Reaction liquid for RAFT polymerization and method for producing reaction liquid for RAFT polymerization

By using the reaction solution of RAFT agent, water-soluble inorganic base and polymerization initiator in aqueous RAFT polymerization, the problem of insufficient mixing in the reaction system is solved, the reaction time is shortened, the molecular weight distribution of the product is narrowed, and clotting is reduced. creation of things.

CN118829660APending Publication Date: 2024-10-22TECHNO UMG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025054.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-24
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing RAFT polymerization, the RAFT agent, monomer and polymerization initiator are not fully mixed in the reaction system, resulting in problems such as prolonged reaction time, increased agglomeration and wide molecular weight distribution.

Method used

By using a reaction solution containing a RAFT agent, a water-soluble inorganic base and a polymerization initiator in aqueous RAFT polymerization, the acid group molar ratio is adjusted so that the acidic groups of the RAFT agent and the water-soluble inorganic base form salts to ensure uniformity in the reaction solution. and dispersion, avoiding the addition of additional emulsifiers.

Benefits of technology

The RAFT agent and its products are fully dispersed in the water system, the reaction time is shortened, the yield and molecular weight distribution of the product are increased, and the amount of clots is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023058860000051
    Figure BDA0005023058860000051
  • Figure BDA0005023058860000121
    Figure BDA0005023058860000121
  • Figure BDA0005023058860000131
    Figure BDA0005023058860000131
Patent Text Reader

Abstract

A reaction solution for RAFT polymerization, which contains a RAFT agent represented by a specific chemical formula, which has an acid group that forms a salt, water, and a water-soluble inorganic base, and which may contain a polymerization initiator as an arbitrary component. The molar ratio (M3 / (M1 + M2)) of the number of moles (M1) of the acid groups forming the salt, the number of moles (M2) of the acid groups of the salt that can form the polymerization initiator, and the number of moles (M3) of the water-soluble inorganic base is 1.0-10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a reaction solution for RAFT polymerization and a method for producing a reaction solution for RAFT polymerization. This application claims priority based on Japanese Patent Application No. 2022-053655 filed in Japan on March 29, 2022 and Japanese Patent Application No. 2022-053659 filed in Japan on March 29, 2022, and the contents thereof are incorporated herein by reference. Background Art

[0002] In the past, RAFT polymerization (Reversible Addition-Fragmentation Chain Transfer) was known. According to RAFT polymerization, not only a polymer with a narrow molecular weight distribution can be formed, but also a block copolymer containing multiple blocks can be easily formed. Various proposals have been made for the RAFT agent that is indispensable for such RAFT polymerization (for example, Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent document 1: Japanese Patent No. 4405807. Summary of the invention

[0006] Technical problem to be solved by the invention

[0007] The essence of RAFT polymerization is living radical polymerization. In other radical polymerizations, the terminal of the polymer formed by chain transfer or stop reaction is no longer polymerized, and the polymer active species die. However, the terminal of the polymer formed in RAFT polymerization is not dead, and the terminal of the polymer can continue to polymerize when the monomer is added. Although RAFT polymerization has such an excellent reaction mechanism, the RAFT agent, monomer and polymerization initiator must exist in the same phase of the reaction system. The reaction system of conventional RAFT polymerization is an emulsion reaction system in which hydrophobic monomers are dispersed in the form of oil droplets in the water phase and emulsified. It is very important to fully mix the RAFT agent and the polymerization initiator with the monomer. In other words, an emulsifier is often used in water-based RAFT polymerization. However, this mixing is not necessarily effective, and there are problems such as a longer reaction time and more coagulum (reaction residue).

[0008] In order to solve the above problems, the present invention focuses on a RAFT agent and provides a reaction solution for RAFT polymerization suitable for aqueous RAFT polymerization and a method for producing the reaction solution for RAFT polymerization.

[0009] Means used to solve problems

[0010] [1-1] A reaction liquid for RAFT polymerization, characterized in that the reaction liquid for RAFT polymerization contains a RAFT agent represented by the following formula (1), water and a water-soluble inorganic base, and may contain a polymerization initiator as an arbitrary component, the molar ratio M3 / (M3+M2) of the number of moles M1 of acid groups possessed by the RAFT agent, the number of moles M2 of acid groups that the polymerization initiator may have, and the number of moles M3 of the water-soluble inorganic base is 1.0 to 10, and at least a portion of the acid groups possessed by the RAFT agent and at least a portion of the acid groups that the polymerization initiator may have form a salt with the cationic component of the water-soluble inorganic base.

[0011] [1-2] The reaction solution for RAFT polymerization according to [1-1], wherein in the above formula (1), Z is an alkylthio group which may be substituted.

[0012] [1-3] The reaction solution for RAFT polymerization according to [1-1] or [1-2], wherein the polymerization initiator is a water-soluble polymerization initiator.

[0013] [1-4] A reaction solution for RAFT polymerization, characterized in that it contains a polymeric RAFT agent represented by the following formula (2), water and a water-soluble inorganic base, wherein at least a part of the acid groups of the polymeric RAFT agent forms a salt with a cationic component of the water-soluble inorganic base.

[0014] [1-5] The reaction solution for RAFT polymerization according to [1-4], wherein the R 1 It is an organic group having a carbon atom bonded to the above X, and the carbon atom of the above organic group is a tertiary carbon.

[0015] [1-6] The reaction solution for RAFT polymerization according to [1-4], wherein the R 1 The above X is methacrylate, the above R 1 It is an organic group having a carbon atom bonded to the above X, wherein the carbon atom of the above organic group is a quaternary carbon, and a cyano group is bonded to the carbon atom.

[0016] [1-7] A reaction liquid for RAFT polymerization, characterized in that it contains a hydrophilic polymeric RAFT agent represented by the following formula (3), water and a water-soluble inorganic base, wherein at least a part of the acid groups possessed by the above hydrophilic polymeric RAFT agent forms a salt with the cationic component of the above water-soluble inorganic base.

[0017] [1-8] The reaction solution for RAFT polymerization according to any one of [1-1] to [1-7], wherein the RAFT agent is one or more selected from the group consisting of the following formulae (1a) to (1n).

[0018] [1-9] The reaction solution for RAFT polymerization according to any one of [1-1] to [1-8], wherein the polymerization initiator is selected from one or more of the following: inorganic peroxides such as potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide; organic peroxides such as benzoyl peroxide and isobutyryl peroxide; azo compounds such as azobisisobutyronitrile, 4-methoxy-azobisvaleronitrile, and 4,4'-azobis(4-cyanovaleric acid); a redox initiator composed of an organic peroxide, ferrous sulfate, a chelating agent, and a reducing agent, such as an initiator composed of isopropyl hydroperoxide, ferrous sulfate, sodium pyrophosphate, and dextrose; or an initiator composed of tert-butyl hydroperoxide, sodium formaldehyde sulfoxylate (Rongalite), ferrous sulfate, and disodium ethylenediaminetetraacetic acid.

[0019] [1-10] The reaction solution for RAFT polymerization according to any one of [1-1] to [1-8], further comprising an ethylenically unsaturated monomer, wherein the ethylenically unsaturated monomer is one or more selected from the group consisting of compounds represented by the following formula (10).

[0020] [2-1] A method for producing a reaction solution for RAFT polymerization, comprising:

[0021] Step 1, mixing a RAFT agent having an acid group represented by the following formula (1), water and a water-soluble inorganic base, so that at least a part of the acid groups of the RAFT agent and a cation derived from the water-soluble inorganic base form a salt, thereby obtaining a RAFT agent aqueous solution in which the RAFT agent is dissolved in water; and

[0022] In step 2, a water-soluble polymerization initiator and an ethylenically unsaturated monomer are added to the above-mentioned RAFT agent aqueous solution, and the mixture is stirred to cause the above-mentioned ethylenically unsaturated monomer dispersed in water to undergo RAFT polymerization, thereby obtaining a RAFT polymerization reaction solution (A) in which the polymeric RAFT agent represented by formula (2) is dispersed in water.

[0023] [2-2] The method for producing a reaction solution for RAFT polymerization according to [2-1], wherein the pH of the reaction solution for RAFT polymerization (A) obtained in the step 2 is 8 to 13.

[0024] [2-3] A method for producing a reaction solution for RAFT polymerization according to [2-1] or [2-2], wherein, in the reaction solution after adding the ethylenically unsaturated monomer and the water-soluble polymerization initiator to the aqueous solution of the RAFT agent and immediately before the start of polymerization, the molar ratio (M4+M5) / (M1+M2) of the number of moles M1 of the acid group possessed by the RAFT agent, the number of moles M2 of the acid group arbitrarily possessed by the water-soluble polymerization initiator, the number of moles M4 of the water-soluble inorganic base added in the step 1, and the number of moles M5 of the water-soluble inorganic base that may be arbitrarily added in the step 2 is 1.0 to 10.

[0025] [2-4] A method for producing a reaction liquid for RAFT polymerization according to any one of [2-1] to [2-3], which further includes the following step 3, namely, adding an ethylenically unsaturated monomer to the reaction liquid for RAFT polymerization (A) obtained in the above step 2, stirring, and subjecting the above ethylenically unsaturated monomer dispersed in water to RAFT polymerization, thereby obtaining a RAFT polymerization reaction liquid (B) in which a hydrophilic copolymeric RAFT agent represented by formula (3) is dispersed in water.

[0026] [2-5] The method for producing a reaction solution for RAFT polymerization according to [2-4], wherein the pH of the reaction solution for RAFT polymerization (B) obtained in the step 3 is 8 to 13.

[0027] [2-6] The method for producing a reaction solution for RAFT polymerization according to [2-4] or [2-5], wherein in the step 3, a water-soluble polymerization initiator is added to the reaction solution for RAFT polymerization (A).

[0028] [2-7] The method for producing a reaction solution for RAFT polymerization according to any one of [2-1] to [2-6], wherein the RAFT agent is one or more selected from the group consisting of the following formulae (1a) to (1n).

[0029] [2-8] The method for producing a reaction solution for RAFT polymerization according to any one of [2-1] to [2-7], wherein the polymerization initiator is selected from one or more of the following: inorganic peroxides such as potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide; organic peroxides such as benzoyl peroxide and isobutyryl peroxide; azo compounds such as azobisisobutyronitrile, 4-methoxy-azobisvaleronitrile, and 4,4'-azobis(4-cyanovaleric acid); a redox initiator composed of an organic peroxide, ferrous sulfate, a chelating agent, and a reducing agent, such as an initiator composed of isopropyl hydroperoxide, ferrous sulfate, sodium pyrophosphate, and glucose; or an initiator composed of tert-butyl hydroperoxide, sodium formaldehyde sulfoxylate (Rongalite), ferrous sulfate, and disodium ethylenediaminetetraacetic acid.

[0030] [2-9] The method for producing a reaction solution for RAFT polymerization according to any one of [2-1] to [2-8], wherein the ethylenically unsaturated monomer is one or more selected from compounds represented by the following formula (10).

[0031] Effects of the Invention

[0032] According to the reaction solution for RAFT polymerization of the present invention, the acid group of the RAFT agent forms a salt, and the ratio of the number of moles of the acid group M1 forming the salt, the number of moles of the water-soluble inorganic base M3 in the reaction solution, and the number of moles of the acid group M2 of the polymerization initiator, i.e., M3 / (M1+M2), is within a specific range, so that good RAFT polymerization can be performed. In this case, without adding other emulsifiers to the aqueous RAFT polymerization reaction solution, each RAFT agent and its reaction product can be fully dispersed in the aqueous reaction solution.

[0033] According to the method for producing a reaction liquid for RAFT polymerization of the present invention, a reaction liquid for RAFT polymerization in which a polymeric RAFT agent is dispersed in water can be produced through step 1 (a step of forming a salt from an acid group of the RAFT agent) and step 2 (a step of reacting the RAFT agent having formed a salt with an ethylenically unsaturated monomer to obtain a polymeric RAFT agent). By adding an ethylenically unsaturated monomer to the prepared aqueous reaction liquid for RAFT polymerization, good RAFT polymerization can be performed. At this time, without adding other emulsifiers to the aqueous reaction liquid for RAFT polymerization, the polymeric RAFT agent and its reaction product can be fully dispersed in the aqueous reaction liquid. DETAILED DESCRIPTION

[0034] The following definitions of terms apply throughout this specification and claims.

[0035] "(Meth)acrylate" means acrylate or methacrylate.

[0036] The expression "C1 to C6" means "the number of carbon atoms is 1 to 6", and "C" in this expression is an abbreviation indicating the number of carbon atoms.

[0037] The term “to” indicating a numerical range means that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0038] <<First option>>

[0039] A first embodiment of the present invention is a reaction solution for RAFT polymerization, which comprises a RAFT agent represented by formula (1), water and a water-soluble inorganic base, and may further contain a polymerization initiator as an optional component.

[0040]

[0041] [In formula (1), R 1 represents an organic group, the organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z is an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, and a part of the organic group represented by Z may be substituted.]

[0042] At least a part of the acid groups of the RAFT agent forms a salt. When the RAFT agent has one acid group in the molecule, the number of moles of the acid groups of the RAFT agent contained in the reaction solution for RAFT polymerization of this embodiment is the same as the number of moles of the molecules of the RAFT agent. When the number of acid groups in the RAFT agent molecule is m, the number of moles of the acid groups of the RAFT agent contained in the reaction solution for RAFT polymerization of this embodiment is represented by the number of moles of the molecules of the RAFT agent × m.

[0043] The polymerization initiator as an optional component may or may not have an acid group. When the polymerization initiator has an acid group, at least a part of the acid group may or may not form a salt, but from the viewpoint of fully obtaining the effect of the present invention, it is preferred to form a salt. As the type of acid group possessed by the polymerization initiator, the same acid groups as exemplified in the acid groups of the above-mentioned RAFT agent can be cited. When the number of acid groups possessed by the polymerization initiator molecule is n, the number of moles of the acid groups of the polymerization initiator contained in the reaction solution for RAFT polymerization of this embodiment is represented by the number of moles of molecules of the polymerization initiator × n.

[0044] In the reaction liquid for RAFT polymerization of the first embodiment, the molar ratio M3 / (M3+M2) of the molar number M1 of the acid group possessed by the above-mentioned RAFT agent, the molar number M2 of the acid group possessed by the above-mentioned polymerization initiator, and the molar number M3 of the above-mentioned water-soluble inorganic base is 1.0 to 10, preferably 1.5 to 7.0, more preferably 2.0 to 5.0, further preferably 2.5 to 4.5, and particularly preferably 3.0 to 4.0.

[0045] When it is at least the lower limit of the above range, the reaction time of RAFT polymerization can be shortened, the yield of the target product can be improved, the amount of agglomerates can be reduced, and the molecular weight distribution of the target product can be narrowed.

[0046] When it is at most the upper limit of the above range, the pH of the reaction solution for RAFT polymerization in the present embodiment can be prevented from becoming too high, and the volume average particle size (MV) of the target product can be reduced.

[0047] The RAFT agent contained in the reaction liquid for RAFT polymerization of the first embodiment may be one kind or two or more kinds. The molar number M1 is the total molar number of the acid groups of all the RAFT agents.

[0048] The polymerization initiator contained in the reaction liquid for RAFT polymerization of the first embodiment may be one kind or two or more kinds. The molar number M2 is the total molar number of the acid groups of all the polymerization initiators.

[0049] The water-soluble inorganic base contained in the reaction liquid for RAFT polymerization of the first embodiment may be one kind or two or more kinds. The molar number M3 is the total molar number of all inorganic bases.

[0050] The acid group of the RAFT agent is preferably one or more selected from -CO2H, -SO3H and -PO4H, and -CO2H is more preferred from the viewpoint of facilitating the formation of a salt and adjusting the pH of the reaction solution.

[0051] When the acid groups of the RAFT agent and the polymerization initiator form salts, the salt is formed by the anion of the acid group and the counter cation. The counter cation is not particularly limited, and examples thereof include cations of alkali metals such as sodium and potassium, and alkaline earth metals such as magnesium and calcium. The counter cation is preferably derived from the water-soluble inorganic base.

[0052] As the water-soluble inorganic base, for example, a hydroxide having a hydroxide ion as an anion is preferred. Specifically, sodium hydroxide and potassium hydroxide are preferred from the viewpoint of enhancing the surface activity effect of the RAFT agent forming a salt.

[0053] The water-soluble inorganic base is an inorganic base that dissolves 1 g or more in 100 g of water at 20°C.

