkaline washing solution used is a mixed solution of ammonia water or potassium hydroxide and hydrogen peroxide, the concentration of ammonia water or potassium hydroxide is 2%-5%, and the concentration of hydrogen peroxide is 3%-5%. Preferably, in the third stage, the alkaline washing conditions are: reaction temperature is 60℃-80℃, and reaction time is 120s-240s.

[0096] The fourth stage: pickling the silicon wafer, wherein the pickling solution used is a mixed solution of hydrochloric acid and hydrogen peroxide, the concentration of hydrochloric acid is 2%-5%, and the concentration of hydrogen peroxide is 3%-5%. Preferably, in the fourth stage, the pickling conditions are: reaction temperature is 60℃-80℃, and reaction time is 120s-240s.

[0097] The fifth stage: the silicon wafer is passivated and washed with water, wherein the washing solution used is an aqueous solution containing hydrofluoric acid, and the concentration of hydrofluoric acid is 1%-5%. Preferably, in the fifth stage, the passivation washing conditions are: the reaction temperature is 10°C-20°C, and the reaction time is 60s-180s.

[0098] Furthermore, in the prior art, the reaction temperature of the passivation water washing is generally controlled at room temperature (25°C-30°C), while in the present invention, in order to reduce the rate at which hydrofluoric acid corrodes silicon nitride, the reaction temperature is controlled between 10°C-20°C, so that the sacrificial layer on the front of the silicon wafer is slowly and evenly corroded at a rate of less than 0.05nm / s. At the same time, due to the low corrosion rate, the sacrificial layer on the front of the silicon wafer does not need to be very thick. Under the condition that the anti-reflection layer is completely intact, even if the sacrificial layer is not completely removed, it will not affect the anti-reflection effect of the anti-reflection layer, thereby ensuring the short-circuit current of the battery.

[0099] Preferably, after S8, the battery preparation method further comprises:

[0100] S9. depositing a second semiconductor layer on the back side of the silicon wafer so that a portion of the second semiconductor layer covers a side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer, wherein the second semiconductor layer includes an intrinsic amorphous silicon layer and a third doped layer disposed in sequence;

[0101] S10. Etching openings on the second semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;

[0102] S11. Forming a conductive film layer on the back side of the silicon wafer;

[0103] S12. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the second semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0104] S13. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0105] It should be noted that, in S9, the thickness of the intrinsic amorphous silicon layer is 5nm-15nm, and the third doped layer is a P-type doped amorphous or microcrystalline silicon layer, and the thickness thereof is 5nm-20nm.

[0106] In S10, an opening is etched on the second semiconductor layer on the back of the silicon wafer by laser or mask etching to form a second opening area, and the second semiconductor layer in the second opening area is etched away. The width of the second opening area W2 is 100 μm-300 μm. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser, and the pulse width is less than 100 ns.

[0107] In S11, a conductive film layer is deposited on the back of the silicon wafer using physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD). The thickness of the conductive film layer is 40nm-80nm. The material of the conductive film layer can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0108] In S12, an isolation groove is formed on the conductive film layer by laser or etching. The isolation groove is used to achieve the insulation function between two adjacent parts of the conductive film layer. The isolation groove is located between the first opening area and the second opening area. The width of the isolation groove W3 is 50μm-200μm. After the isolation groove is formed, the resistance between the first semiconductor layer and the second semiconductor layer is greater than 1KΩ.

[0109] In S13, a first electrode is formed on a portion of the conductive film layer located in a first opening area on the back side of the silicon wafer by using screen printing technology, and a second electrode is formed on a portion of the conductive film layer located in a second opening area on the back side of the silicon wafer.

[0110] In a second aspect, the present invention provides a back-contact battery, which is prepared by the above-mentioned battery preparation method.

