Method for producing hydrogenated polymer using multiple solvents

By using a mixed solvent that adjusts the Hansen solubility parameter, the problem of low solubility of aromatic polymers after hydrogenation is solved, productivity and reaction speed are improved, and uniform dissolution of the polymer in the solvent is achieved.

CN118829664AInactive Publication Date: 2024-10-22MITSUBISHI GAS CHEM CO INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380025249.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-11
Filing Date
2023-04-10
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the hydrogenation process of aromatic polymers, the hydrogenated polymer obtained after hydrogenation has low solubility in the reaction solvent, resulting in precipitation and affecting productivity.

Method used

A mixed solvent containing at least one first solvent and at least one second solvent is used, and the Hansen solubility parameter (HSP) is adjusted to ensure that the polymer before and after hydrogenation can be dissolved in the solvent to avoid the formation of precipitation.

Benefits of technology

The productivity and reaction speed are improved, the precipitate removal process after hydrogenation is avoided, and the uniform dissolution state of the polymer in the solvent is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024781050000291
    Figure BDA0005024781050000291
Patent Text Reader

Abstract

The present invention relates to a hydrogenation method using a solvent capable of well dissolving a polymer before and after hydrogenation. According to the present invention, provided is a method for producing a hydrogenated polymer by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer, the method comprising a step of performing a hydrogenation reaction using an aromatic vinyl compound-based polymer, a solvent, and a hydrogenation catalyst, the solvent is a mixed solvent containing at least one first solvent and at least one second solvent, and the Hansen solubility parameter (HSP) value 1 of the mixed solvent falls into Hansen spheres in a three-dimensional space formed by the [delta] d axis, the [delta] p axis and the [delta] h axis of the aromatic vinyl compound-based polymer before hydrogenation. And 2) falls into Hansen spheres in a three-dimensional space comprising the [delta] d axis, the [delta] p axis, and the [delta] h axis of the hydrogenated aromatic vinyl compound polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a hydrogenated polymer using various solvents, etc. In particular, the present invention relates to a method for producing a hydrogenated polymer by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation). Background Art

[0002] In recent years, polymers represented by acrylic resins, methacrylic resins, styrene resins, polycarbonate resins, and cyclic polyolefin resins have been used for various purposes, and in particular, due to their optical properties, they are in great demand as optical materials such as optical lenses and optical disk substrates. Such optical materials are required to have not only high transparency but also high heat resistance, low water absorption, and excellent balance of mechanical properties.

[0003] In order to meet such demands, various improvements of polymers have been made. One example of such improvements is hydrogenation (ring hydrogenation) of aromatic polymers.

[0004] For example, Japanese Patent No. 5540703 (Patent Document 1) relates to the hydrogenation of aromatic vinyl compounds / (meth)acrylate copolymers, and Japanese Patent Publication No. 2014-77044 (Patent Document 2) relates to a method for producing a ring-hydrogenated polymer using a sulfur-free raw material. In addition, Japanese Patent No. 2890748 (Patent Document 3) relates to a method for producing a hydrogenated styrene resin, and Japanese Patent Table No. 2001-527095 (Patent Document 4), Japanese Patent Table No. 2002-511501 (Patent Document 5) and Japanese Patent Table No. 2002-511508 (Patent Document 6) relate to a method for hydrogenating aromatic polymers. Japanese Patent No. 4224655 (Patent Document 7) and Japanese Patent No. 5007688 (Patent Document 8) relate to alicyclic hydrocarbon copolymers or polymers containing alicyclic structures, and record that these polymers can be obtained by hydrogenation of aromatic polymers.

[0005] Prior Art Literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 5540703

[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-77044

[0009] Patent Document 3: Japanese Patent No. 2890748

[0010] Patent Document 4: Japanese Patent Application No. 2001-527095

[0011] Patent Document 5: Japanese Patent Publication No. 2002-511501

[0012] Patent Document 6: Japanese Patent Application No. 2002-511508

[0013] Patent Document 7: Japanese Patent No. 4224655

[0014] Patent Document 8: Japanese Patent No. 5007688 Summary of the invention

[0015] Problems to be solved by the invention

[0016] However, in the hydrogenation process of an aromatic polymer, precipitation may occur due to the low solubility of the hydrogenated polymer obtained after hydrogenation in the reaction solvent. The productivity may be reduced including the step of removing the precipitate.

[0017] Under the above circumstances, there is a demand for a hydrogenation method using a solvent that can well dissolve the polymer before and after hydrogenation.

[0018] Technical means to solve problems

[0019] The inventors of the present invention have conducted intensive research and found that in a method for producing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer, a mixed solvent comprising at least one first solvent and at least one second solvent is used, and the Hansen Solubility Parameter (HSP) of each solvent or their mixed solvent is adjusted, thereby completing the present invention.