[0054] The above R 1 The organic group represented by is not particularly limited as long as it is an organic group having the above-mentioned acid group, and any organic group can be applied. For example, an organic group having a C1-C10 straight-chain or branched monovalent alkyl group as a basic skeleton, wherein any one or more hydrogen atoms of the above-mentioned alkyl group are substituted by the above-mentioned acid group. Any one or more methylene groups constituting the above-mentioned alkyl group may be substituted by -O-, -C(=O)O-, -OC(=O)-, or -C(=O)NH- (except for the case where oxygen atoms are bonded to each other).

[0055] One or more hydrogen atoms in the above alkyl group may be substituted with -CN.

[0056] As a specific R 1 For example, -CH2CO2H, -CH2CH2CO2H, -CH(CH3)CO2H, -CH(CO2H)CH2CO2H, -C(CH3)(CH3)CO2H, -C(CN)(CH3)CH2CH2CO2H, -CH(CH3)CONR a R b .

[0057] The above R a and R b Each is independently selected from H, C1-C6 alkyl, C1-C6 alkoxy, C6-C12 aryl, C7-C18 alkylaryl and C6-C12 heteroaryl. a and R b At least one of the hydrogen atoms is replaced by an acid group selected from -CO2H, -SO3H and -PO4H, and the acid group forms a salt. a and R b They may be the same as or different from each other.

[0058] In this specification, the term "aryl" refers to a group derived from an aromatic hydrocarbon, i.e., a functional group or substituent containing an aromatic ring. The term "heteroaryl" refers to a group in which one or more carbon atoms possessed by an aryl group are replaced by atoms other than carbon atoms (e.g., nitrogen atoms, oxygen atoms, sulfur atoms). The ring constituting the aryl group may be a monocyclic ring or a polycyclic ring. Each ring is preferably a 5-membered ring or a 6-membered ring. Specific examples of the ring include benzene, biphenyl, terphenyl, quaterphenyl, naphthalene, tetrahydronaphthalene, 1-benzylnaphthalene, anthracene, dihydroanthracene, benzanthracene, dibenzanthracene, phenanthrene, perylene, pyridine, 4-phenylpyridine, 3-phenylpyridine, thiophene, benzothiophene, naphthothiophene, thianthrene, furan, benzofuran, pyrene, isobenzofuran, chromene, xanthene, and phenoxathiin. , pyrrole, imidazole, pyrazole, pyrazine, pyrimidine, pyridazine, indole, indolizine, isoindole, purine, quinoline, isoquinoline, phthalazine, quinoxaline, quinazoline, pteridine, carbazole, carboline, phenanthridine, acridine, phenanthroline, phenazine, isothiazole, isoxazole, phenoxazine, etc.

[0059] In the present specification, the term "aralkyl" refers to an aromatic alkyl group, and examples thereof include groups in which the terminal hydrogen atom of a linear alkyl group (e.g., C1 to C6) is substituted with an aryl group. Specifically, examples thereof include benzyl, phenethyl, diphenylmethyl, triphenylmethyl, 1-naphthylmethyl, 2-naphthylmethyl, 2,2-diphenylethyl, 3-phenylpropyl, 4-phenylbutyl, 5-phenylpentyl, and the like.

[0060] The organic group represented by Z is an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group.

[0061] As the above-mentioned alkyl group, for example, there can be mentioned C1 to C20 straight-chain, branched and cyclic alkyl groups, and alkyl groups formed by any combination thereof. In formula (1), when Z is a cyclic alkyl group or contains a cyclic alkyl group, any one or more carbon atoms constituting the cyclic alkyl group may be substituted by a nitrogen atom, an oxygen atom or a sulfur atom (however, excluding the case where oxygen atoms are bonded to each other). Among the carbon atoms of the cyclic alkyl group, the carbon atom bonded to the thiol group (>C=S) of formula (1) may also be substituted by the above-mentioned heteroatom. Any one or more methylene groups (-CH2-) constituting the cyclic alkyl group may also be substituted by a keto group (>C=O). The above-mentioned cyclic alkyl group is preferably a 5- to 8-membered ring, and more preferably a 5-membered ring or a 6-membered ring.

[0062] The above-mentioned alkylthio group is a group in which the above-mentioned alkyl group is bonded to a sulfide group (—S—).

[0063] The arylthio group is a group in which an aryl group is bonded to a thioether group.

[0064] The aralkylthio group is a group in which an aralkyl group is bonded to a thioether group.

[0065] From the viewpoint of the surface active effect of the RAFT agent that forms a salt in an aqueous system, Z in the formula (1) is preferably an alkylthio group.

[0066] A part of the above-mentioned organic group represented by Z in formula (1) may be substituted by any group or may not be substituted. In the present specification, "arbitrarily substituted" and "substituted by any group" mean that a part of the organic group (for example, a hydrogen atom, a methylene group, a methyl group, etc.) is substituted by one or more groups selected from the following groups: alkyl, alkenyl, alkynyl, aryl, halo, haloalkyl, haloalkenyl, haloalkynyl, haloaryl, hydroxyl, alkoxy, alkenyloxy, aryloxy, benzyloxy, haloalkoxy, haloalkenyloxy, acetileno, carboximidyl, haloaryloxy, isocyano, cyano, formyl, carboxyl, nitro, nitroalkyl, nitroalkenyl, nitroalkyne alkyl, nitroaryl, alkylamino, dialkylamino, alkenylamino, alkynylamino, arylamino, diarylamino, benzylamino, imino, alkylimino, alkenylimino, alkynylimino, arylimino, benzylimino, dibenzylamino, acyl, alkenylacyl, alkynylacyl, arylacyl, acylamino, diacylamino, acyloxy, alkylsulfonyloxy, arylsulfenyloxy, heterocyclyl, heterocyclyloxy, heterocyclylamino, halogenated heterocyclyl, alkylsulfonyl, arylsulfonyl, alkylsulfinyl, The invention also includes but is not limited to alkyl, alkyl, alkylsulfinyl, arylsulfinyl, carboalkoxy, alkylthio, benzylthio, acylthio, sulfonamide, sulfanilyl, a group containing a sulfonic group and phosphorus, an alkoxysilyl group, a silyl group, an alkylsilyl group, an alkylalkoxysilyl group, a phenoxysilyl group, an alkylphenoxysilyl group, an alkoxyphenoxysilyl group, an arylphenoxysilyl group, an allophanyl group, a guanidino group, a hydantoyl group, a ureide group, and a 1,3-ureylene group.

[0067] In this specification, the terms "halogen" and "halo" refer to iodine, bromine, chlorine and fluorine unless otherwise specified.

[0068] In the above definition, the term "alkyl" used alone or in compound words such as "alkenyloxyalkyl", "alkylthio", "alkylamino" and "dialkylamino" refers to a straight chain, branched chain or cyclic alkyl group, preferably a C1-20 alkyl group or a cycloalkyl group. Examples of straight chain and branched chain alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, sec-pentyl, 1,2-dimethylpropyl, 1,1-dimethylpropyl, hexyl, 4-methylpentyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 1,1-dimethylbutyl, 2,2-dimethylbutyl, 3,3-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 1,2,2-trimethylpropyl 1,1,2-trimethylpropyl, heptyl, 5-methoxyhexyl, 1-methylhexyl, 2,2-dimethylpentyl, 3,3-dimethylpentyl, 4,4-dimethylpentyl, 1,2-dimethylpentyl, 1,3-dimethylpentyl, 1,4-dimethylpentyl, 1,2,3-trimethylbutyl, 1,1,2-trimethylbutyl, 1,1,3-trimethylbutyl, octyl, 6-methylheptyl, 1-methylheptyl, 1,1,3,3-tetramethylbutyl, nonyl, 1-, 2-, 3 1-, 2-, 3-, 4-, 5-, 6-, or 7-methyloctyl, 1-, 2-, 3-, 4-, or 5-ethylheptyl, 1-, 2-, or 3-propylhexyl, decyl, 1-, 2-, 3-, 4-, 5-, 6-, 7-, and 8-methylnonyl, 1-, 2-, 3-, 4-, 5-, or 6-ethyloctyl, 1-, 2-, 3-, or 4-propylheptyl, undecyl, 1-, 2-, 3-, 4-, 5-, 6-, 7-, 8-, or 9-methyldecyl, 1-, 2-, 3-, 4-, 5- 1-, 2-, 3-, 4-, 5-, 6-, 7-, 8-, 9-, or 10-methylundecyl, 1-, 2-, 3-, 4-, 5-, 6-, 7-, or 8-ethyldecyl, 1-, 2-, 3-, 4-, 5-, or 6-propylnonyl, 1-, 2-, 3-, or 4-butyloctyl, 1-, 2-pentylheptyl, etc. Examples of the cyclic alkyl group include monocyclic or polycyclic alkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, and cyclodecyl.

[0069] The term "alkoxy" refers to a linear or branched alkoxy group, preferably a C1 to C20 alkoxy group. Examples of the alkoxy group include methoxy, ethoxy, n-propoxy, isopropoxy, and various butoxy isomers.

[0070] The term "alkenyl" includes mono-, di- or polyethylenically unsaturated alkyl or cycloalkyl groups as defined above, and refers to a group formed by a linear, branched or cyclic olefin, preferably a C2-20 alkenyl group. Examples of the alkenyl group include vinyl, allyl, 1-methylvinyl, butenyl, isobutenyl, 3-methyl-2-butenyl, 1-pentenyl, cyclopentenyl, 1-methyl-cyclopentenyl, 1-hexenyl, 3-hexenyl, cyclohexenyl, 1-heptenyl, 3-heptenyl, 1-octenyl, cyclooctenyl, 1-nonenyl, 2-nonenyl, 3-nonenyl, 1-decenyl, 3-decenyl, 1,3-butadienyl, 1,4-pentadienyl, 1,3 cyclopentadienyl, 1,3-hexadienyl, 1,4-hexadienyl, 1,3-cyclohexadienyl, 1,4-cyclohexadienyl, 1,3-cycloheptadienyl, 1,3,5-cycloheptatrienyl, and 1,3,5,7-cyclooctatetraenyl.

[0071] The term "alkynyl" is similar in structure to the alkyl and cycloalkyl groups defined above, and refers to a group formed by a linear, branched or cyclic alkyne, preferably an alkynyl group of C2 to 20. Examples of alkynyl groups include ethynyl, 2-propynyl and 2- or 3-butynyl.

[0072] The compound words such as "acyloxy", "acylthio", "acylamino" or "diacylamino" or the single "acyl", the term "acyl" refers to an acyl group containing carbamoyl, aliphatic acyl and aromatic ring (referred to as aromatic acyl) or an acyl group containing a heterocyclic ring (referred to as heterocyclic acyl), preferably a C1-20 acyl group. Examples of the acyl group include carbamoyl; linear or branched alkanoyl groups such as formyl, acetyl, propionyl, butyryl, 2-methylpropionyl, valeryl, 2,2-dimethylpropionyl, hexanoyl, heptanoyl, octanoyl, nonanoyl, decanoyl, undecanoyl, dodecanoyl, tridecanoyl, tetradecanoyl, pentadecanoyl, hexadecanoyl, heptadecanoyl, octadecanoyl, nonadecanoyl, and icosanoyl; alkoxycarbonyl groups such as methoxycarbonyl, ethoxycarbonyl, tert-butoxycarbonyl, tert-pentyloxycarbonyl, and heptyloxycarbonyl; cyclopropylcarbonyl, cyclobutylcarbonyl, such as cycloalkylcarbonyl, cyclopentylcarbonyl and cyclohexylcarbonyl; alkylsulfonyl such as methylsulfonyl and ethylsulfonyl; alkoxysulfonyl such as methoxysulfonyl and ethoxysulfonyl; aroyl such as benzoyl, toluoyl and naphthoyl; aroyl such as phenylalkanoyl (e.g., phenylacetyl, phenylpropionyl, phenylbutyryl, phenylisobutyryl, phenylvaleryl and phenylhexanoyl) and naphthylalkanoyl (e.g., naphthylacetyl, naphthylpropionyl and naphthylbutyryl); phenylalkenoyl (e.g., phenylalkenoyl, phenylalkanoyl and naphthylalkanoyl); aralkenoyl such as phenylalkenoyl (e.g., phenylacryloyl, phenylbutenoyl, phenylmethacryloyl, phenylpentenoyl and phenylhexenoyl) and naphthylalkenoyl (e.g., naphthylacryloyl, naphthylbutenoyl and naphthylpentenoyl); aryloxycarbonyl such as phenylalkoxycarbonyl (e.g., benzyloxycarbonyl); aryloxycarbonyl such as phenoxycarbonyl and naphthyloxycarbonyl; aryloxyalkanoyl such as phenoxyacetyl and phenoxypropionyl; arylcarbamoyl such as phenylcarbamoyl; arylthiocarbamoyl such as phenylthiocarbamoyl; arylglyoxyloyl such as phenylglyoxyloyl and naphthylglyoxyloyl; glyoxyloyl); arylsulfonyl groups such as phenylsulfonyl and naphthylsulfonyl; heterocyclic carbonyl; heterocycloalkanoyl groups such as thienylacetyl, thienylpropionyl, thienylbutyryl, thienylpentanoyl, thienylhexanoyl, thiazolylacetyl, thiadiazolylacetyl and tetrazolylacetyl; heterocycloalkenoyl groups such as heterocyclopropenyl, heterocyclobutenoyl, heterocyclopentenoyl and heterocyclohexenoyl; and heterocycloglyoxyl groups such as thiazolylglyoxyl and thienylglyoxyl.

[0073] As the RAFT agent contained in the reaction solution for RAFT polymerization of the first embodiment, a known RAFT agent can be used. However, since the acid group of the known RAFT agent does not form a salt, it is preferred to react with a water-soluble inorganic base to form a salt of the acid group of the RAFT agent.

[0074] In this specification, when used alone or as part of a term such as "heterocyclic alkenyl", "heterocyclic oxy" ("heterocyclyloxy") or "halogenated heterocyclic group", the terms "heterocyclic" and "heterocyclic group" refer to aromatic, near-aromatic and non-aromatic rings or ring systems containing one or more heteroatoms selected from nitrogen atoms, oxygen atoms and sulfur atoms and which may be substituted arbitrarily. Preferably, the ring or ring system has 3 to 20 carbon atoms. The ring or ring system may be selected from the groups described above in connection with the definition of "heteroaryl".

[0075] Preferred examples of the RAFT agent represented by the formula (1) include the following compounds.

[0076]

[0077] R in formula (1a) to (1j) 3 is an organic group, for example, each independently is the same organic group as the above Z. + Each independently represents a monovalent cation. The type of cation is not particularly limited, and examples thereof include cations of alkali metals such as sodium and potassium.

[0078] As a particularly preferred RAFT agent for ethylenically unsaturated monomers, for example, a compound represented by formula (1-1) can be cited. Furthermore, as a particularly preferred RAFT agent for methacrylate, for example, a compound represented by formula (1-2) can be cited. In the formula, M + The definition of is the same as above.

[0079]

[0080] As the polymerization initiator of any component of the RAFT polymerization reaction liquid of the first embodiment, a known free radical polymerization initiator can be applied. For example, an azo polymerization initiator, a photopolymerization initiator, an inorganic peroxide, an organic peroxide, a redox initiator composed of an organic peroxide, a transition metal and a reducing agent, etc. can be cited. Among them, an azo polymerization initiator, an inorganic peroxide, an organic peroxide, and a redox initiator that can initiate polymerization by heating are preferred. Only one of them can be used, or two or more of them can be used in combination.

[0081] When the polymerization initiator has an acid group, it is preferred that the acid group of the polymerization initiator be reacted with a water-soluble inorganic base to form a salt.

[0082] Examples of the acid group possessed by the polymerization initiator include one or more selected from -CO2H, -SO3H and -PO4H. Among them, -CO2H is preferred from the viewpoint of easily forming a salt to adjust the pH of the reaction solution.

[0083] The polymerization initiator is preferably water-soluble. A water-soluble polymerization initiator is a polymerization initiator that can dissolve 1 g or more in 100 g of water at 20°C.

[0084] Specific examples of polymerization initiators include inorganic peroxides such as potassium persulfate, sodium persulfate, ammonium persulfate, and hydrogen peroxide, organic peroxides such as benzoyl peroxide and isobutyryl peroxide, azo compounds such as azobisisobutyronitrile, 4-methoxy-azobisvaleronitrile, and 4,4'-azobis(4-cyanovaleric acid), redox initiators in which organic peroxides are combined with ferrous sulfate, a chelating agent, and a reducing agent, such as an initiator composed of cumene hydroperoxide, ferrous sulfate, sodium pyrophosphate, and glucose, and an initiator in which tert-butyl hydroperoxide, sodium formaldehyde sulfoxylate (Rongalite), ferrous sulfate, and disodium ethylenediaminetetraacetate are combined, etc. Among them, 4,4'-azobis(4-cyanovaleric acid) is preferred from the viewpoint of improving the reactivity of RAFT polymerization using the RAFT agent of the present embodiment.