[0111] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0112] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0113] Example 1

[0114] A back contact battery is prepared by the following steps:

[0115] S1. Figure 1 As shown, the N-type single crystal silicon wafer is double-sided polished and cleaned, and the silicon wafer 1 is a Czochralski single crystal silicon wafer.

[0116] S2. Figure 2 As shown, a first semiconductor layer is deposited on the back of a silicon wafer 1 by low pressure chemical vapor deposition (LPCVD) and high temperature diffusion annealing method, wherein the first semiconductor layer includes a first tunneling oxide layer 2 and a first doping layer 3 arranged in sequence, the thickness of the first tunneling oxide layer 2 is 1.5 nm, the thickness of the first doping layer 3 is 200 nm, and the effective doping concentration of the first doping layer 3 is 5e20 cm -3 Specifically, the deposition conditions of the first tunnel oxide layer 2 are: oxygen permeation, deposition temperature of 625° C., and deposition time of 30 min.

[0117] S3. Cleaning and removing the phosphosilicate glass layer produced by the deposition of S2 on the first doping layer 3, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the concentration of hydrofluoric acid is 3%, the cleaning time is 2 minutes, and the cleaning temperature is 25°C.

[0118] S4. Figure 2 As shown, a mask layer 4 is formed on the first doping layer 3 by plasma enhanced chemical vapor deposition (PECVD), and the thickness of the mask layer 4 is 70 nm.

[0119] S5. Figure 3 As shown, laser etching is used to etch openings on the mask layer 4, the first doped layer 3 and the first tunneling oxide layer 2 to form a first opening area, and the mask layer 4, the first doped layer 3 and the first tunneling oxide layer 2 in the first opening area are etched away. The width of the first opening area W1 is 0.6 mm, and the laser used for etching is a green laser with a pulse width of 50 ns.

[0120] S6. Figure 3 As shown, firstly, the first tunneling oxide layer 2 and the first doping layer 3 remaining in the first opening area are removed by texturing cleaning, and a texturing surface is formed in the first opening area and on the front side of the silicon wafer 1 at the same time. The texturing liquid used is a mixed solution of potassium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide is 3%, and the mass percentage of the texturing additive is 0.75%. The texturing time is 10 minutes, the texturing temperature is 80°C, and the texturing additive includes benzoic acid and aminotrimethylphosphonic acid; then, the mask layer 4 outside the first opening area is completely removed by cleaning, and the cleaning liquid used is a mixed solution of hydrofluoric acid and water, wherein the hydrofluoric acid concentration is 7%, the cleaning temperature is 25°C, and the cleaning time is 130 seconds.

[0121] S7. Figure 4 As shown, a passivation layer, an anti-reflection layer and a sacrificial layer 9 are sequentially deposited on the front side of the silicon wafer 1 by plasma enhanced chemical vapor deposition, wherein the passivation layer includes a second tunneling oxide layer 5 and a second doping layer 6 arranged in sequence, the second tunneling oxide layer 5 has a thickness of 1.5 nm, the second doping layer 6 has a thickness of 5 nm, the anti-reflection layer includes a first anti-reflection layer 7 and a second anti-reflection layer 8 arranged in sequence, the first anti-reflection layer 7 has a thickness of 30 nm, the second anti-reflection layer 8 has a thickness of 70 nm, and the sacrificial layer 9 has a thickness of 5 nm. Specifically, the reaction conditions for forming the first anti-reflection layer 7 are as follows: reaction temperature of 440° C., silane flow rate of 1000 sccm, ammonia flow rate of 5000 sccm, reaction time of 300 s, reaction pressure of 1700 mtorr, power of 5000 W, nitrogen content in the first anti-reflection layer 7 of 42%, and refractive index of the first anti-reflection layer 7 of 2.25; the reaction conditions for forming the second anti-reflection layer 8 are as follows: reaction temperature of 440° C., silane flow rate of 700 sccm, ammonia flow rate of 7000 sccm, and laughing gas flow rate of 10 00sccm, reaction time is 400s, reaction pressure is 1700mtorr, power is 5000W, the nitrogen content in the second anti-reflection layer 8 is 47%, and the refractive index of the second anti-reflection layer 8 is 1.9; the reaction conditions for forming the sacrificial layer 9 are: reaction temperature is 440°C, silane flow rate is 1500sccm, ammonia flow rate is 4000sccm, reaction time is 70s, reaction pressure is 1700mtorr, power is 5000W, the nitrogen content in the sacrificial layer 9 is 38%, and the refractive index of the sacrificial layer 9 is 2.4.