[0020] That is, the present invention provides the following production method and the like.

[0021] [1] A method for producing a hydrogenated polymer, comprising: hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer to produce a hydrogenated polymer.

[0022] The production method comprises the steps of carrying out a hydrogenation reaction using the aromatic vinyl compound polymer, a solvent and a hydrogenation catalyst.

[0023] The above-mentioned solvent is a mixed solvent comprising at least one first solvent and at least one second solvent,

[0024] The Hansen Solubility Parameter (HSP) value of the above mixed solvents

[0025] 1) falls into the Hansen sphere in the three-dimensional space consisting of the δd axis, δp axis and δh axis of the aromatic vinyl compound-based polymer before hydrogenation, and

[0026] 2) It falls into the Hansen sphere in the three-dimensional space consisting of the δd axis, δp axis and δh axis of the hydrogenated aromatic vinyl compound-based polymer.

[0027] [2] A method for producing a hydrogenated polymer, comprising: hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer to produce a hydrogenated polymer,

[0028] The production method comprises the steps of carrying out a hydrogenation reaction using the aromatic vinyl compound polymer, a solvent and a hydrogenation catalyst.

[0029] The above-mentioned solvent is a mixed solvent comprising at least one first solvent and at least one second solvent,

[0030] The Hansen Solubility Parameters (HSP) of the at least one first solvent are as follows,

[0031] δd: 10 to 20 (preferably 11 to 19, more preferably 12 to 18, and even more preferably 14 to 17), δp: 1 to 15 (preferably 2 to 12, more preferably 3 to 10, and even more preferably 4 to 8),

[0032] δh: 1 to 25 (preferably 2 to 20, more preferably 4 to 15, and even more preferably 5 to 10),

[0033] The HSP of the at least one second solvent is as follows,

[0034] δd: 10 to 20 (preferably 11 to 19, more preferably 12 to 18, and even more preferably 14 to 18),

[0035] δp: 0 or more and less than 1 (preferably 0 to 0.9, more preferably 0 to 0.6, and even more preferably 0 to 0.4),

[0036] δh: 0 to 2 (preferably 0 to 1.5, more preferably 0 to 1, and even more preferably 0 to 0.8),

[0037] The weight ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:1 (preferably 2:8 to 9:1, more preferably 2:8 to 8:2),

[0038] The first solvent is a solvent selected from the group consisting of ester solvents, aromatic solvents, monocyclic monoterpenes and dioxane.

[0039] [3] The production method according to [1], wherein the weight ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:1 (preferably 2:8 to 9:1, more preferably 2:8 to 8:2).

[0040] [4] The production method according to [1] or [3], further comprising the step of obtaining Hansen spheres of the aromatic vinyl compound-based polymer before hydrogenation and Hansen spheres of the aromatic vinyl compound-based polymer after hydrogenation.

[0041] [5] The production method according to any one of [1] to [4], wherein the HSP of the mixed solvent is as follows:

[0042] δd: 15.6~16.7

[0043] δp: 0.3~4.7

[0044] δh: 0.5~5.8.

[0045] [6] The production method according to any one of [1] to [5], wherein the at least one first solvent comprises one or more selected from methyl acetate, ethyl acetate, butyl acetate, methyl isobutyrate, methyl propionate and propylene glycol monomethyl ether acetate, preferably comprises one or more selected from butyl acetate, methyl isobutyrate and methyl propionate.

[0046] [7] The production method according to any one of [1] to [6], wherein the at least one second solvent comprises one or more selected from saturated hydrocarbon solvents and hydrogenated products of monocyclic monoterpenes.

[0047] [8] The production method according to any one of [1] to [7], wherein the at least one second solvent comprises one or more selected from cyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane, C10-C15 tetraalkylcyclohexane, cyclooctane, C9-C15 monoalkylcyclooctane, C10-C15 dialkylcyclooctane, C11-C15 trialkylcyclooctane, C12-C15 tetraalkylcyclooctane, n-octane and n-decane, preferably comprises one or more selected from cyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane and C10-C15 tetraalkylcyclohexane.

[0048] [9] The production method according to any one of [1] to [7], wherein the at least one second solvent comprises C9 alkylcyclohexane and / or C10 alkylcyclohexane.

[0049]

[10] The production method according to any one of [1] to [9], wherein the first solvent has a boiling point of 50° C. or higher and a flash point of 400° C. or higher.

[0050]

[11] The production method according to any one of [1] to

[10] , wherein the second solvent has a boiling point of 80° C. or higher and a flash point of 230° C. or higher.