[0085] In the preparation liquid for forming the salt of the RAFT agent, the content of the RAFT agent is preferably, for example, 0.001 to 10% by mass, more preferably 0.01 to 7.0% by mass, and still more preferably 0.03 to 5.0% by mass relative to the total mass of the preparation liquid. Within the above preferred range, the reaction (saponification reaction) for forming the salt of the RAFT agent proceeds sufficiently, and a RAFT agent with a stable saponification state can be obtained.

[0086] The content of the RAFT agent before the RAFT polymerization reaction solution of the first embodiment is used, that is, before the polymerizable monomer is added, preferably 0.001 to 0.50% by mass, more preferably 0.01 to 0.20% by mass, and further preferably 0.03 to 0.10% by mass relative to the total mass of the RAFT polymerization reaction solution before use. Within the above preferred range, the monomers in the reaction solution can be fully RAFT polymerized to obtain a polymer with a narrow molecular weight distribution in a short reaction time. The amount of coagulum remaining in the reaction solution after the reaction can be reduced.

[0087] The content of the polymerization initiator before the RAFT polymerization reaction solution of the first embodiment is used, that is, before the polymerizable monomer is added, preferably 0.001 to 0.50% by mass, more preferably 0.01 to 0.20% by mass, and further preferably 0.03 to 0.10% by mass relative to the total mass of the RAFT polymerization reaction solution before use. Within the above preferred range, the monomers in the reaction solution can be fully RAFT polymerized to obtain a polymer with a narrow molecular weight distribution in a short reaction time. The amount of coagulum remaining in the reaction solution after the reaction can be reduced.

[0088] The water content of the reaction solution for RAFT polymerization of the first embodiment before use, i.e., before adding the polymerizable monomer, is preferably 80% by mass or more, more preferably 90% by mass or more, and further preferably 95% by mass or more relative to the total mass of the reaction solution for RAFT polymerization before use. As a standard for the upper limit value, for example, 99% by mass or less can be cited. When it is within the above preferred range, adding the monomer to the reaction solution can easily initiate RAFT polymerization.

[0089] The reaction liquid for RAFT polymerization of the first embodiment may contain a dispersion medium other than water and other additives within a range not inhibiting RAFT polymerization, but preferably does not contain them.

[0090] Examples of dispersion media other than water include organic solvents that are miscible with water (eg, alcohols). Examples of other additives include surfactants and the like.

[0091] The acid group of the RAFT agent of this embodiment forms a salt, so the reactivity of the monomer is good. Therefore, even without using a surfactant, RAFT polymerization can be carried out well.

[0092] <Production of Reaction Solution for RAFT Polymerization of First Aspect>

[0093] The preparation of the salt forming the RAFT agent is preferably performed at a temperature of 20 to 100° C., more preferably 25 to 90° C. At the above preferred preparation temperature, the time until the preparation is completed is typically about 10 to 300 minutes. Within the above range, a RAFT agent preparation solution dissolved or dispersed in water can be obtained.

[0094] The RAFT polymerization reaction liquid of the first embodiment may also contain a polymerization initiator as an arbitrary component. The polymerization initiator may be added when preparing the RAFT polymerization reaction liquid, may be added together with the polymerizable monomer described later, or may be prepared separately. Preferably, it is prepared separately, and when it is a thermally decomposed polymerization initiator, the preparation temperature is preferably below the 10-hour half-life temperature, for example, 20 to 60°C. The standard preparation time is about 5 to 300 minutes. When it is within the above range, a preparation liquid of the polymerization initiator dissolved or dispersed in water or the above monomer can be obtained.

[0095] The reaction solution for RAFT polymerization of the first scheme can be obtained by conventional methods by mixing the above-mentioned RAFT agent or its solution, water, the above-mentioned water-soluble inorganic base, and the above-mentioned polymerization initiator as needed in a desired ratio. As an example, first, the above-mentioned RAFT agent, water and the above-mentioned water-soluble inorganic base are mixed to obtain a solution of a salt of the acid group possessed by the above-mentioned RAFT agent (hereinafter sometimes referred to as a saponified RAFT agent aqueous solution). Then, the above-mentioned polymerization initiator, water and the above-mentioned water-soluble inorganic base are mixed to obtain a solution of a salt of the acid group possessed by the above-mentioned polymerization initiator (hereinafter sometimes referred to as an initiator aqueous solution). Finally, by mixing the saponified RAFT agent aqueous solution and the initiator aqueous solution, the ratio of the above-mentioned M3 / (M1+M2) is adjusted to a specified ratio to obtain the reaction solution for RAFT polymerization of this scheme.

[0096] <Use of the RAFT Polymerization Reaction Solution of the First Aspect>

[0097] By adding a polymerizable monomer to the RAFT polymerization reaction solution of the first embodiment and performing RAFT polymerization, a living radical polymerization reaction based on the action of the RAFT agent can be induced, and a polymer with a narrow molecular weight distribution (Mw / Mn) can be obtained in a short reaction time. The amount of residue (agglomerates) remaining as impurities in the reaction solution after the reaction can be reduced.

[0098] As the monomer, a radical polymerizable monomer is preferred, and an ethylenically unsaturated monomer is more preferred from the viewpoint of good reactivity. Examples of the ethylenically unsaturated monomer include monomers represented by formula (10).

[0099]

[0100] In formula (10), U and W are each independently selected from -CO2H, -CO2R 2 、-COR 2 、-CSR 2 ,-CSOR 2 ,-COSR 2 , -CONH2, -CONHR 2 、-CON(R 2)2, hydrogen, halogen and optionally substituted C1-C4 alkyl (the substituents may be independently selected from hydroxyl, -CO2H, -CO2R 2 、-COR 2 、-CSR 2 ,-CSOR 2 ,-COSR 2 、-CN、-CONH2、-CONHR 2 、-CON(R 2 )2.-OR 2 、-SR 2 、-O2CR 2 ,-SCOR 2 and-OCSR 2 ) in the group composed of .

[0101] In formula (10), V is selected from hydrogen, -R 2 、-CO2H、-CO2R 2 、-COR 2 、-CSR 2 ,-CSOR 2 ,-COSR 2 , -CONH2, -CONHR 2 、-CON(R 2 )2.-OR 2 、-SR 2 、-O2CR 2 ,-SCOR 2 and-OCSR 2 In the group composed of.

[0102] The above R in U, W and V of formula (10) 2 The substituent is selected from the group consisting of optionally substituted C1-C18 alkyl, optionally substituted C2-C18 alkenyl, optionally substituted aryl, optionally substituted heteroaryl, optionally substituted carbocyclyl, optionally substituted heterocyclyl, optionally substituted aralkyl, optionally substituted heteroarylalkyl, optionally substituted alkaryl, optionally substituted alkylheteroaryl and polymer chains. The substituents are independently selected from the group consisting of alkylene oxidyl (epoxy), hydroxyl, alkoxy, acyl, acyloxy, formyl, alkylcarbonyl, carboxyl, sulfonic acid, alkoxy- or aryloxy-carbonyl, isocyanato, cyano, silyl, halo, amino (including salts and derivatives thereof). Preferred polymer chains include polyalkylene oxides, polyarylene ethers and polyalkylene ethers.

[0103] In this specification, the term "carbocyclic group" refers to any ring system in which all ring atoms are carbon and preferably contains 3 to 12 carbon atoms, more preferably 3 to 10 carbon atoms, and further preferably 3 to 8 carbon atoms. The carbocyclic group may be saturated or partially unsaturated, but does not contain an aromatic ring.

[0104] In the present specification, the term "heterocyclic group" refers to a group in which one or more atoms constituting a ring of a carbocyclic group are substituted with a heteroatom selected from nitrogen, oxygen and sulfur.

[0105] In the present specification, the term "aralkyl group" refers to a group in which any one or more hydrogen atoms of an alkyl group are substituted with an aryl group.

[0106] In the present specification, the term "alkaryl group" refers to a group in which one or more hydrogen atoms of an aryl group are substituted with an alkyl group.

[0107] As specific examples of monomers, maleic anhydride, N-alkyl maleimide, N-aryl maleimide, dialkyl fumarate and cyclopolymerizable monomers, acrylate, methacrylate, acrylic acid, methacrylic acid, styrene, acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, mixtures of these monomers, and mixtures of these monomers with other monomers can be cited. The selection of comonomers is appropriately determined according to their stereo and electronic properties. The factors that determine the copolymerizability of various monomers are well documented in the technology.

[0108] More specific examples of the monomer include: methyl methacrylate, ethyl methacrylate, propyl methacrylate (and all isomers thereof), butyl methacrylate (and all isomers thereof), 2-ethylhexyl methacrylate, isobornyl methacrylate, methacrylic acid, benzyl methacrylate, phenyl methacrylate, phenoxyethyl methacrylate, methacrylonitrile, α-methylstyrene, methyl acrylate, ethyl acrylate, propyl acrylate (and all isomers thereof), butyl acrylate (and all isomers thereof), 2-ethylhexyl acrylate, isobornyl methacrylate, acrylic acid, benzyl acrylate, phenyl methacrylate, phenoxyethyl acrylate, acrylonitrile, styrene, functional methyl Acrylates, acrylates and styrene, and glycidyl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate (and all its isomers), hydroxybutyl methacrylate (and all its isomers), N,N-dimethylaminoethyl methacrylate, N,N-diethylaminoethyl methacrylate, triethylene glycol methacrylate, itaconic anhydride, itaconic acid, glycidyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate (and all its isomers), hydroxybutyl acrylate (and all its isomers), N,N-dimethylaminoethyl methacrylate, N,N-diethylaminoethyl methacrylate, triethylene glycol acrylate, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, N-tert-butylmethacrylamide, N-n-butylmethacrylamide, N-hydroxymethylmethacrylamide, N-hydroxyethylmethacrylamide, N-tert-butylacrylamide, N-n-butylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethylacrylamide, vinylbenzoic acid (and all its isomers), diethylaminostyrene (and all its isomers), α-methylvinylbenzoic acid (and all its isomers), diethylaminoα-methylstyrene (and all its isomers), p-vinylbenzenesulfonic acid, p-vinylbenzenesulfonic acid sodium salt, trimethoxysilylpropyl methacrylate, triethoxysilylpropyl methacrylate, tributoxysilylpropyl methacrylate, dimethoxymethylsilylpropyl methacrylate, diethoxymethylsilylpropyl methacrylate, dibutoxymethylsilylpropyl methacrylate, diisopropoxymethylsilylpropyl methacrylate, dimethyl methacrylate Silyl methacrylate, diethoxysilyl propyl methacrylate, dibutoxysilyl propyl methacrylate, diisopropoxysilyl propyl methacrylate, trimethoxysilyl propyl acrylate, triethoxysilyl propyl acrylate, tributoxysilyl propyl acrylate, dimethoxymethyl silyl propyl acrylate, diethoxymethyl silyl propyl acrylate, dibutoxymethyl silyl propyl acrylate, diisopropoxysilyl propyl methacrylate, trimethoxysilyl propyl acrylate, triethoxysilyl propyl acrylate, tributoxysilyl propyl acrylate, dimethoxymethyl silyl propyl acrylate, diethoxymethyl silyl propyl acrylate, dibutoxymethyl silyl propyl acrylate, diisopropoxysilyl propyl methacrylate Propoxymethylsilylpropyl ester, dimethoxysilylpropyl acrylate, diethoxysilylpropyl acrylate, dibutoxysilylpropyl acrylate, diisopropoxysilylpropyl acrylate, vinyl acetate, vinyl butyrate, vinyl benzoate, vinyl chloride, vinyl fluoride, vinyl bromide, maleic anhydride, N-phenylmaleimide, N-butylmaleimide, N-vinylpyrrolidone, N-vinylcarbazole, butadiene, ethylene, chloroprene, etc. These may be used alone or in combination of two or more.

[0109] The amount of the monomer added to the RAFT polymerization reaction liquid of the first embodiment is, for example, preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and even more preferably 10 to 25 parts by mass relative to 1 part by mass of the RAFT agent contained in the reaction liquid. When it is within the above preferred range, the above effect can be better obtained.

[0110] The water content is, for example, preferably 50% by mass or more, and more preferably 60% by mass or more, relative to the total mass of the reaction solution after the monomers are added to the reaction solution for RAFT polymerization of the first embodiment.

[0111] From the viewpoint of increasing the monomer reaction rate in the RAFT polymerization in the above-mentioned reaction solution, reducing the volume average particle size of the polymer (polymeric RAFT agent) obtained by RAFT polymerization, reducing the amount of coagulum, and shortening the reaction time, the higher the water content, the more preferred, for example, preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably 98% by mass or more. As the standard of the upper limit value in this case, 99.5% by mass or less can be cited.

[0112] On the contrary, from the viewpoint of increasing the volume average particle size of the polymer (polymeric RAFT agent) obtained by RAFT polymerization in the above-mentioned reaction solution, the lower the water content, the more preferred, for example, preferably 97% by mass or less, more preferably 92% by mass or less, further preferably 85% by mass or less, and particularly preferably 75% by mass or less. As a standard for the lower limit in this case, 50% by mass can be cited.

[0113] The reaction temperature in the RAFT reaction using the reaction solution for RAFT polymerization of the first embodiment is, for example, preferably 60 to 100° C., more preferably 70 to 90° C. At these preferred reaction temperatures, the typical reaction time until the RAFT reaction is completed is about 200 to 1500 minutes.

[0114] Other reaction conditions in the RAFT reaction using the reaction solution for RAFT polymerization of the first embodiment can be appropriately set with reference to conventional RAFT polymerization.

[0115] More detailed examples of RAFT polymerization using the reaction solution for RAFT polymerization of the first embodiment are shown in Examples 1a to 19a and the like described later.

[0116] The reaction solution after RAFT polymerization using the reaction solution for RAFT polymerization of the first embodiment is one embodiment of the reaction solution for RAFT polymerization of the second embodiment of the present invention described below.

[0117] By RAFT polymerization using the reaction solution for RAFT polymerization of the first embodiment, the polymeric RAFT agent described below can be obtained.

[0118] <<Second Option>>

[0119] A second aspect of the present invention is a reaction solution for RAFT polymerization, comprising a polymeric RAFT agent represented by formula (2), water and a water-soluble inorganic base, wherein at least part of the acid groups of the polymeric RAFT agent form a salt with a cation component of the water-soluble inorganic base.

[0120]

[0121] [In formula (2), R 1 represents an organic group, the organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 10000 (from the viewpoint of reducing the amount of coagulum, preferably 1 to 200, more preferably 1 to 100). ), when n is 2 or more, multiple Xs may be the same or different from each other. ]

[0122] In formula (2), R 1 The description of Z is the same as that of R in formula (1) of the first embodiment. 1 The descriptions of and Z are the same, so repeated descriptions are omitted here.

[0123] As any ethylenically unsaturated monomer represented by X, the above examples can be cited. Among them, styrene, acrylonitrile, methyl (meth)acrylate, butyl (meth)acrylate or (meth)acrylic acid is preferred from the perspective of facilitating RAFT polymerization using a polymeric RAFT agent. These may be used alone or in combination of two or more.

[0124] In the above R 1 The above X bonded is an ethylenically unsaturated monomer, and the above R derived from the RAFT agent 1 In the case of an organic group having a carbon atom A bonded to the above X, the carbon atom A of the above organic group is preferably a tertiary carbon atom. In the case of a tertiary carbon atom, the substituent replacing the hydrogen atom of the above carbon atom A is preferably a linear or branched alkyl group having 1 to 6 carbon atoms, more preferably a linear alkyl group having 1 to 3 carbon atoms. In the above preferred case, the next step of RAFT polymerization using a polymeric RAFT agent becomes easy.

[0125] In the above R 1 The above X bonded is methacrylate, and the above R derived from the RAFT agent 1In the case of an organic group having a carbon atom B bonded to the above-mentioned X, the above-mentioned carbon atom B of the above-mentioned organic group is preferably a quaternary carbon atom. In the case of a quaternary carbon atom, the two substituents replacing the hydrogen atoms of the above-mentioned carbon atom B are preferably independently a linear or branched alkyl group having 1 to 6 carbon atoms, and more preferably a linear alkyl group having 1 to 3 carbon atoms. Furthermore, it is preferred that at least one of the hydrogen atoms of the above-mentioned alkyl group constituting the above-mentioned substituent is substituted by a cyano group. As a particularly preferred example, an example in which the above-mentioned carbon atom B is a quaternary carbon atom bonded to an alkyl group having 1 to 3 carbon atoms and a cyano group can be cited. In the above-mentioned preferred case, the next stage RAFT polymerization using a polymeric RAFT agent becomes easy.