[0122] S8. Figure 5As shown, the winding coating produced by S7 deposition on the back of the silicon wafer 1 is cleaned and removed, and then the silicon wafer 1 is alkaline washed and acid washed in sequence, and then the silicon wafer 1 is passivated and washed with water, and the sacrificial layer 9 is removed. Specifically, the first winding coating and the second winding coating are cleaned and removed in sequence by a chain cleaning machine, and the cleaning solution used is an aqueous solution containing hydrofluoric acid, and the hydrofluoric acid concentration is 10%. The cleaning conditions are: the reaction temperature is 30°C, the reaction time is 45s, and the chain cleaning machine drive roller speed is 2.0m / min; then the third winding coating is cleaned and removed by a tank cleaning machine, and the cleaning solution used has a hydrogen peroxide concentration of 0.5%, a potassium hydroxide concentration of 3.5%, and a concentration ratio of hydrogen peroxide to potassium hydroxide of 1 / 7. At this concentration ratio, the corrosion rate of the cleaning solution on polysilicon is 0.07nm / s, and the cleaning conditions are: the reaction temperature is 30°C, and the reaction time is The reaction time is 150s; then the silicon wafer 1 is alkaline washed, and the alkaline washing solution used is a mixed solution of ammonia water and hydrogen peroxide, the ammonia concentration is 3%, the hydrogen peroxide concentration is 4%, and the alkaline washing conditions are: the reaction temperature is 70°C, and the reaction time is 180s; then the silicon wafer 1 is acid washed, and the acid washing solution used is a mixed solution of hydrochloric acid and hydrogen peroxide, the hydrochloric acid concentration is 2%, and the hydrogen peroxide concentration is 4%, and the acid washing conditions are: the reaction temperature is 70°C, and the reaction time is 180s; finally, the silicon wafer 1 is passivated and washed with water, and the washing solution used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 2%, and the passivation washing conditions are: the reaction temperature is 15°C, and the reaction time is 120s.

[0123] S9. Figure 6 As shown, a second semiconductor layer is deposited on the back side of the silicon wafer 1 so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer 1, and the other portion extends into the first opening area and covers the silicon wafer 1. The second semiconductor layer includes an intrinsic amorphous silicon layer 10 and a third doped layer 11 arranged in sequence. The thickness of the intrinsic amorphous silicon layer 10 is 10 nm, and the thickness of the third doped layer 11 is 12 nm.

[0124] S10. Figure 7 As shown, laser etching is used to etch openings on the second semiconductor layer to form second opening areas that are alternately arranged with the first opening areas and spaced apart, and the second semiconductor layer in the second opening areas is etched away. The width of the second opening area W2 is 200μm, and the etching laser is a green laser with a pulse width of 50ns.

[0125] S11. Figure 8 As shown, a conductive film layer 12 is formed on the back of the silicon wafer 1 by physical vapor deposition (PVD) technology. The thickness of the conductive film layer 12 is 60 nm, and the material of the conductive film layer 12 is a tin oxide-doped indium oxide film.

[0126] S12. Fig. 9As shown, an isolation groove is formed on the conductive film layer 12 by laser etching, so that a portion of the conductive film layer 12 separated from each other extends into the first opening area and covers the second semiconductor layer, and another portion extends into the second opening area and covers the first semiconductor layer. The width of the isolation groove W3 is 120μm. After the isolation groove is formed, the resistance between the first semiconductor layer and the second semiconductor layer is 2KΩ.