[0051]

[12] The production method according to any one of [1] to

[11] , wherein the aromatic vinyl compound-based polymer comprises one or more selected from copolymers of styrene and butadiene, copolymers of styrene and isoprene, copolymers of styrene and methyl methacrylate, copolymers of styrene and maleic anhydride, copolymers of styrene and vinyl acetate, and polystyrene.

[0052]

[13] The production method according to any one of [1] to

[12] , comprising the step of forming a polymer resin by devolatilization extrusion after the hydrogenation reaction.

[0053]

[14] The production method according to any one of [1] to

[13] , further comprising a concentration step between the hydrogenation reaction and the devolatilization extrusion.

[0054]

[15] The production method according to any one of [1] to

[14] , wherein the hydrogenation catalyst is a solid catalyst supporting one or more selected from palladium, platinum, ruthenium, rhodium and nickel.

[0055] Effects of the Invention

[0056] According to one embodiment of the present invention, a method for producing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer using a solvent that can well dissolve the polymer before and after hydrogenation is provided. According to a preferred embodiment of the present invention, by using a mixed solvent comprising at least one first solvent and at least one second solvent, the polymer can be maintained in a state of being dissolved in the solvent both before and after hydrogenation, so that a precipitation removal step after hydrogenation is not required, and productivity is improved. In addition, according to another preferred embodiment of the present invention, the polymer can be maintained in a state of being dissolved in the solvent both before and after hydrogenation, so the reaction rate can be increased. DETAILED DESCRIPTION

[0057] The present invention will be described in detail below. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various ways without departing from the gist of the present invention.

[0058] [Method for producing hydrogenated polymer]

[0059] According to a first aspect of the present invention, there is provided a method for producing a hydrogenated polymer, wherein the hydrogenated polymer is produced by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer.

[0060] The production method comprises the steps of carrying out a hydrogenation reaction using the aromatic vinyl compound polymer, a solvent and a hydrogenation catalyst.

[0061] The above-mentioned solvent is a mixed solvent comprising at least one first solvent and at least one second solvent,

[0062] The Hansen Solubility Parameter (HSP) value of the above mixed solvents

[0063] 1) falls into the Hansen sphere in the three-dimensional space consisting of the δd axis, δp axis and δh axis of the aromatic vinyl compound-based polymer before hydrogenation, and

[0064] 2) It falls into the Hansen sphere in the three-dimensional space consisting of the δd axis, δp axis and δh axis of the hydrogenated aromatic vinyl compound-based polymer.

[0065] According to a second aspect of the present invention, there is provided a method for producing a hydrogenated polymer, wherein the hydrogenated polymer is produced by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer.

[0066] The production method comprises the steps of carrying out a hydrogenation reaction using the aromatic vinyl compound polymer, a solvent and a hydrogenation catalyst.

[0067] The above-mentioned solvent is a mixed solvent comprising at least one first solvent and at least one second solvent,

[0068] The Hansen Solubility Parameters (HSP) of the at least one first solvent are as follows,

[0069] δd: 10~20,

[0070] δp: 1~15,

[0071] δh: 1~25,

[0072] The HSP of the at least one second solvent is as follows,

[0073] δd: 10~20,

[0074] δp: greater than 0 and less than 1,

[0075] δh: 0~2,

[0076] The weight ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:1,

[0077] The first solvent is a solvent selected from the group consisting of ester solvents, aromatic solvents, monocyclic monoterpenes and dioxane.

[0078] Specific implementations of the first and second aspects of the present invention are described below. However, unless otherwise stated, the following implementations are applicable to both the first and second aspects.

[0079] <Aromatic vinyl compound polymer>

[0080] The manufacturing method of certain embodiments of the present invention involves manufacturing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer. In this specification, an "aromatic vinyl compound-based polymer" refers to a polymer comprising a unit derived from an aromatic vinyl compound as a structural unit. Therefore, the aromatic vinyl compound-based polymer can be a polymer (homopolymer) formed by units derived from one aromatic vinyl compound, or a copolymer comprising units derived from two or more aromatic vinyl compounds as structural units, or comprising units derived from one or more aromatic vinyl compounds and units derived from one or more compounds other than aromatic vinyl compounds as structural units. The unit derived from an aromatic vinyl compound refers to a unit having a structure in which the C=C double bond of the vinyl group in the aromatic vinyl compound is disconnected due to polymerization.