[0126] It is preferred that the acid group forming the salt is bonded to the carbon atom A or the carbon atom B directly or via a linking group. Examples of the linking group include a linear or branched alkylene group having 1 to 6 carbon atoms. Any methylene group constituting the alkylene group may be substituted with -O-, -C(=O)O-, -OC(=O)-, or -C(=O)NH- (except for the case where oxygen atoms are bonded to each other).

[0127] The number of repeating units represented by n is preferably 5 or more, more preferably 10 or more, further preferably 20 or more, particularly preferably 30 or more, and most preferably 40 or more. Here, the number of repeating units refers to the total number of repeating units of one or more monomers corresponding to X.

[0128] When n is greater than the above lower limit, the polymerized site (X) n It can function as a block of a polymer.

[0129] The polymeric RAFT agent can form particles in the reaction solution for RAFT polymerization. The volume average particle size is preferably 5 to 500 nm, more preferably 7 to 100 nm, and further preferably 10 to 50 nm. When it is in the above preferred range, the advantages of improving the dispersibility of the polymeric RAFT agent in water and shortening the reaction time can be obtained.

[0130] The volume average particle size (MV) of the polymeric RAFT agent contained in the reaction solution for RAFT polymerization of the present scheme can be determined as follows: using Nanotrac UPA-EX150 manufactured by Nikkiso Co., Ltd., the volume-based particle size distribution of the polymer in the emulsion is measured by a measurement method based on a dynamic light scattering method (solvent: water, temperature 25°C), and the average particle size (volume average particle size) is determined from the particle size distribution.

[0131] The molecular weight distribution represented by Mw / Mn of the polymeric RAFT agent is preferably as narrow as possible, preferably 2.0 or less, more preferably 1.8 or less, further preferably 1.6 or less, particularly preferably 1.4 or less, and most preferably 1.2 or less. Usually, the lower limit of the molecular weight distribution is 1.0 or more.

[0132] The molecular weight distribution of the polymeric RAFT agent contained in the reaction liquid for RAFT polymerization of this scheme is determined as follows: using calcium chloride as a coagulant, the emulsion is coagulated at 60 to 95°C, dehydrated, washed, dried and recovered, dissolved in tetrahydrofuran, and the Mw and Mn converted to standard polystyrene are determined by GPC.

[0133] The pH of the reaction liquid for RAFT polymerization of the second embodiment is preferably 8 to 13. The pH is a value measured at 25° C. according to the method specified in JIS Z8802:2011. In this specification, pH is expressed as an integer with an effective value of 1. That is, the first decimal place of the measured value is a rounded value.

[0134] The pH of the reaction solution for RAFT polymerization of the second embodiment is preferably 8 to 13, more preferably 10 to 13, further preferably 11 to 13, and particularly preferably 12 to 13. Within the above preferred range, the molecular weight distribution of the polymer formed by RAFT polymerization can be further narrowed.

[0135] The content of the polymeric RAFT agent before the RAFT polymerization reaction solution of the second embodiment is used, that is, before the polymerizable monomer is added, is preferably 0.01 to 10.0% by mass, more preferably 0.1 to 5.0% by mass, and further preferably 0.5 to 3.0% by mass, relative to the total mass of the RAFT polymerization reaction solution of the second embodiment before use. Within the above preferred range, the monomers in the reaction solution can be fully RAFT polymerized to obtain a polymer with a narrow molecular weight distribution in a short reaction time. The amount of coagulum remaining in the reaction solution after the reaction can be reduced.

[0136] The polymeric RAFT agent contained in the reaction solution for RAFT polymerization of the second embodiment may be one kind or two or more kinds.

[0137] When the reaction solution for RAFT polymerization of the second embodiment is used, a polymerization initiator may also be added. The amount of the polymerization initiator added may be, for example, 0.01 to 0.1 mass % relative to the total mass of the reaction solution for RAFT polymerization of the second embodiment before the addition of the polymerizable monomer. It is preferably appropriately set to be equimolar to the amount of the polymeric RAFT agent. For example, from the viewpoint of achieving stable RAFT polymerization, it is preferred to add about 1 to 5 mass parts of the polymerization initiator relative to 100 mass parts of the polymeric RAFT agent.

[0138] The polymerization initiator added to the reaction liquid for RAFT polymerization of the second embodiment may be one kind or two or more kinds.

[0139] The water content of the reaction solution for RAFT polymerization of the second embodiment before use, i.e., before adding the polymerizable monomer, is preferably 80% by mass or more, more preferably 90% by mass or more, and further preferably 95% by mass or more, relative to the total mass of the reaction solution for RAFT polymerization before use. As a standard for the upper limit value, for example, 99% by mass or less can be cited. When it is within the above preferred range, adding the monomer to the reaction solution can easily initiate RAFT polymerization.

[0140] The reaction liquid for RAFT polymerization of the second embodiment may contain a dispersion medium other than water and other additives within a range that does not inhibit RAFT polymerization, but preferably does not contain them.

[0141] Examples of dispersion media other than water include organic solvents that are miscible with water (eg, alcohols). Examples of other additives include surfactants and the like.

[0142] Since the acid group of the polymeric RAFT agent of this embodiment forms a salt, the reactivity of the monomer is good, and therefore RAFT polymerization can be carried out well even without using a surfactant.

[0143] <Production of Reaction Solution for RAFT Polymerization of Second Aspect>

[0144] The reaction liquid for RAFT polymerization of the second embodiment can be obtained by adding a polymerizable monomer to the reaction liquid for RAFT polymerization of the first embodiment and performing RAFT polymerization. The specific method is as described above.

[0145] <Use of the reaction solution for RAFT polymerization according to the second embodiment>

[0146] By adding one or more polymerizable monomers to the RAFT polymerization reaction solution of the second embodiment and performing RAFT polymerization, a living radical polymerization reaction can be induced in an aqueous system under the action of a polymeric RAFT agent, and a polymer with a narrow molecular weight distribution can be obtained in a short reaction time. The amount of residue (agglomerates) remaining as impurities in the reaction solution after the reaction can be reduced.

[0147] Examples of the monomer include the monomers exemplified in the first embodiment. By using a monomer that is different in type or mixed in a different manner from the ethylenically unsaturated monomer represented by X constituting the polymeric RAFT agent, a monomer having the same structure as (X) represented by formula (2) can be obtained. n The blocks represented are diblock copolymers of different blocks.

[0148] The amount of the monomer added to the reaction solution for RAFT polymerization of the second embodiment is preferably 1 to 90 parts by mass, more preferably 5 to 60 parts by mass, and even more preferably 9 to 30 parts by mass, relative to 1 part by mass of the polymeric RAFT agent contained in the reaction solution. When it is within the above preferred range, the molecular weight distribution of the generated polymer can be further narrowed.

[0149] The reaction temperature in the RAFT reaction using the reaction solution for RAFT polymerization of the second embodiment is, for example, preferably 60 to 100° C., more preferably 70 to 90° C. At the above preferred reaction temperature, the reaction time until the RAFT reaction is completed is typically about 60 to 600 minutes.

[0150] Other reaction conditions in the RAFT reaction using the reaction solution for RAFT polymerization of the second embodiment can be appropriately set with reference to conventional RAFT polymerization.

[0151] More detailed examples of RAFT polymerization using the reaction solution for RAFT polymerization according to the second embodiment are shown in Examples 1b to 19b and the like described later.

[0152] The reaction solution after RAFT polymerization using the reaction solution for RAFT polymerization of the second embodiment is one embodiment of the reaction solution for RAFT polymerization of the third embodiment of the present invention described below.

[0153] By RAFT polymerization using the reaction solution for RAFT polymerization of the second embodiment, the hydrophilic copolymer-type RAFT agent described below can be obtained.

[0154] <<Third Option>>

[0155] A third embodiment of the present invention is a reaction solution for RAFT polymerization, comprising a hydrophilic copolymerizable RAFT agent represented by formula (3), water, and a water-soluble inorganic base.

[0156] At least part of the acid groups of the hydrophilic copolymeric RAFT agent forms a salt with the cationic component of the water-soluble inorganic base.

[0157]

[0158] [In formula (3), R 1represents an organic group, the organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 100, and when n is 2 or more, a plurality of Xs may be the same as or different from each other, Y is a repeating unit of any ethylenically unsaturated monomer, m represents an integer of 10 to 10000, and a plurality of Ys may be the same as or different from each other, (X) n The polymer chain represented by (Y) m The polymer chains represented are different from each other.]

[0159] R in formula (3) 1 The description of Z is the same as that of R in formula (1) of the first embodiment. 1 The descriptions of and Z are the same, so repeated descriptions are omitted here.

[0160] The description of X and n in the formula (3) is the same as the description of X and n in the formula (2) of the second embodiment, and therefore, the repeated description is omitted here.

[0161] Examples of the optional ethylenically unsaturated monomer represented by Y include the above-mentioned examples. Among them, styrene, acrylonitrile, butyl acrylate, or (meth)acrylic acid is preferred from the viewpoint of facilitating RAFT polymerization using a hydrophilic copolymerization type RAFT agent.

[0162] These may be used alone or in combination of two or more.

[0163] The number of repeating units represented by m is preferably 50 or more, more preferably 100 or more, further preferably 200 or more, particularly preferably 300 or more, and most preferably 400 or more. Here, the number of repeating units refers to the total number of repeating units of one or more monomers corresponding to Y.

[0164] When m is greater than the above lower limit, the polymerized site (Y) m It can function as a block of a polymer.

[0165] The hydrophilic copolymeric RAFT agent can form particles in the reaction solution for RAFT polymerization. The volume average particle size is preferably 10 to 500 nm, more preferably 15 to 300 nm, and further preferably 20 to 200 nm. When it is in the above preferred range, the advantages of improving the dispersibility of the hydrophilic copolymeric RAFT agent in water and shortening the reaction time can be obtained.

[0166] The volume average particle size (MV) of the hydrophilic copolymeric RAFT agent contained in the reaction liquid for RAFT polymerization of this scheme is calculated as follows: Using Nanotrac UPA-EX150 manufactured by Nikkiso Co., Ltd., the volume-based particle size distribution of the polymer in the emulsion is measured by a measurement method based on dynamic light scattering (solvent: water, temperature 25), and the average particle size (volume average particle size) is calculated from the particle size distribution.

[0167] The molecular weight distribution of the hydrophilic copolymeric RAFT agent represented by Mw / Mn is preferably narrower, preferably 3.0 or less, more preferably 2.5 or less, further preferably 2.0 or less, particularly preferably 1.8 or less, and most preferably 1.6 or less. Usually, the lower limit of the molecular weight distribution is 1.0 or more.

[0168] The molecular weight distribution of the hydrophilic copolymeric RAFT agent contained in the reaction liquid for RAFT polymerization of this embodiment can be obtained as follows: using calcium chloride as a coagulant, the emulsion is coagulated at 60 to 95°C, dehydrated, washed, dried and recovered, dissolved in tetrahydrofuran, and the Mw and Mn converted to standard polystyrene are obtained by GPC.

[0169] The pH of the RAFT polymerization reaction liquid of the third embodiment is preferably 8 to 13, more preferably 7 to 13. Within this range, the dispersibility of the hydrophilic copolymeric RAFT agent in the RAFT polymerization reaction liquid is further improved. The method for measuring pH is as described above.

[0170] The content of the hydrophilic copolymeric RAFT agent before the RAFT polymerization reaction liquid of the third embodiment is used, that is, before the polymerizable monomer is added, preferably 0.1 to 20.0% by mass, more preferably 1.0 to 15.0% by mass, and further preferably 5.0 to 10.0% by mass, relative to the total mass of the RAFT polymerization reaction liquid of the third embodiment before use. Within the above preferred range, the monomers in the reaction liquid can be fully RAFT polymerized to obtain a polymer with a narrow molecular weight distribution in a short reaction time. The amount of coagulum remaining in the reaction liquid after the reaction can be reduced.

[0171] The hydrophilic copolymer-type RAFT agent contained in the reaction liquid for RAFT polymerization of the third embodiment may be one kind or two or more kinds.

[0172] When the RAFT polymerization reaction liquid of the third embodiment is used, a polymerization initiator may be added. The amount of the polymerization initiator added may be, for example, 0.01 to 0.1% by mass relative to the total mass of the RAFT polymerization reaction liquid of the third embodiment before the addition of the polymerizable monomer. The amount may be appropriately set according to the amount of the hydrophilic copolymer RAFT agent.

[0173] The polymerization initiator added to the reaction liquid for RAFT polymerization of the third embodiment may be one kind or two or more kinds.

[0174] The water content of the reaction solution for RAFT polymerization of the third embodiment before use, i.e., before adding the polymerizable monomer, is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more, relative to the total mass of the reaction solution for RAFT polymerization before use. As a standard for the upper limit value, for example, 99% by mass or less can be cited. When it is within the above preferred range, adding the monomer to the reaction solution can easily initiate RAFT polymerization.

[0175] The reaction liquid for RAFT polymerization of the third embodiment may or may not contain a dispersion medium other than water and other additives within a range that does not inhibit RAFT polymerization. Examples of the dispersion medium other than water include organic solvents miscible with water (eg, alcohol).

[0176] Examples of other additives include surfactants and the like.

[0177] The acid group of the hydrophilic copolymeric RAFT agent of this embodiment forms a salt, so the reactivity of the monomer is good. Therefore, RAFT polymerization can be carried out well even without using a surfactant.

[0178] <Production of Reaction Solution for RAFT Polymerization of the Third Aspect>

[0179] The reaction liquid for RAFT polymerization of the third embodiment is obtained by adding a polymerizable monomer to the reaction liquid for RAFT polymerization of the second embodiment and performing RAFT polymerization. The specific method is as described above.

[0180] <Use of the RAFT Polymerization Reaction Solution of the Third Aspect>

[0181] By adding one or more polymerizable monomers to the RAFT polymerization reaction solution of the third embodiment to carry out RAFT polymerization, a living radical polymerization reaction can be induced under the action of a hydrophilic copolymer RAFT agent, and a polymer with a narrow molecular weight distribution can be obtained in a short reaction time. The amount of residue (agglomerates) remaining as impurities in the reaction solution after the reaction can be reduced. Similarly, by using the obtained polymer solution as a RAFT polymerization reaction solution and further polymerizing the monomers, any multi-stage block copolymer solution can be obtained.

[0182] As the above-mentioned monomer, the monomers exemplified in the first embodiment can be mentioned. By using a monomer different in type or in combination with the ethylenically unsaturated monomer represented by X and Y constituting the above-mentioned hydrophilic copolymerizable RAFT agent, a monomer having the same structure as (X) of formula (3) can be obtained. n The block represented by (Y)m Triblock copolymers of different blocks.

[0183] The amount of the monomer added to the RAFT polymerization reaction liquid of the third embodiment is preferably 1 to 90 parts by mass, more preferably 3 to 60 parts by mass, and even more preferably 6 to 30 parts by mass, relative to 1 part by mass of the hydrophilic copolymeric RAFT agent contained in the reaction liquid. When it is within the above preferred range, the molecular weight distribution of the generated polymer can be further narrowed.

[0184] The reaction temperature in the RAFT reaction using the reaction solution for RAFT polymerization of the third embodiment is, for example, preferably 60 to 100° C., more preferably 70 to 90° C. At these preferred reaction temperatures, the typical reaction time until the RAFT reaction is completed is about 60 to 600 minutes.

[0185] Other reaction conditions in the RAFT reaction using the reaction solution for RAFT polymerization of the third embodiment can be appropriately set with reference to conventional RAFT polymerization.

[0186] More detailed examples of RAFT polymerization using the reaction solution for RAFT polymerization according to the third embodiment are shown in Examples 1c to 19c and the like described later.

[0187] <Method for recovering polymer from RAFT polymerization reaction liquid>

[0188] If necessary, the block copolymer can be recovered from the reaction solution for RAFT polymerization of the second embodiment and the third embodiment and the reaction solution after use (hereinafter sometimes collectively referred to as an aqueous dispersion).