[0127] S13. Fig.10 As shown, a first electrode 13 is formed on a portion of the conductive film layer 12 extending into the first opening region, and a second electrode 14 is formed on a portion of the conductive film layer 12 extending into the second opening region by using screen printing technology.

[0128] Example 2

[0129] The method of Example 1 is referred to, except that the thickness of the sacrificial layer 9 is adjusted to 3 nm, and the nitrogen content in the sacrificial layer 9 is 40%.

[0130] Example 3

[0131] The method of Example 1 is referred to, except that the cleaning method in S8 is adjusted, and the third winding coating is removed by cleaning in a tank cleaning machine. The hydrogen peroxide concentration of the cleaning solution used is 0.2%, and the potassium hydroxide concentration is 2%. The concentration ratio of hydrogen peroxide to potassium hydroxide is 1 / 10. At this concentration ratio, the corrosion rate of the cleaning solution on polysilicon is 0.05nm / s. The cleaning conditions are: reaction temperature is 25°C, and reaction time is 60s.

[0132] Example 4

[0133] The method of Example 1 is referred to, except that the cleaning conditions in S8 are adjusted, the silicon wafer 1 is passivated and washed with water, the washing solution used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 1%, and the passivation washing conditions are: the reaction temperature is 10°C, and the reaction time is 80s.

[0134] Comparative Example 1

[0135] The method of Example 1 is referred to, except that the thickness of the sacrificial layer 9 is adjusted to 3 nm, and the nitrogen content in the sacrificial layer 9 is adjusted to 45%.

[0136] Comparative Example 2

[0137] The method of Example 1 is referred to, except that the process step S73 is eliminated.

[0138] Comparative Example 3

[0139] The method of Example 1 is referred to, except that the cleaning method in S8 is adjusted, and the third winding coating is removed by cleaning in a tank cleaning machine. The hydrogen peroxide concentration of the cleaning solution used is 0.1%, the potassium hydroxide concentration is 2%, and the concentration ratio of hydrogen peroxide to potassium hydroxide is 1 / 20. At this concentration ratio, the corrosion rate of the cleaning solution on polysilicon is 0.6nm / s, and the cleaning conditions are: reaction temperature is 30°C, and reaction time is 120s.

[0140] Comparative Example 4

[0141] The method of Example 1 is followed, except that the cleaning conditions in S8 are adjusted, the silicon wafer 1 is passivated and washed with water, the washing solution used is an aqueous solution containing hydrofluoric acid, the hydrofluoric acid concentration is 7%, and the passivation washing conditions are: reaction temperature is 30°C, and reaction time is 200s.

[0142] Test Case

[0143] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in the following performance index comparison table.

[0144] Performance index comparison table:

[0145]

[0146] It can be seen from the above performance index comparison table that, relative to the comparative example, the embodiment scheme of the present invention is adopted, and the silicon wafer 1 is cleaned by a mixed solution of hydrogen peroxide and potassium hydroxide in a certain concentration ratio range to remove the coating layer, so as to greatly reduce the corrosion rate of the passivation film layer, avoid affecting the passivation performance of the first semiconductor layer, and avoid affecting the suede reflectivity in the first opening area, thereby ensuring the short-circuit current of the battery; and the anti-reflection layer is protected by a sacrificial layer 9 arranged outside the anti-reflection layer to avoid damage to the anti-reflection layer during the passivation water washing process, thereby further ensuring the short-circuit current of the battery and improving the battery efficiency.

[0147] Furthermore, according to Example 1 and Examples 2-4, it can be seen that the preferred battery structure of the present invention is more conducive to reducing optical absorption while ensuring conductivity, ensuring the passivation effect, increasing short-circuit current, and improving battery conversion efficiency.