[0081] (monomer)

[0082] The aromatic vinyl compound polymer used in the manufacturing method of certain embodiments of the present invention is not particularly limited, and examples thereof include polymers using the following compounds as aromatic vinyl compound monomers: styrene; alkyl styrenes such as α-methylstyrene, α-ethylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 1,3-dimethylstyrene, and p-tert-butylstyrene (the number of carbon atoms in the alkyl portion is preferably 1 to 5); p-hydroxystyrene; alkoxystyrenes such as p-methoxystyrene, m-butoxystyrene, and p-butoxystyrene (the number of carbon atoms in the alkoxy portion is preferably 1 to 5); halogenated styrenes such as o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4-dichlorostyrene, and 2,6-dichlorostyrene; vinylnaphthalene and vinylanthracene, etc. These monomers may be used alone or in combination. In a preferred embodiment of the present invention, styrene is used as an aromatic vinyl compound monomer.

[0083] The aromatic vinyl compound-based polymer used in the production method of certain embodiments of the present invention is a polymer using monomers of compounds other than aromatic vinyl compounds in addition to aromatic vinyl compound monomers. Monomers of compounds other than aromatic vinyl compounds include (meth)acrylates, dienes, and acid anhydrides. Examples of the (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate (the number of carbon atoms in the alkyl portion is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5); cycloalkyl (meth)acrylates or cyclic saturated hydrocarbon esters such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate (the number of carbon atoms in the ring of both is preferably 5 to 20, and more preferably 5 to 10); hydroxyalkyl (meth)acrylates such as (2-hydroxyethyl) (meth)acrylate, (2-hydroxypropyl) (meth)acrylate, and (2-hydroxy-2-methylpropyl) (meth)acrylate (the number of carbon atoms in the alkyl portion is preferably 20, and the number of carbon atoms in the alkyl portion is preferably 20); Preferably, the carbon number of the alkyl group is 1 to 20, more preferably 1 to 10, and further preferably 1 to 5); (meth) acrylate alkoxyalkyl esters such as (meth) acrylate (2-methoxyethyl) ester and (meth) acrylate (2-ethoxyethyl) ester (the carbon number of the alkyl group is preferably 1 to 20, more preferably 1 to 10, and further preferably 1 to 5, and the carbon number of the alkoxy group is preferably 1 to 10, more preferably 1 to 5, and further preferably 1 or 2); (meth) acrylate phenyl esters such as (meth) acrylate; (meth) acrylate arylalkyl esters such as (meth) benzyl ester (the carbon number of the aryl group is preferably 6 to 10, and further preferably 1 to 5); (meth) acrylates having a phospholipid structure such as 2-(meth) acryloyloxyethyl phosphorylcholine, etc. One type of (meth) acrylate may be used alone, or two or more types may be used in combination. As the (meth) acrylate, methyl (meth) acrylate is preferred.

[0084] Examples of the diene include 1,2-butadiene, 1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, 1,4-pentadiene, 1,2-hexadiene, 1,3-hexadiene, 1,4-hexadiene, 1,5-hexadiene, 1,3-heptadiene, 1,3-octadiene, 1,3-nonadiene, 1,3-decadiene, isoprene, cyclopentadiene, 1,3-cyclohexadiene, and 1,4-cyclohexadiene. One type of diene may be used alone, or two or more types may be used in combination. As the diene, a conjugated diene such as 1,3-butadiene or isoprene is preferred.

[0085] Examples of the acid anhydride include anhydrides of maleic acid, itaconic acid, citraconic acid, aconitic acid, and the like. Among them, maleic anhydride is preferred.

[0086] The aromatic vinyl compound polymer used in the production method of certain embodiments of the present invention may contain monomer components other than the above as long as the effect of the present invention is not impaired. For example, the monomer components other than the above may be contained in a molar ratio of 0 to 10% or 0 to 5% relative to all monomer components.

[0087] In a preferred embodiment of the present invention, the aromatic vinyl compound-based polymer includes one or more selected from the copolymers of styrene and butadiene (1,2-butadiene, 1,3-butadiene or a combination thereof), copolymers of styrene and isoprene, copolymers of styrene and methyl methacrylate, copolymers of styrene and maleic anhydride, copolymers of styrene and vinyl acetate, and polystyrene. In another preferred embodiment of the present invention, the aromatic vinyl compound-based polymer is a polymer selected from the copolymers of styrene and butadiene (1,2-butadiene, 1,3-butadiene or a combination thereof), copolymers of styrene and isoprene, copolymers of styrene and methyl methacrylate, copolymers of styrene and maleic anhydride, copolymers of styrene and vinyl acetate, and polystyrene. These polymers can be polymerized from each monomer as described later, or commercial products can be used. For example, as polystyrene, "GPPS HF77" produced by PS Japan can be used.