[0189] Examples of methods for recovering block copolymers from aqueous dispersions include: (i) a method in which an aqueous dispersion of a block copolymer is added to hot water in which a coagulant is dissolved, and the block copolymer is recovered by coagulating it into a slurry state (wet method); and (ii) a method in which an aqueous dispersion of a block copolymer is sprayed in a heated atmosphere to semi-directly recover the block copolymer (spray drying method).

[0190] As the coagulant, there can be mentioned inorganic acids such as sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, and metal salts such as calcium chloride, calcium acetate, and aluminum sulfate. The coagulant can be selected according to the emulsifier used in the polymerization. In other words, when only carboxylic acid soaps such as fatty acid soaps and rosin acid soaps are used, any coagulant can be used. When an emulsifier such as sodium dodecylbenzene sulfonate is included that can show a stable emulsifying power even in an acidic region, a metal salt needs to be used.

[0191] As a method for obtaining a block copolymer in a dry state from a block copolymer in a slurry state, there can be listed: (i) after the emulsifier residue remaining in the slurry is dissolved into water by washing, the slurry is dehydrated with a centrifugal dehydrator or a pressure dehydrator, and then dried with an air flow dryer or the like; (ii) a method of simultaneously dehydrating and drying with a press dehydrator, an extruder, etc. After the drying, the block copolymer is obtained in the form of powder or particles. In addition, the block copolymer discharged from the press dehydrator or the extruder can also be directly transported to an extruder or a molding machine for manufacturing a thermoplastic resin composition.

[0192] <<Thermoplastic resin composition>>

[0193] The polymer obtained by RAFT polymerization using the reaction solution for RAFT polymerization of the first to third embodiments as described above is a thermoplastic resin reflecting the characteristics of each constituent block. Other optional components may be added to the thermoplastic resin as needed to prepare a thermoplastic resin composition.

[0194] Examples of other optional components include components that can be blended in known thermoplastic resin compositions, such as metal components, other thermoplastic resins other than the above-mentioned polymers, additives, and the like.

[0195] Examples of the metal component include alkali metals such as sodium and potassium.

[0196] Examples of other thermoplastic resins include polycarbonate, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyvinyl chloride, polystyrene, polyacetal, modified polyphenylene ether (modified PPE), ethylene-vinyl acetate copolymer, polyarylate, liquid crystal polyester, polyethylene, polypropylene, fluororesin, and polyamide (nylon).

[0197] As the additives, antioxidants, lubricants, processing aids, pigments, dyes, fillers, silicone oils and paraffin oils can be cited.

[0198] <Method for producing thermoplastic resin composition>

[0199] The method for producing the thermoplastic resin composition is not particularly limited. For example, the thermoplastic resin obtained by RAFT polymerization and other optional components as required can be mixed and dispersed using a V-type mixer, Henschel mixer, etc., and the mixture thus obtained is melt-kneaded using a melt-kneading machine such as a screw extruder, a Banbury mixer, a pressure kneading machine, a mixing roll, etc. to obtain a thermoplastic resin composition. After melt-kneading, the melt-kneaded product can also be granulated using a granulator, etc. as required.

[0200] <<Molding products>>

[0201] In this specification, the term "molded article" refers to a product obtained by molding a thermoplastic resin composition.

[0202] The thermoplastic resin composition is molded by a known molding method to obtain a molded product. Examples of the molding method include injection molding, press molding, extrusion molding, vacuum molding, and blow molding.

[0203] Examples of uses of the molded article include vehicle interior and exterior parts, office equipment, home appliances, and building materials.

[0204] <<Fourth Option>>

[0205] The fourth embodiment of the present invention is a method for producing a reaction solution for RAFT polymerization, comprising step 1 and step 2. Step 1 and step 2 of this embodiment are not limited to the examples in the following embodiments, and various modifications can be applied within the scope of the purpose of the present invention. The phrase "a step of obtaining ..." in this embodiment can also be expressed as "obtaining ...".

[0206] <Process 1>

[0207] Step 1 is a step of mixing a RAFT agent having an acid group represented by formula (1), water and a water-soluble inorganic base, forming a salt between at least a portion of the acid groups of the RAFT agent and cations derived from the water-soluble inorganic base, and obtaining a RAFT agent aqueous solution in which the RAFT agent is dissolved in water.

[0208]

[0209] [In formula (1), R 1 represents an organic group, the organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, and a part of the organic group represented by Z may be substituted.]

[0210] The above R 1 The organic group represented by is not particularly limited as long as it has the above-mentioned acid group, and any organic group can be applied. For example, an organic group having a C1-C10 straight-chain or branched monovalent alkyl group as a basic skeleton, wherein any one or more hydrogen atoms of the above-mentioned alkyl group are substituted by the above-mentioned acid group. Any one or more methylene groups constituting the above-mentioned alkyl group may be substituted by -O-, -C(=O)O-, -OC(=O)-, or -C(=O)NH- (except for the case where oxygen atoms are bonded to each other).

[0211] One or more hydrogen atoms in the above alkyl group may be substituted with -CN.

[0212] As a specific R 1 For example, -CH2CO2H, -CH2CH2CO2H, -CH(CH3)CO2H, -CH(CO2H)CH2CO2H, -C(CH3)(CH3)CO2H, -C(CN)(CH3)CH2CH2CO2H, -CH(CH3)CONR a R b .

[0213] The above R a and R b Each is independently selected from H, C1-C6 alkyl, C1-C6 alkoxy, C6-C12 aryl, C7-C18 alkylaryl and C6-C12 heteroaryl. a and R b At least one of the hydrogen atoms is substituted by an acid group selected from -CO2H, -SO3H and -PO4H. a and R b They may be the same as or different from each other.

[0214] The description of the organic group represented by Z is the same as the description of Z in the formula (1) of the first embodiment, and therefore, duplicate descriptions are omitted here.

[0215] A known RAFT agent can be used as the RAFT agent in step 1. However, the acid groups of known RAFT agents do not form salts, so in step 1, cations from the water-soluble inorganic base form salts with at least a part of the acid groups of the RAFT agent by mixing with water and a water-soluble inorganic base. Thus, an aqueous RAFT agent solution in which the RAFT agent (having an acid group that forms a salt) is dissolved in water is obtained.

[0216] The type of cation derived from a water-soluble inorganic base is not particularly limited, and examples thereof include cations of alkali metals such as sodium and potassium, and alkaline earth metals such as magnesium and calcium. From the viewpoint of enhancing the surface activity of the RAFT agent formed into a salt, alkali metals such as sodium and potassium are preferred.

[0217] The acid group possessed by the RAFT agent in step 1 is preferably one or more selected from -CO2H, -SO3H and -PO4H, and -CO2H is more preferred from the viewpoint of facilitating salt formation and adjusting the pH of the reaction solution.

[0218] The acid group of the RAFT agent represented by formula (1) forms a salt (hereinafter sometimes referred to as a salt of the RAFT agent (1)). Preferred examples include the compounds represented by formula (1a) to formula (1n) exemplified in the first embodiment.

[0219] As a salt of the RAFT agent (1) which is particularly preferred for ethylenically unsaturated monomers, for example, there can be mentioned a compound represented by the above formula (1-1). Furthermore, as a salt of the RAFT agent (1) which is particularly preferred for methacrylates, for example, there can be mentioned a compound represented by the above formula (1-2). In the formula, M + The definition of is the same as above.

[0220] As the water-soluble inorganic base, for example, a hydroxide having a hydroxide ion as an anion is preferred, and specific examples thereof include sodium hydroxide and potassium hydroxide. The water-soluble inorganic base is an inorganic base that dissolves 1 g or more per 100 g of water at 20°C.

[0221] The mixing ratio of the RAFT agent and the water-soluble inorganic base in step 1 is preferably a ratio at which the acid groups of the RAFT agent sufficiently form salts. Here, the number of moles M1 of the acid groups of the RAFT agent contained in the RAFT agent aqueous solution obtained in step 1 is considered.

[0222] When the RAFT agent mixed in step 1 has one acid group in the molecule, the number of moles M1 of the acid groups of the RAFT agent contained in the RAFT agent aqueous solution is the same as the number of moles of the molecules of the RAFT agent. When the number of acid groups in the RAFT agent molecule is m, the number of moles M1 of the acid groups of the RAFT agent contained in the RAFT agent aqueous solution is represented by the number of moles of the molecules of the RAFT agent × m.

[0223] In the RAFT agent aqueous solution obtained in step 1, the molar ratio of the molar number M1 of the acid group possessed by the above-mentioned RAFT agent to the molar number M4 of the above-mentioned water-soluble inorganic base is represented by (M4 / M1), and is preferably 1.0 to 10, more preferably 1.5 to 7.0, further preferably 2.0 to 5.0, particularly preferably 2.5 to 4.5, and most preferably 3.0 to 4.0.

[0224] When it is above the lower limit of the above range, the salt formation of the RAFT agent aqueous solution obtained in step 1 can be fully carried out, and the reaction time of RAFT polymerization (using the RAFT polymerization reaction solution obtained in the subsequent step 2) can be shortened, the yield of the target product is improved, the amount of coagulum can be reduced, and the molecular weight distribution of the target product can be narrowed.

[0225] When it is below the upper limit of the above range, the salt of the aqueous RAFT agent solution obtained in step 1 is stable, the pH of the RAFT polymerization reaction solution obtained in the subsequent step 2 is prevented from becoming too high, and the volume average particle size (MV) of the target product can be reduced.

[0226] The RAFT agent to be added in step 1 may be one kind or two or more kinds. The molar number M1 is the total molar number of the acid groups of all the RAFT agents.

[0227] The water-soluble inorganic base blended in step 1 may be one kind or two or more kinds. The molar number M4 is the total molar number of all inorganic bases.

[0228] <Process 2>

[0229] Step 2 is the following step: adding a water-soluble polymerization initiator (hereinafter sometimes referred to as a polymerization initiator) and an ethylenically unsaturated monomer to the above-mentioned RAFT agent aqueous solution, stirring, and subjecting the above-mentioned ethylenically unsaturated monomer dispersed in water to RAFT polymerization to obtain a RAFT polymerization reaction liquid (A) in which a polymer-type RAFT agent represented by formula (2) is dispersed in water.

[0230] Here, the water-soluble polymerization initiator refers to a polymerization initiator that can dissolve 1 g or more in 100 g of water at 20°C.

[0231] As the polymerization initiator of this process, a known free radical polymerization initiator can be applied. As a specific polymerization initiator, for example, inorganic peroxides such as potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, benzoyl peroxide, isobutyryl peroxide, azobisisobutyronitrile, 4-methoxy-azobisvaleronitrile, 4,4'-azobis(4-cyanovaleric acid) and other azo compounds can be listed, organic peroxides and ferrous sulfate, chelating agents and reducing agents are combined to form a redox initiator, for example, an initiator composed of cumene hydroperoxide, ferrous sulfate, sodium pyrophosphate and glucose, tert-butyl hydroperoxide, sodium formaldehyde sulfoxylate (Rongalite), ferrous sulfate and disodium ethylenediaminetetraacetic acid are combined to form an initiator, etc. Among them, from the viewpoint of improving the reactivity of the RAFT polymerization using the RAFT agent of this scheme, 4,4'-azobis(4-cyanovaleric acid) is preferred.

[0232] The polymerization initiator used in step 2 may or may not have an acid group. When the polymerization initiator has an acid group, the acid group may or may not form a salt, but from the viewpoint of fully obtaining the effect of the present invention, it is preferred to form a salt. As the acid group possessed by the polymerization initiator, for example, one or more selected from -CO2H, -SO3H and -PO4H can be cited. Among them, from the viewpoint of forming a salt and easily adjusting the pH of the reaction solution, -CO2H is preferred. When the number of acid groups possessed by the polymerization initiator in the molecule is n, the number of moles of the acid group of the polymerization initiator added in this step is represented by the number of moles of the molecules of the polymerization initiator × n.

[0233] In step 2, as a method for adding a water-soluble polymerization initiator to the RAFT agent aqueous solution obtained in step 1, the water-soluble polymerization initiator may be directly added to the RAFT agent aqueous solution, or an aqueous polymerization initiator solution prepared by dissolving the water-soluble polymerization initiator in water may be prepared first and then added to the RAFT agent aqueous solution. When the water-soluble polymerization initiator has an acid group, it is preferred to prepare an aqueous polymerization initiator solution and add a water-soluble inorganic base to the aqueous polymerization initiator solution to form a salt of the acid group of the water-soluble polymerization initiator from the viewpoint of fully obtaining the effects of the present invention.

[0234] The type of the water-soluble inorganic base optionally added in step 2 may be the same as the type of the water-soluble inorganic base added in step 1, or may be different.

[0235] In the above-mentioned polymerization initiator aqueous solution, when the above-mentioned polymerization initiator has an acid group, the molar ratio of the molar number M2 of the acid group to the molar number M5 of the above-mentioned water-soluble inorganic base arbitrarily added in step 2 is expressed by (M5 / M2), which is preferably 1.0 to 10, more preferably 1.5 to 7.0, further preferably 2.0 to 5.0, particularly preferably 2.5 to 4.5, and most preferably 3.0 to 4.0.

[0236] When it is at least the lower limit of the above range, the reaction time of RAFT polymerization using the reaction solution for RAFT polymerization obtained in step 2 can be shortened, the yield of the target product can be improved, the amount of coagulated materials can be reduced, and the molecular weight distribution of the target product can be narrowed.

[0237] When it is at most the upper limit value of the above range, the pH of the reaction solution for RAFT polymerization obtained in step 2 can be prevented from becoming too high, and the volume average particle size (MV) of the target product can be reduced.

[0238] In the reaction solution after adding the ethylenically unsaturated monomer and the water-soluble polymerization initiator to the aqueous solution of the RAFT agent and immediately before the polymerization starts, the molar ratio of the number of moles M1 of the acid group possessed by the RAFT agent, the number of moles M2 of the acid group arbitrarily possessed by the water-soluble polymerization initiator, the number of moles M4 of the water-soluble inorganic base added in the step 1, and the number of moles M5 of the water-soluble inorganic base that can be arbitrarily added in the step 2 is (M4+M5) / (M1+M2), preferably 1.0 to 10, more preferably 1.5 to 7.0, further preferably 2.0 to 5.0, particularly preferably 2.5 to 4.5, and most preferably 3.0 to 4.0.

[0239] When it is at least the lower limit of the above range, the reaction time of RAFT polymerization using the reaction solution for RAFT polymerization obtained in step 2 can be shortened, the yield of the target product can be improved, the amount of coagulated materials can be reduced, and the molecular weight distribution of the target product can be narrowed.

[0240] When it is at most the upper limit value of the above range, the pH of the reaction solution for RAFT polymerization obtained in step 2 can be prevented from becoming too high, and the volume average particle size (MV) of the target product can be reduced.

[0241] The polymerization initiator blended in step 2 may be one kind or two or more kinds. The molar number M2 is the total molar number of the acid groups of all the polymerization initiators.

[0242] The water-soluble inorganic base blended in step 2 may be one kind or two or more kinds. The molar numbers M4 and M5 are the total molar numbers of all the inorganic bases blended in each step.

[0243] In the reaction liquid for RAFT polymerization obtained in step 2, the molar ratio of the number of moles M1 of the acid group forming the salt of the above-mentioned RAFT agent, the number of moles M2 of the acid group capable of forming the salt of the above-mentioned polymerization initiator, and the total number of moles M3 (which may be M4+M5) of the water-soluble inorganic base added in steps 1 and 2 is M3 / (M1+M2), and the molar ratio is 1.0 to 10, preferably 1.5 to 7.0, more preferably 2.0 to 5.0, further preferably 2.5 to 4.5, and particularly preferably 3.0 to 4.0.

[0244] When it is at least the lower limit of the above range, the reaction time of RAFT polymerization using the reaction solution for RAFT polymerization can be shortened, the yield of the target product can be improved, the amount of coagulated materials can be reduced, and the molecular weight distribution of the target product can be narrowed.

[0245] When it is at most the upper limit of the above range, the pH of the reaction solution for RAFT polymerization can be prevented from becoming too high, and the volume average particle size (MV) of the target product obtained using the reaction solution for RAFT polymerization can be reduced.

[0246] In step 2, the content of the RAFT agent in the mixed solution at the stage where other components other than the polymerizable monomer are added is preferably 0.001 to 0.50 mass %, more preferably 0.01 to 0.20 mass %, and further preferably 0.03 to 0.10 mass % relative to the total mass of the mixed solution. When it is within the above preferred range, the monomers in the reaction solution can be fully RAFT polymerized in step 2, and a polymer with a narrow molecular weight distribution can be obtained in a short reaction time. The amount of coagulum remaining in the reaction solution after the reaction can be reduced.