[0148] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a battery, characterized in that: The following steps are involved: S1. Provide double-sided polished silicon wafers; S2. depositing a first semiconductor layer on the back side of the silicon wafer, wherein the first semiconductor layer comprises a first tunneling oxide layer and a first doping layer arranged in sequence; S3. Cleaning and removing the phosphosilicate glass layer produced by the deposition of S2 on the first doped layer; S4. forming a mask layer on the first doped layer; S5. Etching an opening on the first tunneling oxide layer, the first doping layer and the mask layer to form a first opening region; S6. Removing the first tunneling oxide layer and the first doping layer remaining in the first opening region by texturing and cleaning, and forming a texturing surface in the first opening region and on the front side of the silicon wafer at the same time, and then completely or partially removing the mask layer outside the first opening region by cleaning; S7. depositing a passivation layer, an anti-reflection layer and a sacrificial layer on the front side of the silicon wafer in sequence, wherein the passivation layer comprises a second tunneling oxide layer and a second doping layer arranged in sequence, the sacrificial layer is a silicon nitride layer, and the nitrogen content in the sacrificial layer is 35%-40%; S8. Clean and remove the winding coating produced by the deposition in S7 on the back of the silicon wafer, then perform alkali cleaning and acid cleaning on the silicon wafer in sequence, and then perform passivation water washing on the silicon wafer, wherein the winding coating includes a first winding coating produced by depositing the sacrificial layer, a second winding coating produced by depositing the anti-reflection layer, and a third winding coating produced by depositing the passivation layer, and the cleaning solution used to remove the third winding coating is a mixed solution of hydrogen peroxide and potassium hydroxide, the concentration ratio of hydrogen peroxide to potassium hydroxide is 1 / 10-1 / 6, and the corrosion rate of polysilicon is 0.05nm / s-0.1nm / s, including: The first winding coating and the second winding coating are sequentially cleaned and removed by a chain cleaning machine, wherein the cleaning solution used is an aqueous solution containing hydrofluoric acid, and the concentration of hydrofluoric acid is 5%-15%; The third winding coating is removed by cleaning with a tank cleaning machine, wherein the concentration of hydrogen peroxide in the cleaning solution is 0.2%-1%, and the concentration of potassium hydroxide is 2%-5%; The silicon wafer is subjected to alkaline washing, wherein the alkaline washing solution used is a mixed solution of ammonia water or potassium hydroxide and hydrogen peroxide, the concentration of ammonia water or potassium hydroxide is 2%-5%, and the concentration of hydrogen peroxide is 3%-5%; The silicon wafer is pickled, wherein the pickling solution used is a mixed solution of hydrochloric acid and hydrogen peroxide, the concentration of hydrochloric acid is 2%-5%, and the concentration of hydrogen peroxide is 3%-5%; The silicon wafer is passivated and washed with water, wherein the washing solution used is an aqueous solution containing hydrofluoric acid, and the concentration of hydrofluoric acid is 1%-5%.

2. The battery preparation method according to claim 1, characterized in that: S7 includes: S71. Depositing the second tunneling oxide layer and the second doping layer in sequence on the front side of the silicon wafer by plasma enhanced chemical vapor deposition, wherein the thickness of the second tunneling oxide layer is 1nm-2nm, and the thickness of the second doping layer is 1nm-10nm; S72. Depositing the anti-reflection layer on the second doped layer by plasma enhanced chemical vapor deposition, wherein the anti-reflection layer comprises a first anti-reflection layer and a second anti-reflection layer disposed in sequence, and the total thickness of the anti-reflection layer is 70nm-100nm; S73. Depositing the sacrificial layer on the anti-reflection layer by plasma enhanced chemical vapor deposition, wherein the sacrificial layer has a thickness of 3 nm to 8 nm.