[0088] (Method for producing aromatic vinyl compound-based polymer)

[0089] Aromatic vinyl compound-based polymers can be manufactured by polymerizing various monomers. There is no particular limitation on the method of polymerizing one or more aromatic vinyl compounds or the method of copolymerizing aromatic vinyl compounds with monomers other than aromatic vinyl compound monomers, and known methods such as free radical polymerization, ionic polymerization, and coordination polymerization can be used. In industry, free radical polymerization is preferred because of its simplicity. As free radical polymerization methods, known methods such as bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization can be appropriately selected. For example, as a bulk polymerization method or a solution polymerization method, there is a continuous polymerization method, in which a monomer composition mixed with monomer components, a chain transfer agent, and a polymerization initiator (and a solvent further added during solution polymerization) is continuously supplied to a complete mixing tank and polymerized at 100 to 180°C. Examples of the solvent used in the solution polymerization method include hydrocarbon solvents such as toluene, xylene, cyclohexane, and methylcyclohexane; ester solvents such as ethyl acetate; ketone solvents such as acetone and butanone; ether solvents such as tetrahydrofuran and 1,4-dioxane; and alcohol solvents such as methanol and isopropanol. The reaction mixture after polymerization is taken out from the complete mixing tank and then introduced into a devolatilizing extruder or a vacuum devolatilizing tank to devolatilize the volatile components (monomer components and solvent, etc.), thereby obtaining a polymer of an aromatic vinyl compound or a copolymer of an aromatic vinyl compound and a monomer other than an aromatic vinyl compound monomer (these are also collectively referred to as "aromatic vinyl compound-based polymers").

[0090] In the structural units of the aromatic vinyl compound-based polymer, the molar ratio (A / B) of the structural units of monomers other than the aromatic vinyl compound monomer (A mol) to the structural units derived from the aromatic vinyl compound (B mol) is preferably 0 to 4, more preferably 0 to 3, and even more preferably 0 to 2.

[0091] The weight average molecular weight of the aromatic vinyl compound-based polymer used in certain embodiments of the present invention is preferably 10,000 to 1,000,000, more preferably 50,000 to 700,000, further preferably 100,000 to 500,000, and particularly preferably 130,000 to 250,000. Although polymers less than 10,000 or more than 1,000,000 can also be hydrogenated on the ring by the method of certain embodiments of the present invention, the mechanical strength of the copolymer with a weight average molecular weight within the above range is sufficient to withstand actual use, and the viscosity is moderate and easy to operate, so it is more preferred. Among them, in this specification, the weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent and converted to polystyrene.

[0092] <Hydrogenation>

[0093] In this specification, "hydrogenation of an aromatic vinyl compound polymer" refers to a reaction in which hydrogen is added to the aromatic ring of an aromatic vinyl compound polymer, for example, reduction of a benzene ring to cyclohexane. Such hydrogenation is also referred to as ring hydrogenation or hydrogenation.

[0094] (Solvent)

[0095] The aromatic vinyl compound polymer used in some embodiments of the present invention is dissolved in an appropriate solvent for hydrogenation. As a factor to be considered when selecting a solvent, it is preferred that the polymer (i.e., both the aromatic polymer and the hydrogenated polymer) before and after hydrogenation has good solubility and does not have a hydrogenated site. Moreover, a solvent that reacts quickly is more preferred. This is because the hydrogenation rate is increased, the reaction time is shortened, and damage to the polymer such as molecular weight reduction can be reduced. In addition, in the case of devolatilization of the solvent component after assuming hydrogenation, it is preferred that the ignition point of the solvent is high. As long as the devolatilization extrusion process can be performed, the hydrogenated polymer can be efficiently manufactured, so it is preferred.

[0096] The solvent used in the manufacturing method of certain embodiments of the present invention is a mixed solvent comprising at least one first solvent and at least one second solvent. Here, the first solvent is preferably a solvent with high solubility for the polymer before hydrogenation, and the second solvent is preferably a solvent with high solubility for the polymer after hydrogenation. However, the solubility of a polymer in a solvent is not easy to predict, and mixing these two solvents does not necessarily result in a solvent that can dissolve both polymers before and after the hydrogenation reaction well. In this case, the inventors of the present invention unexpectedly learned that by using a solvent whose Hansen solubility parameter (HSP) value of a mixed solvent 1) falls into the Hansen sphere on the three-dimensional space composed of the δd axis, δp axis and δh axis of the aromatic vinyl compound-based polymer before hydrogenation, and 2) falls into the Hansen sphere on the three-dimensional space composed of the δd axis, δp axis and δh axis of the above-mentioned aromatic vinyl compound-based polymer after hydrogenation, a solvent that can dissolve both polymers before and after the hydrogenation reaction well can be obtained (the first aspect of the invention). In addition, the inventors of the present invention have also learned that by using at least one first solvent having Hansen solubility parameters (HSP) of δd: 10-20, δp: 1-15 and δh: 1-25, at least one second solvent having HSP of δd: 10-20, δp: 0 or more and less than 1, δh: 0-2, the weight ratio of at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9-9:1, and the first solvent is a solvent selected from ester solvents, aromatic solvents, monocyclic monoterpenes and dioxanes, a solvent that can well dissolve both the polymers before and after the hydrogenation reaction can be obtained (the second invention). The Hansen solubility parameters and Hansen spheres will be described in detail later.