[0247] In step 2, the content of the polymerization initiator in the mixed solution at the stage after the other components other than the polymerizable monomer are added is preferably 0.001 to 0.50 mass %, more preferably 0.01 to 0.20 mass %, and further preferably 0.03 to 0.10 mass % relative to the total mass of the mixed solution. When it is within the above preferred range, the monomers in the reaction solution can be fully RAFT polymerized in step 2, and a polymer with a narrow molecular weight distribution can be obtained in a short reaction time. The amount of coagulum remaining in the reaction solution after the reaction can be reduced.

[0248] In step 2, the water content in the mixed solution at the stage after the other components other than the polymerizable monomer are added is preferably 80% by mass or more, more preferably 90% by mass or more, and further preferably 95% by mass or more relative to the total mass of the mixed solution. As a standard for the upper limit value, for example, 99% by mass or less can be cited. When it is in the above preferred range, adding the monomer to the reaction solution in step 2 can easily initiate RAFT polymerization.

[0249] In step 2, the reaction solution for RAFT polymerization of the ethylenically unsaturated monomer may contain a dispersion medium other than water and other additives within the range that does not hinder RAFT polymerization, but preferably does not contain them. As a dispersion medium other than water, for example, an organic solvent (for example, alcohol) miscible with water can be cited. As other additives, for example, a surfactant can be cited.

[0250] Since the acid group of the RAFT agent in step 2 forms a salt, the reactivity of the monomer is good. Therefore, RAFT polymerization can be carried out well even without using a surfactant.

[0251] In step 2, by adding a polymerizable monomer to carry out RAFT polymerization, a living radical polymerization reaction can be induced under the action of a RAFT agent, and a polymer with a narrow molecular weight distribution (Mw / Mn) can be obtained in a short reaction time. The amount of residue (agglomerates) remaining as impurities in the reaction solution after the reaction can be reduced.

[0252] As the monomer, a radical polymerizable monomer is preferred, and an ethylenically unsaturated monomer is more preferred from the viewpoint of good reactivity. Examples of the ethylenically unsaturated monomer include monomers represented by the above formula (10).

[0253] The amount of the monomer added in step 2 is, for example, preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and even more preferably 10 to 25 parts by mass relative to 1 part by mass of the RAFT agent added in step 1. Within the above preferred range, the above effects can be further obtained.

[0254] In Step 2, the water content is preferably, for example, 50% by mass or more, more preferably 60% by mass or more, based on the total mass of the reaction solution after adding the above monomers.

[0255] From the viewpoints of increasing the monomer reaction rate in the RAFT polymerization in the above reaction solution, reducing the volume average particle diameter of the polymer (polymeric RAFT agent) obtained by RAFT polymerization, reducing the amount of agglomerates, and shortening the reaction time, the more the water content, the more preferable. For example, it is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably 98% by mass or more. As a standard for the upper limit value in this case, 99.5% by mass or less can be cited.

[0256] On the contrary, from the viewpoint of increasing the volume average particle diameter of the polymer (polymeric RAFT agent) obtained by RAFT polymerization in the above reaction solution, the less the water content, the more preferable. For example, it is preferably 97% by mass or less, more preferably 92% by mass or less, further preferably 85% by mass or less, and particularly preferably 75% by mass or less. As a standard for the lower limit value in this case, 50% by mass can be cited.

[0257] In Step 2, the reaction temperature of the above monomers is preferably, for example, 60 to 100 °C, more preferably 70 to 90 °C. Under the above preferred reaction temperature, the standard for the reaction time until the RAFT reaction is completed is about 200 to 1500 minutes.

[0258] In Step 2, other reaction conditions in the RAFT reaction of the above monomers are appropriately set with reference to conventional RAFT polymerization.

[0259] More detailed examples of the RAFT polymerization of the above monomers in Step 2 are shown in Examples 1a to 19a described later.

[0260] By the RAFT polymerization in Step 2, a RAFT polymerization reaction solution (A) containing a polymeric RAFT agent described below can be obtained.

[0261] <RAFT polymerization reaction solution (A)>

[0262] The RAFT polymerization reaction solution (A) is a dispersion of a polymeric RAFT agent represented by the formula (2) in water. At least a part of the acid groups possessed by the above polymeric RAFT agent forms a salt with the cation component of the water-soluble inorganic base used in the above manufacturing process.

[0263]

[0264] [In the formula (2), R 1represents an organic group, the organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 1000 (from the viewpoint of reducing the amount of coagulum, preferably 1 to 200, more preferably 1 to 100.), when n is 2 or more, a plurality of Xs may be the same or different from each other.]

[0265] R in formula (2) 1 The description of Z is the same as that of R in formula (1) of the first embodiment. 1 The descriptions of and Z are the same, so repeated descriptions are omitted here.

[0266] As any ethylenically unsaturated monomer represented by X, the above examples can be cited. Among them, styrene, acrylonitrile, butyl acrylate or (meth) acrylic acid is preferred from the perspective of facilitating RAFT polymerization using a polymeric RAFT agent. Only one of them can be used, or two or more of them can be used in combination.

[0267] In the above R 1 The above X bonded is an ethylenically unsaturated monomer, and the above R derived from the RAFT agent 1 In the case of an organic group having a carbon atom A bonded to the above X, the carbon atom A of the above organic group is preferably a tertiary carbon atom. In the case of a tertiary carbon atom, the substituent replacing the hydrogen atom of the above carbon atom A is preferably a linear or branched alkyl group having 1 to 6 carbon atoms, more preferably a linear alkyl group having 1 to 3 carbon atoms. In the above preferred case, the next step of RAFT polymerization using a polymeric RAFT agent becomes easy.

[0268] In the above R 1 The above X bonded is methacrylate, and the above R derived from the RAFT agent 1 In the case of an organic group having a carbon atom B bonded to the above-mentioned X, the above-mentioned carbon atom B of the above-mentioned organic group is preferably a quaternary carbon atom. In the case of a quaternary carbon atom, the two substituents replacing the hydrogen atoms of the above-mentioned carbon atom B are preferably independently a linear or branched alkyl group having 1 to 6 carbon atoms, and more preferably a linear alkyl group having 1 to 3 carbon atoms. Furthermore, it is preferred that at least one of the hydrogen atoms of the above-mentioned alkyl group constituting the above-mentioned substituent is substituted by a cyano group. As a particularly preferred example, the above-mentioned carbon atom B is a quaternary carbon atom bonded to an alkyl group having 1 to 3 carbon atoms and a cyano group. In these preferred cases, the next stage RAFT polymerization using a polymeric RAFT agent becomes easy.

[0269] It is preferred that the acid group forming the salt is bonded to the carbon atom A or the carbon atom B directly or via a linking group. Examples of the linking group include a linear or branched alkylene group having 1 to 6 carbon atoms. Any methylene group constituting the alkylene group may be substituted with -O-, -C(=O)O-, -OC(=O)-, or -C(=O)NH- (except for the case where oxygen atoms are bonded to each other).

[0270] The number of repeating units represented by n is preferably 5 or more, more preferably 10 or more, further preferably 20 or more, particularly preferably 30 or more, and most preferably 40 or more. Here, the number of repeating units refers to the total number of repeating units of one or more monomers corresponding to X.

[0271] When n is greater than the above lower limit, the polymerized site (X) n It can function as a block of a polymer.

[0272] The polymeric RAFT agent can form particles in the reaction solution for RAFT polymerization. The volume average particle size is preferably 5 to 500 nm, more preferably 7 to 100 nm, and further preferably 10 to 50 nm. When it is in the above preferred range, the advantages of improving the dispersibility of the polymeric RAFT agent in water and shortening the reaction time can be obtained.

[0273] The volume average particle size (MV) of the polymeric RAFT agent contained in the reaction solution (A) for RAFT polymerization can be determined as follows: using Nanotrac UPA-EX150 manufactured by Nikkiso Co., Ltd., the volume-based particle size distribution of the polymer in the emulsion is measured by a measurement method based on a dynamic light scattering method (solvent: water, temperature 25°C), and the average particle size (volume average particle size) is determined from the particle size distribution.

[0274] The molecular weight distribution of the polymeric RAFT agent represented by Mw / Mn is preferably narrower, preferably 2.0 or less, more preferably 1.8 or less, further preferably 1.6 or less, particularly preferably 1.4 or less, and most preferably 1.2 or less. Generally, the lower limit of the molecular weight distribution is 1.0 or more.

[0275] The molecular weight distribution of the polymeric RAFT agent contained in the reaction liquid (A) for RAFT polymerization can be obtained as follows: using calcium chloride as a coagulant, the emulsion is coagulated at 60 to 95°C, dehydrated, washed, dried and recovered, dissolved in tetrahydrofuran, and Mw and Mn converted to standard polystyrene are obtained by GPC.

[0276] The pH of the reaction liquid (A) for RAFT polymerization is preferably 8-13, more preferably 9-13, further preferably 10-13, particularly preferably 11-13, most preferably 12-13.

[0277] When the molecular weight is within the above preferred range, the molecular weight distribution of the polymer formed by RAFT polymerization using the reaction solution for RAFT polymerization (A) can be further narrowed.

[0278] The pH is a value measured at 25° C. according to the method specified in JIS Z8802: 2011. In this specification, the pH is expressed as an integer with an effective value to 1. That is, the first decimal place of the measured value is a rounded value.

[0279] The content of the polymeric RAFT agent before use of the reaction solution (A) for RAFT polymerization, i.e. before adding the polymerizable monomer, is preferably, for example, 0.01 to 10.0% by mass, more preferably 0.1 to 5.0% by mass, and further preferably 0.5% to 3.0% by mass relative to the total mass of the reaction solution (A) for RAFT polymerization before use. When it is within the above preferred range, the monomers in the reaction solution can be fully RAFT polymerized, and a polymer with a narrow molecular weight distribution can be obtained in a short reaction time. The amount of coagulum remaining in the reaction solution after the reaction can be reduced.

[0280] The polymeric RAFT agent contained in the reaction liquid for RAFT polymerization (A) may be one kind or two or more kinds.

[0281] The water content of the reaction solution (A) for RAFT polymerization before use, i.e., before adding the polymerizable monomer, is preferably 80% by mass or more, more preferably 90% by mass or more, and further preferably 95% by mass or more, relative to the total mass of the reaction solution (A) for RAFT polymerization before use. As a standard for the upper limit value, for example, 99% by mass or less can be cited. When it is in the above preferred range, adding the monomer to the reaction solution can easily initiate RAFT polymerization.

[0282] The RAFT polymerization reaction liquid (A) may contain a dispersion medium other than water and other additives within the range that does not hinder RAFT polymerization, but preferably does not contain. As a dispersion medium other than water, for example, an organic solvent (such as alcohol) that can be mixed with water can be cited. As other additives, for example, a surfactant can be cited.

[0283] Since the acid group of the polymeric RAFT agent in the reaction liquid for RAFT polymerization (A) forms a salt, the reactivity of the monomer is good. Therefore, RAFT polymerization can be carried out well even without using a surfactant.

[0284] <Process 3>

[0285] In the present invention, step 3 may be further performed after step 2.

[0286] Step 3 is a step of adding an ethylenically unsaturated monomer to the RAFT polymerization reaction liquid (A) obtained in step 2, stirring, and subjecting the ethylenically unsaturated monomer dispersed in water to RAFT polymerization, thereby obtaining a RAFT polymerization reaction liquid (B) in which a hydrophilic copolymerizable RAFT agent represented by formula (3) is dispersed in water.

[0287] In step 3, by adding one or more polymerizable monomers to the RAFT polymerization reaction solution (A) to carry out RAFT polymerization, a living radical polymerization reaction can be initiated under the action of a polymeric RAFT agent, and a polymer with a narrow molecular weight distribution can be obtained in a short reaction time. The amount of residue (agglomerates) remaining as impurities in the reaction solution after the reaction can be reduced.

[0288] Examples of the monomer include the monomers exemplified in step 2. By using a monomer different in type or blended differently from the ethylenically unsaturated monomer represented by X constituting the polymeric RAFT agent, a monomer having the same structure as (X) of formula (2) can be obtained. n The blocks represented are diblock copolymers of different blocks.

[0289] The amount of the monomer added to the RAFT polymerization reaction solution (A) is, for example, preferably 1 to 90 parts by mass, more preferably 5 to 60 parts by mass, and even more preferably 9 to 30 parts by mass relative to 1 part by mass of the polymeric RAFT agent contained in the reaction solution. When the amount is within the above preferred range, the molecular weight distribution of the generated polymer can be further narrowed.

[0290] In step 3, a polymerization initiator may be added to the RAFT polymerization reaction solution (A). The amount of the polymerization initiator added may be, for example, 0.01 to 0.1 mass % relative to the total mass of the RAFT polymerization reaction solution (A) before the addition of the polymerizable monomer. It is preferably appropriately set to be equimolar to the amount of the polymeric RAFT agent. For example, from the viewpoint of achieving stable RAFT polymerization, it is preferred to add about 1 to 5 mass parts of the polymerization initiator relative to 100 mass parts of the polymeric RAFT agent.

[0291] Examples of the polymerization initiator to be added include the polymerization initiators exemplified in step 2. The polymerization initiator to be added to the reaction solution (A) for RAFT polymerization may be one kind or two or more kinds.

[0292] The reaction temperature in the RAFT reaction using the reaction solution for RAFT polymerization (A) is, for example, preferably 60 to 100° C., more preferably 70 to 90° C. At the above preferred reaction temperature, the reaction time until the RAFT reaction is completed is typically about 60 to 600 minutes.

[0293] Other reaction conditions in the RAFT reaction using the RAFT polymerization reaction solution (A) can be appropriately set with reference to conventional RAFT polymerization.

[0294] More detailed examples of the RAFT polymerization using the RAFT polymerization reaction solution (A) are shown in Examples 1b to 19b described later.

[0295] By the RAFT polymerization using the RAFT polymerization reaction solution in Step 3, the hydrophilic copolymerizable RAFT agent described below can be obtained.

[0296] <RAFT polymerization reaction solution (B)>

[0297] The RAFT polymerization reaction solution (B) is formed by dispersing the hydrophilic copolymerizable RAFT agent represented by the formula (3) in water. At least a part of the acid groups possessed by the above-mentioned hydrophilic copolymerizable RAFT agent forms a salt with the cation component of the above-mentioned water-soluble inorganic base.

[0298]

[0299] [In the formula (3), R 1 represents an organic group, the above-mentioned organic group has one or more acid groups selected from -CO2H, -SO3H, and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group, and an aralkylthio group, a part of the above-mentioned organic group represented by Z may be substituted, X represents a repeating unit of an arbitrary ethylenically unsaturated monomer, n represents an integer of 1 to 100, when n is 2 or more, a plurality of Xs may be the same as or different from each other, Y is a repeating unit of an arbitrary ethylenically unsaturated monomer, m represents an integer of 10 to 10000, a plurality of Ys may be the same as or different from each other, the polymer chain represented by (X) n is different from the polymer chain represented by (Y) m .]

[0300] The descriptions of R 1 and Z in the formula (3) are the same as the descriptions of R 1 and Z in the formula (1), and therefore the repeated descriptions are omitted here.

[0301] The descriptions of X and n in the formula (3) are the same as the descriptions of X and n in the formula (2), and therefore the repeated descriptions are omitted here.

[0302] As the arbitrary ethylenically unsaturated monomer represented by the above-mentioned Y, the above-mentioned examples can be cited. Among them, from the viewpoint of facilitating the RAFT polymerization using the hydrophilic copolymerizable RAFT agent, styrene, acrylonitrile, butyl acrylate, or (meth)acrylic acid is preferred.

[0303] These may be used alone or in combination of two or more.

[0304] The number of repeating units represented by m is preferably 50 or more, more preferably 100 or more, further preferably 200 or more, particularly preferably 300 or more, and most preferably 400 or more. Here, the number of repeating units refers to the total number of repeating units of one or more monomers corresponding to Y.

[0305] When m is greater than the above lower limit, the polymerized site (Y) m It can function as a block of a polymer.

[0306] The hydrophilic copolymeric RAFT agent can form particles in the reaction solution for RAFT polymerization. The volume average particle size is preferably 10 to 500 nm, more preferably 15 to 300 nm, and further preferably 20 to 200 nm. When it is in the above preferred range, the advantages of improving the dispersibility of the hydrophilic copolymeric RAFT agent in water and shortening the reaction time can be obtained.