3. The battery preparation method according to claim 2, characterized in that: S72 includes: Silane and ammonia are introduced and reacted under the condition of turning on the glow to form the first anti-reflection layer, wherein the first anti-reflection layer is a silicon nitride layer, the nitrogen content in the first anti-reflection layer is 40%-45%, the thickness of the first anti-reflection layer is 20nm-40nm, and the refractive index of the first anti-reflection layer is 2.2-2.3; Silane, ammonia and laughing gas are introduced and reacted under the condition of turning on the glow to form the second anti-reflection layer, the second anti-reflection layer is a silicon nitride layer, the nitrogen content in the second anti-reflection layer is 45%-50%, the thickness of the second anti-reflection layer is 50nm-70nm, and the refractive index of the second anti-reflection layer is 1.8-2.

0.

4. The battery preparation method according to claim 3, characterized in that: The reaction conditions for forming the first anti-reflection layer are: reaction temperature of 400° C.-450° C., silane flow rate of 800 sccm-1200 sccm, ammonia flow rate of 4000 sccm-6000 sccm, reaction time of 300 s-500 s, reaction pressure of 500 mtorr-3000 mtorr, and power of 4000 W-6000 W; And / or, the reaction conditions for forming the second anti-reflection layer are: reaction temperature of 400°C-450°C, silane flow rate of 500sccm-900sccm, ammonia flow rate of 5000sccm-8000sccm, nitrous oxide flow rate of 500sccm-2000sccm, reaction time of 300s-500s, reaction pressure of 500mtorr-3000mtorr, and power of 4000W-6000W.

5. The battery preparation method according to claim 2, characterized in that: S73 includes: Silane and ammonia are introduced and reacted under the condition of turning on the glow to form the sacrificial layer, and the refractive index of the sacrificial layer is 2.3-2.

5.

6. The battery preparation method according to claim 5, characterized in that: The reaction conditions for forming the sacrificial layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1800sccm, ammonia flow rate of 3000sccm-5000sccm, reaction time of 40s-100s, reaction pressure of 500mtorr-3000mtorr, and power of 4000W-6000W.

7. The battery preparation method according to claim 1, characterized in that: The cleaning conditions for removing the first winding coating and the second winding coating are as follows: the reaction temperature is 20°C-35°C, the reaction time is 30s-120s, and the transmission roller speed of the chain cleaning machine is 1.2m / min-3.0m / min; And / or, the cleaning conditions for removing the third winding coating are: reaction temperature is 25° C.-35° C., reaction time is 60s-240s; And / or, the alkaline washing conditions are: reaction temperature is 60°C-80°C, reaction time is 120s-240s; And / or, the pickling conditions are: reaction temperature is 60°C-80°C, reaction time is 120s-240s; And / or, the passivation water washing conditions are: reaction temperature is 10°C-20°C, and reaction time is 60s-180s.

8. The battery preparation method according to claim 1, characterized in that: After S8, the battery preparation method further includes: S9. depositing a second semiconductor layer on the back side of the silicon wafer, so that a portion of the second semiconductor layer covers a side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer, wherein the second semiconductor layer includes an intrinsic amorphous silicon layer and a third doped layer arranged in sequence; S10. Etching openings on the second semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart from each other; S11 forming a conductive film layer on the back side of the silicon wafer; S12. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening area and covers the second semiconductor layer, and another portion extends into the second opening area and covers the first semiconductor layer; S13. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

9. A back contact battery, characterized in that: The battery is prepared by the battery preparation method according to any one of claims 1 to 8.

10. A photovoltaic module, characterized in that: Comprising a back contact cell as claimed in claim 9.

Citation Information

Patent Citations

  • Back contact heterojunction solar cell capable of improving insulation isolation effect and manufacturing method thereof

    CN114038922A

  • Winding plating removing method and preparation method of tunneling oxide layer passivation contact solar cell

    CN114400260A

  • High-current-density back contact battery, preparation method thereof and photovoltaic module

    CN118156324A

  • Preparation method of heterojunction solar cell and heterojunction solar cell

    CN118198196A

  • Manufacturing method of back contact battery

    CN118198200A