[0097] <Hansen Solubility Parameters>

[0098] The SP value (solubility parameter or solubility factor) is a value that characterizes the strength of the intermolecular forces of a molecular group. The closer the SP value is, the easier it is to mix, the easier it is to infiltrate, and the easier it is to bond. In addition to Hildebrand's SP value (δt), there is also Hansen's SP value (HSP value: London dispersion force term δd, dipole force term δp, and hydrogen bond force term δh), which has the following relationship.

[0099] δt 2 =δd 2 +δp 2 +δh 2

[0100] In this specification, the HSP of the solvent and the solute can adopt the data recorded in the dedicated software (HSPiP). For the case not recorded in the database, it can be calculated by the Y-MB method. Among them, in this specification, when it is expressed as "Hansen Solubility Parameter (HSP) value", it refers to the coordinates in the three-dimensional space composed of the δd axis, δp axis and δh axis derived from the above three Hansen Solubility Parameters.

[0101] The HSP of various solvents including the solvent used in the present invention are shown in the following Tables 1 and 2. The "calculated values" listed in the remarks column of the tables are values ​​obtained by the Y-MB method and can be calculated using dedicated software (HSPiP Version 5, 5.2.05).

[0102] [Table 1]

[0103] Table 1: HSP of each solvent

[0104] Solvents δd δp δh Remark Methyl isobutyrate (IBM) 15.6 5.1 6.1 Calculated Value Tetrahydrofuran (THF) 16.8 5.7 8 1,4-Dioxane 17.5 1.8 9 Butyl acetate 15.8 5.1 6.1 Ethyl acetate 15.8 5.3 7.2 Methyl isobutyl ketone (MIBK) 15.3 6.1 4.1 Styrene 18.6 1 4.1 Toluene 18 1.4 2 Meta-Xylene 17.8 1 3.1 D-Limonene 17.2 1.8 4.3 Decalin 17.6 0 0 Dimethylformamide (DMF) 17.4 12.3 22.3 Methanol 14.7 12.3 22.3 Ethylene glycol 17.0 11 26 Methyl tert-butyl ether 14.8 4.3 5 Ethylene glycol dimethyl ether 15.4 6.3 6 Cyclohexane 16.8 0 0.2 Methylcyclohexane 16 0 1 Ethylcyclohexane 16.1 0.1 0.1 n-Butylcyclohexane 16.2 0 0.6 1,3-Dimethylcyclohexane 16.0 0.1 0.1 1,2,4-Trimethylcyclohexane 15.8 0.1 0.1 1,2,3,4-Tetramethylcyclohexane 15.6 0.1 0.1 1,2,4,5-Tetramethylcyclohexane 15.5 0.1 0.1 Calculated Value 1,2,3,5-Tetramethylcyclohexane 15.5 0.1 0.1 Calculated Value

[0105] [Table 2]

[0106] Table 2: HSP of each solvent

[0107] Solvents δd δp δh Remark acetone 15.5 10.4 7 Acetonitrile 15.3 18 6.1 1-Butanol 16 5.7 15.8 γ-Butyrolactone 18 16.6 7.4 Chloroform 17.8 3.1 5.7 Cyclohexanol 17.4 4.1 13.5 Diacetone Alcohol 15.8 8.2 10.8 Diethylene glycol 16.6 12 19 Dimethyl sulfoxide (DMSO) 18.4 16.4 10.2 Ethanol 15.8 8.8 19.4 Methyl Ethyl Ketone (MEK) 16 9 5.1 N-Methyl-2-pyrrolidone 18 12.3 7.2 Dichloromethane 17 7.3 7.1 Ethylene dichloride 18 7.4 4.1 Acetic anhydride 16 11.7 10.2 aniline 20.1 5.8 11.2 Nitrobenzene 20 10.6 3.1 Propylene carbonate 20 18 4.1 Cyclohexanone 17.8 8.4 5.1 Cyclohexylamine 17.2 3.1 11.3 2-Methyl-1,3-dioxolane 17.8 8.4 7.7 Piperidine 17.3 4.5 8.2 Cyclohexene 17.2 1 2

[0108] The HSP of a mixed solvent can be calculated based on the volume average of each solvent. That is, when the δd of a mixed solvent with a volume ratio of solvent A to solvent B of 9:1 is calculated, AB When δd of solvent A and B are set to δd A and δd B According to the calculation formula "δd AB =0.9×δd A +0.1×δd B" Calculated. When the mixing ratio of the mixed solvent is determined, it can be calculated using the mixing ratio. When the mixing ratio is uncertain, the mass ratio of each solvent can be measured by the internal standard method of gas chromatography-mass spectrometry (GC), and then the volume ratio can be obtained based on the specific gravity of each solvent.