[0307] The volume average particle size (MV) of the hydrophilic copolymeric RAFT agent contained in the reaction liquid for RAFT polymerization of this scheme is calculated as follows: Using Nanotrac UPA-EX150 manufactured by Nikkiso Co., Ltd., the volume-based particle size distribution of the polymer in the emulsion is measured by a measurement method based on dynamic light scattering (solvent: water, temperature 25°C), and the average particle size (volume average particle size) is calculated from the particle size distribution.

[0308] The molecular weight distribution of the hydrophilic copolymeric RAFT agent represented by Mw / Mn is preferably narrower, preferably 3.0 or less, more preferably 2.5 or less, further preferably 2.0 or less, particularly preferably 1.8 or less, and most preferably 1.6 or less. Usually, the lower limit of the molecular weight distribution is 1.0 or more.

[0309] The molecular weight distribution of the hydrophilic copolymeric RAFT agent contained in the reaction liquid (B) for RAFT polymerization can be obtained as follows: using calcium chloride as a coagulant, the emulsion is coagulated at 60 to 95°C, dehydrated, washed, dried and recovered, dissolved in tetrahydrofuran, and Mw and Mn converted to standard polystyrene are obtained by GPC.

[0310] The pH of the RAFT polymerization reaction liquid (B) is preferably 8 to 13, more preferably 7 to 13. Within this range, the dispersibility of the hydrophilic copolymeric RAFT agent in the RAFT polymerization reaction liquid is further improved. The method for measuring pH is as described above.

[0311] Regarding the content of the above hydrophilic copolymerizable RAFT agent before use of the reaction liquid (B) for RAFT polymerization, that is, before adding the polymerizable monomer, relative to the total mass of the reaction liquid (B) for RAFT polymerization before use, it is preferably, for example, 0.1 to 20.0% by mass, more preferably 1.0 to 15.0% by mass, and still more preferably 5.0 to 10.0% by mass. When it is within the above preferred range, the monomers in the reaction liquid can sufficiently undergo RAFT polymerization, and a polymer with a narrow molecular weight distribution can be obtained within a short reaction time. The amount of clumps remaining in the reaction liquid after the reaction can be reduced.

[0312] The hydrophilic copolymerizable RAFT agent contained in the reaction liquid (B) for RAFT polymerization may be one kind or two or more kinds.

[0313] Regarding the water content before use of the reaction liquid (B) for RAFT polymerization, that is, before adding the polymerizable monomer, relative to the total mass of the reaction liquid (B) for RAFT polymerization before use, it is preferably, for example, 60% by mass or more, more preferably 70% by mass or more, and still more preferably 80% by mass or more. As a standard for the upper limit value, for example, 99% by mass or less can be cited. When it is within the above preferred range, adding the monomer to the reaction liquid can easily initiate RAFT polymerization.

[0314] Within the range that does not hinder RAFT polymerization, the reaction liquid (B) for RAFT polymerization may or may not contain a dispersion medium other than water and other additives. As a dispersion medium other than water, for example, an organic solvent (such as alcohol) that can be mixed with water can be cited. As other additives, for example, surfactants and the like can be cited.

[0315] Since the acid group of the hydrophilic copolymerizable RAFT agent in the reaction liquid (B) for RAFT polymerization forms a salt, the reactivity of the monomer is good. Therefore, RAFT polymerization can be carried out well even without using a surfactant.

[0316] <Use of the reaction liquid (B) for RAFT polymerization>

[0317] By adding one or more polymerizable monomers to the reaction liquid (B) for RAFT polymerization to carry out RAFT polymerization, an active radical polymerization reaction can be caused under the action of the hydrophilic copolymerizable RAFT agent, and a polymer with a narrow molecular weight distribution can be obtained within a short reaction time. The amount of residue (clumps) remaining as impurities in the reaction liquid after the reaction can be reduced.

[0318] As the above monomers, the monomers exemplified in Step 2 can be cited. By using monomers of different types or different formulations from the ethylenically unsaturated monomers represented by X and Y that constitute the above hydrophilic copolymerizable RAFT agent, a product having the same as (X) in Formula (3) nThe block represented by (Y) m Similarly, by using the obtained polymer solution as a reaction solution for RAFT polymerization and further polymerizing the monomers, an arbitrary multi-stage block copolymer solution can be obtained.

[0319] The amount of the monomer added to the RAFT polymerization reaction solution (B) is, for example, preferably 1 to 90 parts by mass, more preferably 3 to 60 parts by mass, and even more preferably 6 to 30 parts by mass, relative to 1 part by mass of the hydrophilic copolymeric RAFT agent contained in the reaction solution. When the amount is within the above preferred range, the molecular weight distribution of the generated polymer can be further narrowed.

[0320] When using the RAFT polymerization reaction solution (B), a polymerization initiator may be added. The amount of the polymerization initiator added may be, for example, 0.01 to 0.1% by mass relative to the total mass of the RAFT polymerization reaction solution (B) before adding the polymerizable monomer, and can be appropriately set according to the amount of the hydrophilic copolymer RAFT agent.

[0321] The polymerization initiator added to the reaction liquid (B) for RAFT polymerization may be one kind or two or more kinds.

[0322] The reaction temperature in the RAFT reaction using the reaction solution for RAFT polymerization (B) is, for example, preferably 60 to 100° C., more preferably 70 to 90° C. At the above preferred reaction temperature, the reaction time until the RAFT reaction is completed is typically about 60 to 600 minutes.

[0323] Other reaction conditions in the RAFT reaction using the reaction solution (B) for RAFT polymerization can be appropriately set with reference to conventional RAFT polymerization.

[0324] More detailed examples of RAFT polymerization using the reaction solution (B) for RAFT polymerization are shown in Examples 1c to 19c and the like described later.

[0325] <<Thermoplastic resin composition>>

[0326] The polymer obtained by RAFT polymerization using the RAFT polymerization reaction solution obtained by the production method of this embodiment is a thermoplastic resin reflecting the characteristics of each block. Other optional components can also be added to the thermoplastic resin as needed to prepare a thermoplastic resin composition. The description of the thermoplastic resin composition is as described above.

[0327] Example

[0328] <Experimental system focusing on particle size>

[0329] [Example 1a]

[0330] 138 parts by mass of water were added to a container equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dropping funnel, and a reflux condenser, 3.3 parts by mass of potassium hydroxide was dissolved, 6 parts by mass of 2-{[(dodecylsulfanyl)carbothioyl]sulfanyl}propanoic acid (manufactured by BRONMOLECULAR, model: BM1430) was added, and after nitrogen substitution, the mixture was stirred for 1 hour while being kept warm at 60°C. Thus, an aqueous solution of a saponified RAFT agent (the following formula Q) in which the carboxyl group of BM1430 was treated with potassium hydroxide was obtained. In the reaction solution, the molar ratio (base / acid group) of potassium hydroxide as a base to BM1430 as an acid was 3.4. Here, since BM1430 has one carboxyl group in the molecule, when the above molar ratio is produced, the number of moles of the acid group is equal to the number of moles of BM1430.

[0331] 200 parts by mass of water were added to a container equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dropping funnel, and a reflux condenser, 6.7 parts by mass of potassium hydroxide were dissolved, 5 parts by mass of 4,4'-azobis(4-cyanovaleric acid) (manufactured by Fuji Film & Wako Pure Chemical Industries, Ltd., model: V-501) were added, and after nitrogen substitution, the mixture was stirred at room temperature for 60 minutes. Thus, an initiator aqueous solution in which the carboxyl group of V-501 was treated with potassium hydroxide was obtained. In this reaction solution, the molar ratio (base / acid group) of potassium hydroxide as a base to V-501 as an acid was the same as that of the saponified RAFT agent aqueous solution, which was 3.4. Here, since V-501 has two carboxyl groups in the molecule, when calculating the above molar ratio, the number of moles of the acid group is twice the number of moles of V-501.

[0332]

[0333] Next, 9662 parts by mass of water were added to a reactor equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dropping funnel and a reflux condenser, and 147.3 parts by mass of the saponified RAFT agent aqueous solution, 211.7 parts by mass of the initiator aqueous solution, and 100 parts by mass of styrene (ST) were added and stirred, and nitrogen substitution was performed. The mass of the solute (solution concentration) was 1.20% by mass relative to the total mass of the reaction solution immediately before the reaction was started. Then, the mixture was heated to 80°C and stirred, and samples were taken at intervals of 30 minutes. The time point when the solid content (non-volatile component) did not change was considered as the completion of the reaction. As a result, the reaction was carried out for 300 minutes to obtain a RAFT polymerization reaction solution (A) in which a polymeric RAFT agent represented by the following formula X was dispersed in water.

[0334] At the time point when the reaction was completed, the total solid content contained in the reaction solution was 1.18% by mass, and the monomer reaction rate was 98.4%. Here, the total solid content refers to the total solid content contained in the total mass of the reaction solution. The monomer reaction rate is the value calculated by [(total solid content-RAFT agent added amount-polymerization initiator added amount-potassium hydroxide added amount) ÷ ST monomer added amount] × 100 (%).

[0335] In the above reaction solution, the volume average particle size (MV) of the polymeric RAFT agent represented by formula X is 10 nm. In each example, the volume average particle size (MV) is determined as follows: using Nanotrac UPA-EX150 manufactured by Nikkiso Co., Ltd., the volume-based particle size distribution of the polymer in the emulsion is measured by a measurement method based on a dynamic light scattering method (solvent: water, temperature 25° C.), and the average particle size (volume average particle size) is determined from the particle size distribution. The pH of the reaction solution is 11.

[0336] The amount of the agglomerated matter (reaction residue) agglomerated on the inner wall surface of the reactor was 0.1 parts by mass based on the styrene monomer used.

[0337] The polymeric RAFT agent was analyzed by GPC. As a result, the number average molecular weight (Mn) converted to standard polystyrene was 5,800, and the molecular weight distribution (Mw / Mn) was 1.1.

[0338]

[0339] [Example 1b]

[0340] 75 parts by mass of water were added to a reactor equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dropping funnel and a reflux condenser, and 424 parts by mass of a RAFT polymerization reaction solution (A) containing a polymeric RAFT agent having a pH of 11 obtained in Example 1a (5 parts by mass as a solid content) were added, followed by stirring and nitrogen substitution. Then, while heating to 80° C., 0.1 parts by mass of V-501 as a polymerization initiator was added, and then a mixed solution of 32.5 parts by mass of styrene and 12.5 parts by mass of acrylonitrile (AN) was dripped into the reactor over 60 minutes, and after completion of the dripping, stirring was continued for 30 minutes.

[0341] It was confirmed that the monomer reaction rate at this time was 95%. Here, the monomer reaction rate is a value calculated by [(total solid content - polymeric RAFT agent added amount - polymerization initiator added amount - amount of potassium hydroxide introduced) ÷ monomer added amount] × 100%. Since it is more than 90%, the reaction time is set to 90 minutes to complete the reaction. Thus, a RAFT polymerization reaction liquid (B) in which a block copolymer 1 represented by the following formula Y (hydrophilic copolymeric RAFT agent) is dispersed in water is obtained.

[0342] In the test examples described below, when a change in the solid content (non-volatile content) in the reaction solution is confirmed, if the monomer reaction rate does not exceed 90%, the stirring is extended until the monomer reaction rate exceeds 90% or the change in the solid content stabilizes to complete the reaction.

[0343] The volume average particle size (MV) of the block copolymer 1 represented by the formula Y was 20 nm. The pH of the reaction solution was 11, and the total solid content was 8.8% by mass.

[0344] Furthermore, the block copolymer 1 was analyzed by GPC. As a result, the number average molecular weight (Mn) in terms of standard polystyrene was 58,000, and the molecular weight distribution (Mw / Mn) was 1.5.

[0345]

[0346] [Example 1c]

[0347] While heating 544.1 parts by mass of the RAFT polymerization reaction liquid (B) containing the block copolymer 1 obtained in Example 1b to 80°C, 50 parts by mass of butyl acrylate (BA) was added dropwise over 30 minutes, followed by stirring for 60 minutes.

[0348] The monomer reaction rate at this time point was confirmed. Here, the monomer reaction rate is a value calculated by [(total solid content - amount of block copolymer 1 added - amount of potassium hydroxide brought in) ÷ amount of monomer added] × 100%. Since the monomer reaction rate is more than 90%, the reaction time is set to 90 minutes to complete the reaction. Thus, a dispersion of block copolymer 2 represented by the following formula Z is obtained.

[0349] In the test examples described below, when a change in the solid content (non-volatile content) in the reaction solution is confirmed, if the monomer reaction rate does not exceed 90%, the stirring is extended until the monomer reaction rate exceeds 90% or the change in the solid content is stabilized to complete the reaction.

[0350] In the above reaction solution, the volume average particle size (MV) of the block copolymer 2 represented by the formula Z was 30 nm. The pH of the reaction solution was 8, the total solid content was 16.2% by mass, and the reaction rate of the monomers in the step of Example 1c was 96.8%. The amount of the coagulum (reaction residue) condensed on the inner wall of the reactor was 0.1 parts by mass relative to the butyl acrylate monomer used.

[0351] The block copolymer 2 was analyzed by GPC. As a result, the number average molecular weight (Mn) in terms of standard polystyrene was 116,000, and the molecular weight distribution (Mw / Mn) was 1.8.

[0352]

[0353] [Example 2a to Example 6a, Example R1a, Example R2a]

[0354] As shown in Table 1, the concentration of each component in the reaction solution immediately before the reaction was changed, and the other steps were carried out in the same manner as in Example 1a to obtain a reaction solution (A) for RAFT polymerization containing a polymeric RAFT agent represented by the above formula X. The measurement results of the volume average particle size (MV) and the like of the obtained polymeric RAFT agent are shown in Table 1. The concentration of each component in the reaction solution was adjusted by increasing or decreasing the amount of water in the reaction solution.

[0355] [Table 1]

[0356]

[0357] The volume average particle size (MV) of Example R1a is small, while the reaction time of Example R2a is long, the amount of coagulated products is large, and the molecular weight distribution is wide. From the viewpoint of improving productivity, it is preferred to have a volume average particle size (MV) of a certain value or more, react in a shorter reaction time, reduce the amount of coagulated products, and narrow the molecular weight distribution.

[0358] [Example 2b to Example 6b, Example R1b, Example R2b]

[0359] As shown in Table 2, the reaction solution (A) for RAFT polymerization containing each polymeric RAFT agent obtained in Examples 2a to 6a, Example R1a, and Example R2a was used, and the reaction time and the like were changed to allow the reaction to proceed sufficiently, and the other steps were carried out in the same manner as in Example 1b to obtain a block copolymer 1 represented by the above formula Y. The measurement results of the volume average particle size (MV) and the like of the obtained block copolymer 1 are shown in Table 2.

[0360] [Table 2]

[0361]

[0362] Example R1b has a broad molecular weight distribution, while Example R2b has a broad molecular weight distribution after a long reaction time. From the viewpoint of improving productivity, it is preferred to react in a shorter reaction time to narrow the molecular weight distribution.

[0363] [Example 2c to Example 6c, Example R1c, Example R2c]

[0364] As shown in Table 3, the reaction solution (B) for RAFT polymerization containing each block copolymer 1 obtained in Examples 2b to 6b, Example R1b, and Example R2b was used, and the reaction time and the like were changed so that the reaction proceeded sufficiently, and the other conditions were the same as in Example 1b to obtain a block copolymer 2 represented by the above formula Z. The measurement results of the volume average particle size (MV) and the like of the obtained block copolymer 2 are shown in Table 3.

[0365] [Table 3]

[0366]

[0367] Example R1c has a wide molecular weight distribution, while Example R2c has a long reaction time, a large amount of coagulated materials, and a wide molecular weight distribution. From the viewpoint of improving productivity, it is preferred to react in a shorter reaction time, reduce the amount of coagulated materials, and narrow the molecular weight distribution.

[0368] <Experimental system focusing on alkali amount>

[0369] [Examples 7a to 9a, Example R3a, Example R4a]

[0370] As shown in Table 4, the carboxyl groups of BM1430 were saponified, and the molar ratio of the base / acid group was changed to maintain the state, and the other procedures were carried out in the same manner as in Example 1a to obtain a RAFT polymerization reaction solution (A) containing a polymeric RAFT agent represented by the above formula X. The measurement results of the molecular weight distribution and the like of the obtained polymeric RAFT agent are shown in Table 4.

[0371] [Table 4]

[0372]

[0373] Since Examples R3a and R4a do not satisfy the range of the molar ratio {M3 / (M1+M2)} of the first embodiment of the invention, that is, the above-mentioned [1-1], they are comparative examples for the first embodiment of the invention.

[0374] The molar ratio of the base / acid group in Example R3a is small, the yield is low, the amount of coagulation is large, and the molecular weight distribution is wide. From the viewpoint of improving productivity and the quality of the polymer, it is preferred to react in a shorter reaction time, reduce the amount of coagulation, and narrow the molecular weight distribution. The molar ratio of the base / acid group in Example R4b is large, and the pH of the reaction solution is high. In the subsequent steps (enlargement treatment or coagulation treatment, etc.), the decomposition reaction of the monomer may occur at the same time, and the reaction yield is reduced. Therefore, from the viewpoint of improving productivity, it is not preferred that the pH is too high.

[0375] [Example 7b to Example 9b, Example R3b, Example R4b]

[0376] As shown in Table 5, a RAFT polymerization reaction solution (A) containing each polymeric RAFT agent obtained in Examples 7a to 9a, Example R3a, and Example R4a was used, and the reaction time was changed to allow the reaction to proceed sufficiently. Otherwise, the reaction was carried out in the same manner as in Example 1b to obtain a block copolymer 1 represented by the above formula Y.

[0377] Table 5 shows the measurement results of the molecular weight distribution and the like of the obtained block copolymer 1.

[0378] [Table 5]

[0379]

[0380] The molecular weight distribution of Example R3b is broad. The molecular weight distribution of Example R4b is broad. From the viewpoint of improving the quality of the polymer, it is preferred to narrow the molecular weight distribution.

[0381] [Example 7c to Example 9c, Example R3c, Example R4c]

[0382] As shown in Table 6, a RAFT polymerization reaction solution (B) containing each block copolymer 1 obtained in Examples 7b to 9b, Example R3b, and Example R4b was used, and the reaction time was changed to allow the reaction to proceed sufficiently. Otherwise, the reaction was carried out in the same manner as in Example 1b to obtain a block copolymer 2 represented by the above formula Z.

[0383] Table 6 shows the measurement results of the molecular weight distribution and the like of the obtained block copolymer 2.

[0384] [Table 6]

[0385]

[0386] The amount of coagulated material in Example R3c is large and the molecular weight distribution is broad. From the viewpoint of improving productivity and polymer quality, it is preferred to reduce the amount of coagulated material and narrow the molecular weight distribution. The molecular weight distribution of Example R4c is broad. From the viewpoint of improving polymer quality, it is preferred to narrow the molecular weight distribution.

[0387] <Experimental system focusing on the amount of RAFT agent>

[0388] [Examples 10a to 13a, Example R5a, Example R6a]

[0389] As shown in Table 7, the RAFT polymerization reaction solution (A) containing the polymeric RAFT agent represented by the above formula X was obtained in the same manner as in Example 1a except that the amounts of V-501 and BM1430 were changed and the amount of potassium hydroxide was adjusted so that the molar ratio of the base / acid group was constant.

[0390] Table 7 shows the measurement results of the molecular weight distribution and the like of the obtained polymeric RAFT agent.

[0391] [Table 7]

[0392]

[0393] The volume average particle size (MV) of Example R5a is small. From the viewpoint of improving productivity, a volume average particle size (MV) of a certain value or more is preferred. In Example R6a, the amount of coagulated materials is large and the molecular weight distribution is wide. From the viewpoint of improving productivity and the quality of the polymer, it is preferred to reduce the amount of coagulated materials and narrow the molecular weight distribution.

[0394] [Examples 10b to 13b, Example R5b, Example R6b]

[0395] As shown in Table 8, the RAFT polymerization reaction solution (A) containing each polymeric RAFT agent obtained in Examples 10a to 13a, Example R5a, and Example R6a was used. In order to make the number of molecules of the polymeric RAFT agent contained in the reaction solution of each Example the same, the amount of the RAFT agent was changed, and the reaction time was changed so that the reaction proceeded sufficiently. The block copolymer 1 represented by the above formula Y was obtained in the same manner as in Example 1b.

[0396] Table 8 shows the measurement results of the molecular weight distribution and the like of the obtained block copolymer 1.

[0397] [Table 8]

[0398]

[0399] The reaction time of Example R5b is long and the molecular weight distribution is wide. From the viewpoint of improving productivity, it is preferred to react in a shorter reaction time and narrow the molecular weight distribution. The molecular weight distribution of Example R6b is wide. From the viewpoint of improving the quality of the polymer, it is preferred to narrow the molecular weight distribution.

[0400] [Examples 10c to 13c, Example R5c, Example R6c]

[0401] As shown in Table 9, a RAFT polymerization reaction solution (B) containing each block copolymer 1 obtained in Examples 10b to 13b, Example R5b, and Example R6b was used, and the reaction time was changed to allow the reaction to proceed sufficiently. Otherwise, the reaction was carried out in the same manner as in Example 1c to obtain a block copolymer 2 represented by the above formula Z.

[0402] Table 9 shows the measurement results of the molecular weight distribution and the like of the obtained block copolymer 2.

[0403] [Table 9]

[0404]

[0405] In Example R5c, the reaction time was long, the amount of coagulated products was large, and the molecular weight distribution was broad. From the viewpoint of improving productivity and polymer quality, it is preferred to react in a shorter reaction time, reduce the amount of coagulated products, and narrow the molecular weight distribution.

[0406] In Example R6c, the amount of coagulated materials is large and the molecular weight distribution is broad. From the viewpoint of improving productivity and polymer quality, it is preferred to reduce the amount of coagulated materials and narrow the molecular weight distribution.

[0407] <Experimental system focusing on the types of monomers that form polymeric RAFT agents>

[0408] [Examples 14a to 19a]

[0409] As shown in Table 10, the types of monomers to be polymerized were changed, the types of corresponding RAFT agents were combined, and the other operations were carried out in the same manner as in Example 1a to obtain a RAFT polymerization reaction solution (A) containing a polymeric RAFT agent represented by the above formula X. The PS chain block of the above formula X was replaced by a polymer chain of the monomer used in each example. The measurement results of the number average molecular weight and the like of the obtained polymeric RAFT agent are shown in Table 10.

[0410] [Table 10]

[0411]

[0412] The effect of the RAFT agent sometimes differs depending on the type of monomer to be polymerized. Example 17a has a wider molecular weight distribution than Example 3a. From the viewpoint of improving productivity, BM1430 is preferably used for styrene monomer. Example 16a has a wider molecular weight distribution and a longer reaction time than Example 19a. From the viewpoint of improving productivity and polymer quality, BM1432 is preferably used for methyl methacrylate.

[0413] [Example 14b to Example 19b]

[0414] As shown in Table 11, the block copolymer 1 represented by the above formula Y was obtained in the same manner as in Example 1b except for changing the amount of monomers blended, using the reaction solution (A) for RAFT polymerization containing each polymeric RAFT agent obtained in Examples 14a to 19a. The PS chain block of the above formula Y was replaced by a polymer chain derived from the polymeric RAFT agent of each example.

[0415] Table 11 shows the measurement results of the number average molecular weight and the like of the obtained block copolymer 1.

[0416] [Table 11]

[0417]

[0418] [Example 14c to Example 19c]

[0419] As shown in Table 12, the RAFT polymerization reaction solution (B) containing each block copolymer 1 obtained in Example 14b to Example 19b was used, and the other steps were carried out in the same manner as in Example 1c to obtain a block copolymer 2 represented by the above formula Z. The PS chain block of the above formula Z was replaced by a polymer chain from the polymeric RAFT agent of each example. The measurement results of the number average molecular weight and the like of the obtained block copolymer 2 are shown in Table 12.

[0420] [Table 12]

[0421]

[0422] <Experimental system focusing on the amount of polymeric RAFT agent used>

[0423] [Example 20b to Example 22b]

[0424] As shown in Table 13, the block copolymer 1 represented by the above formula Y was obtained in the same manner as in Example 1b except that the amounts used were changed, using the reaction solution (A) for RAFT polymerization containing each polymeric RAFT agent obtained in Example 3a.

[0425] Table 13 shows the measurement results of the number average molecular weight and the like of the obtained block copolymer 1.

[0426] [Table 13]

[0427]

[0428] From the results in Table 13, diblock copolymers with narrow molecular weight distribution and various molecular weights can be obtained.

[0429] [Example 20c to Example 22c]

[0430] As shown in Table 14, the block copolymer 2 represented by the above formula Z was obtained in the same manner as in Example 1c except for using the reaction solution (B) for RAFT polymerization containing each block copolymer 1 obtained in Example 20b to Example 22b.

[0431] Table 14 shows the measurement results of the number average molecular weight and the like of the obtained block copolymer 2.

[0432] [Table 14]

[0433]

[0434] From the results in Table 14, it is possible to obtain triblock copolymers having a narrow molecular weight distribution and various molecular weights.

[0435] <Experimental system focusing on monomer types forming copolymer 1>

[0436] [Example 23b to Example 29b]

[0437] As shown in Table 15, the RAFT polymerization reaction solution (A) containing the polymeric RAFT agent obtained in Example 3a was used, and the types and composition ratios of the monomers polymerized in the reaction solution were changed, and the block copolymer 1 represented by the above formula Y was obtained in the same manner as in Example 1b. However, the AS chain block of the above formula Y was replaced by the (co)polymer chain of the monomer used in each example.

[0438] Table 15 shows the measurement results of the number average molecular weight and the like of the obtained block copolymer 1.

[0439] [Table 15]

[0440]

[0441] From the results in Table 15, it can be seen that for polymeric RAFT agents, a variety of monomers can be polymerized in the same manner to obtain a large number of diblock copolymers.

[0442] [Example 23c to Example 29c]

[0443] As shown in Table 16, the RAFT polymerization reaction solution (B) containing each block copolymer 1 obtained in Example 23b to Example 29b was used, and the type and composition ratio of the monomers polymerized in the solution were changed, and the other was carried out in the same manner as in Example 1c to obtain a block copolymer 2 represented by the above formula Z. Among them, the PBA chain block of the above formula Z was replaced by the (co)polymer chain of the monomer used in each example. The measurement results of the number average molecular weight, etc. of the obtained block copolymer 2 are shown in Table 16.

[0444] [Table 16]

[0445]

[0446] From the results in Table 16, it can be seen that, for Block Copolymer 1, a variety of monomers can be polymerized in the same manner to obtain a large number of triblock copolymers.

[0447] Industrial Applicability

[0448] The RAFT polymerization reaction liquid suitable for RAFT polymerization is suitable for the production of any polymer with narrow molecular weight distribution, block copolymer, etc. The obtained polymer can be used as an aqueous dispersion, for example, for adhesives, adhesives, coatings, etc. The resin composition recovered by coagulation, etc. can be used, for example, for molded bodies, films, sheets, etc.

Claims

1. A reaction solution for RAFT polymerization, characterized in that: The RAFT polymerization reaction liquid comprises a RAFT agent represented by formula (1), water and a water-soluble inorganic base, and may comprise a polymerization initiator as an arbitrary component. The molar ratio M3 / (M1+M2) of the number of moles M1 of the acid groups of the RAFT agent, the number of moles M2 of the acid groups that the polymerization initiator may have, and the number of moles M3 of the water-soluble inorganic base is 1.0 to 10, At least a part of the acid groups of the RAFT agent and at least a part of the acid groups that the polymerization initiator may have form a salt with the cationic component of the water-soluble inorganic base, In formula (1), R 1 represents an organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, and a part of the organic group represented by Z may be substituted.

2. The reaction solution for RAFT polymerization according to claim 1, wherein In the formula (1), Z is an alkylthio group which may be substituted.

3. The reaction solution for RAFT polymerization according to claim 1, wherein The polymerization initiator is a water-soluble polymerization initiator.

4. A reaction solution for RAFT polymerization, characterized in that: comprising a polymeric RAFT agent represented by formula (2), water and a water-soluble inorganic base, At least a part of the acid groups of the polymeric RAFT agent forms a salt with the cationic component of the water-soluble inorganic base, In formula (2), R 1 represents an organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 1000, and when n is 2 or more, a plurality of Xs may be the same as or different from each other.

5. The reaction solution for RAFT polymerization according to claim 4, wherein The R 1 is an organic group having a carbon atom bonded to the X, wherein the carbon atom of the organic group is a tertiary carbon.

6. The reaction solution for RAFT polymerization according to claim 4, wherein Bonded with the R 1 The X is methacrylate, the R 1 is an organic group having a carbon atom bonded to the X, wherein the carbon atom of the organic group is a quaternary carbon, and a cyano group is bonded to the carbon atom.

7. A reaction solution for RAFT polymerization, characterized in that: comprising a hydrophilic polymeric RAFT agent represented by formula (3), water and a water-soluble inorganic base, At least a part of the acid groups of the hydrophilic polymeric RAFT agent forms a salt with the cationic component of the water-soluble inorganic base, In formula (3), R 1 represents an organic group, the organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 100, and when n is 2 or more, a plurality of Xs may be the same as or different from each other, Y represents a repeating unit of any ethylenically unsaturated monomer, m represents an integer of 10 to 10000, and a plurality of Ys may be the same as or different from each other, (X) n The polymer chain represented by (Y) m The represented polymer chains are different from each other.

8. A method for producing a reaction solution for RAFT polymerization, characterized in that: include: Step 1, mixing a RAFT agent having an acid group represented by formula (1), water and a water-soluble inorganic base, so that at least a part of the acid groups of the RAFT agent and a cation derived from the water-soluble inorganic base form a salt, thereby obtaining a RAFT agent aqueous solution in which the RAFT agent is dissolved in water; and Step 2, adding a water-soluble polymerization initiator and an ethylenically unsaturated monomer to the aqueous RAFT agent solution, stirring, and subjecting the ethylenically unsaturated monomer dispersed in water to RAFT polymerization, thereby obtaining a RAFT polymerization reaction solution (A) in which a polymeric RAFT agent represented by formula (2) is dispersed in water, In formula (1), R 1 represents an organic group having one or more acid groups selected from -CO2H, -SO3H and -PO4H, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, and a part of the organic group represented by Z may be substituted, In formula (2), R 1 represents an organic group, the organic group has one or more acid groups selected from -CO2H, -SO3H and -PO4H, and the acid groups form a salt, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 1000, and when n is 2 or more, multiple Xs may be the same as or different from each other.

9. The method for producing a reaction solution for RAFT polymerization according to claim 8, wherein The pH of the reaction solution (A) for RAFT polymerization obtained in the step 2 is 8 to 13.

10. The method for producing a reaction solution for RAFT polymerization according to claim 8, wherein In the reaction solution immediately before the polymerization starts after the ethylenically unsaturated monomer and the water-soluble polymerization initiator are added to the aqueous solution of the RAFT agent, The molar ratio (M4+M5) / (M1+M2) of the molar number M1 of the acid group possessed by the RAFT agent, the molar number M2 of the acid group optionally possessed by the water-soluble polymerization initiator, the molar number M4 of the water-soluble inorganic base added in the step 1, and the molar number M5 of the water-soluble inorganic base that can be arbitrarily added in the step 2 is 1.0 to 10.

11. The method for producing a reaction solution for RAFT polymerization according to claim 8, wherein: The method further comprises a step 3 of adding an ethylenically unsaturated monomer to the RAFT polymerization reaction solution (A) obtained in the step 2, stirring the mixture, and subjecting the ethylenically unsaturated monomer dispersed in water to RAFT polymerization, thereby obtaining a RAFT polymerization reaction solution (B) in which a hydrophilic copolymerizable RAFT agent represented by formula (3) is dispersed in water. In formula (3), R 1 represents an organic group, the organic group has one or more acid groups selected from -CO2H, -SO3H and -PO4H, and the acid groups form a salt, Z represents an organic group selected from an alkyl group, an aryl group, an aralkyl group, an alkylthio group, an arylthio group and an aralkylthio group, a part of the organic group represented by Z may be substituted, X represents a repeating unit of any ethylenically unsaturated monomer, n represents an integer of 1 to 100, and when n is 2 or more, a plurality of Xs may be the same as or different from each other, Y represents a repeating unit of any ethylenically unsaturated monomer, m represents an integer of 10 to 10000, and a plurality of Ys may be the same as or different from each other, (X) n The polymer chain represented by (Y) m The represented polymer chains are different from each other.

12. The method for producing a reaction solution for RAFT polymerization according to claim 11, wherein The pH of the reaction solution (B) for RAFT polymerization obtained in the step 3 is 8 to 13.

13. The method for producing a reaction solution for RAFT polymerization according to claim 11, wherein In the step 3, a water-soluble polymerization initiator is added to the reaction solution (A) for RAFT polymerization.