[0109] (Hansen sphere)

[0110] A Hansen sphere is a sphere obtained by dissolving a resin in a plurality of solvents (about 10 to 30 solvents) to study the solubility, and plotting the obtained results in a three-dimensional space (Hansen space) consisting of a δd axis, a δp axis, and a δh axis. The Hansen solubility parameter (HSP) value (δTot) of each resin is obtained based on the central coordinates of the Hansen sphere thus obtained. Specifically, a Hansen sphere can be obtained by the method described in the examples of this specification.

[0111] As the solvent for obtaining the Hansen balls of the resin, 10 or more, preferably 12 or more, and more preferably 14 or more solvents selected from acetone, acetonitrile, 1-butanol, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, cyclohexanol, diacetone alcohol, diethylene glycol, DMF, DMSO, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, N-methyl-2-pyrrolidone, dichloromethane, decalin, styrene, dichloroethane, IBM, toluene, m-xylene, acetic anhydride, aniline, nitrobenzene, propylene carbonate, cyclohexanone, cyclohexylamine, 2-methyl-1,3-dioxolane, piperidine, and cyclohexene can be used. In certain embodiments of the present invention, 14 or more solvents including at least acetone, acetonitrile, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, DMF, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, IBM, and toluene can be used. In addition, in certain embodiments of the present invention, 15 solvents including acetone, acetonitrile, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, DMF, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, IBM, toluene and m-xylene can be used to obtain Hansen balls of SBC resin before and after hydrogenation. In addition, in certain embodiments of the present invention, 21 solvents including acetone, acetonitrile, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, cyclohexanol, DMF, DMSO, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, N-methyl-2-pyrrolidone, dichloromethane, decalin, styrene, dichloroethane, IBM and toluene can be used to obtain Hansen balls of PS resin before and after hydrogenation. In certain embodiments of the present invention, 33 solvents including acetone, acetonitrile, 1-butanol, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, cyclohexanol, diacetone alcohol, diethylene glycol, DMF, DMSO, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, N-methyl-2-pyrrolidone, dichloromethane, decalin, styrene, dichloroethane, IBM, toluene, m-xylene, acetic anhydride, aniline, nitrobenzene, propylene carbonate, cyclohexylamine, 2-methyl-1,3-dioxolane, piperidine and cyclohexene can be used to obtain Hansen spheres of SMA resin. In certain embodiments of the present invention, 26 solvents including acetone, acetonitrile, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, cyclohexanol, DMF, DMSO, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, N-methyl-2-pyrrolidone, dichloromethane, decalin, styrene, dichloroethane, IBM, toluene, m-xylene, cyclohexylamine, 2-methyl-1,3-dioxolane, piperidine and cyclohexene can be used to obtain Hansen balls of hydrogenated SMA resin.In certain embodiments of the present invention, 23 solvents including acetone, acetonitrile, 1-butanol, butyl acetate, γ-butyrolactone, chloroform, cyclohexane, diacetone alcohol, DMF, 1,4-dioxane, ethanol, ethyl acetate, MEK, MIBK, N-methyl-2-pyrrolidone, dichloromethane, decalin, dichloroethane, IBM, toluene, m-xylene, nitrobenzene and cyclohexanone, or 24 solvents including styrene can be used to obtain Hansen spheres of MS resin before and after hydrogenation.

[0112] The solubility of various solvents as described above is input into the dedicated software (HSPiP), and the Hansen sphere is gradually formed. Then, the data of about 10 to 30 solvents are input, and the shape of the Hansen sphere is gradually determined. Therefore, the solubility test is performed until the fluctuation of δd, δp, δh and the radius of the Hansen sphere is no longer more than ±0.1, and the results with reproducibility are obtained.

[0113] In certain embodiments of the first aspect of the present invention, by using a solvent whose Hansen Solubility Parameter (HSP) value of a mixed solvent 1) falls into the Hansen sphere of the aromatic vinyl compound-based polymer before hydrogenation on the three-dimensional space consisting of the δd axis, the δp axis and the δh axis, and 2) falls into the Hansen sphere of the aromatic vinyl compound-based polymer after hydrogenation on the three-dimensional space consisting of the δd axis, the δp axis and the δh axis, when the aromatic ring of the aromatic vinyl compound-based polymer is hydrogenated, the state in which the polymer is dissolved in the solvent both before and after hydrogenation is maintained, thereby suppressing the generation of precipitation after hydrogenation and improving productivity. Moreover, since the state in which the polymer is dissolved in the solvent both before and after hydrogenation is maintained, the reaction rate can be increased. Among them, whether the HSP value of a certain solvent falls into the Hansen sphere of the resin can be determined by the method described in the examples.

[0114] If known information about Hansen spheres is available, the known information can be used. Alternatively, the solubility in about 10 to 30 solvents can be input into a dedicated software (HSPiP) to obtain the results, and the hydrogenation reaction is performed on this basis. In certain embodiments of the first aspect of the present invention, the step of obtaining Hansen spheres of an aromatic vinyl compound-based polymer before hydrogenation and Hansen spheres of an aromatic vinyl compound-based polymer after hydrogenation is also included.

[0115] In certain embodiments of the second aspect of the present invention, the Hansen Solubility Parameters (HSP) of the at least one first solvent are respectively as follows,

[0116] δd: 10~20,

[0117] δp: 1~15,

[0118] δh: 1~25,

[0119] The HSP of at least one second solvent is respectively as follows,

[0120] δd: 10~20,

[0121] δp: greater than 0 and less than 1,

[0122] δh: 0~2,

[0123] The weight ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:1,

[0124] The first solvent is a solvent selected from ester solvents, aromatic solvents, monocyclic monoterpenes and dioxane. Thus, when the aromatic ring of the aromatic vinyl compound polymer is hydrogenated, the polymer can be dissolved in the solvent both before and after hydrogenation, thereby suppressing precipitation after hydrogenation and improving productivity. Moreover, since the polymer can be dissolved in the solvent both before and after hydrogenation, the reaction rate can be improved.

[0125] In certain embodiments of the present invention, the Hansen solubility parameters (HSP) of at least one first solvent are δd: 11-19, δp: 2-12, and δh: 2-20, preferably δd: 12-18, δp: 3-10, and δh: 4-15, more preferably δd: 14-17, δp: 4-8, and δh: 5-10. In certain embodiments of the present invention, the Hansen solubility parameters (HSP) of at least one second solvent are δd: 11-19, δp: 0-0.9, and δh: 0-1.5, preferably δd: 12-18, δp: 0-0.6, and δh: 0-1, more preferably δd: 14-18, δp: 0-0.4, and δh: 0-0.8.

[0126] In certain embodiments of the present invention, the weight ratio of at least one first solvent to at least one second solvent (first solvent: second solvent) is 1:9-9:1, preferably 1:9-8:2, 1:9-7:3, 1:9-6:4, 1:9-5:5, 2:8-9:1, 2:8-8:2, 2:8-7:3, 2:8-6:4, 2:8-5:5, 3:7-8:2, 2:8-7:3, 2:8-6:4, 2:8-5:5, 3:7-9:1, 3:7-8:2, 3:7-7:3, 3:7-6:4 or 3:7-5:5. In the case where the aromatic vinyl compound polymer is polystyrene, the first solvent: second solvent is preferably 1:9-5:5. In the case where the aromatic vinyl compound polymer is a copolymer of styrene and methyl methacrylate, the first solvent: second solvent is preferably 3:7-7:3. When the aromatic vinyl compound polymer is a copolymer of styrene and maleic anhydride, the first solvent: second solvent ratio is preferably 3:7 to 9:1. When the aromatic vinyl compound polymer is a copolymer of styrene and butadiene or isoprene, the first solvent: second solvent ratio is preferably 1:9 to 7:3.

[0127] In certain embodiments of the present invention, a mixed solvent having HSPs of δd: 15.6-16.7, δp: 0.3-4.7, and δh: 0.5-5.8, respectively, may be used. In another embodiment of the present invention, a mixed solvent having HSPs of δd: 16.2-16.7, δp: 0.5-2.4, and δh: 0.7-3.0, respectively, may be used. In yet another embodiment of the present invention, a mixed solvent having HSPs of δd: 16.0-16.5, δp: 1.4-3.4, and δh: 1.8-4.2, respectively, may be used. In yet another embodiment of the present invention, a mixed solvent having HSPs of δd: 15.6-16.5, δp: 1.4-4.5, and δh: 1.8-5.4, respectively, may be used. In yet another embodiment of the present invention, a mixed solvent having HSPs of δd: 16.0-16.7, δp: 0.5-3.4, and δh: 0.7-4.2, respectively, may be used.

[0128] In certain embodiments of the present invention, the at least one first solvent comprises one or more selected from methyl acetate, ethyl acetate, butyl acetate, methyl propionate, methyl isobutyrate and propylene glycol monomethyl ether acetate.

[0129] In certain embodiments of the present invention, at least one second solvent comprises one or more selected from saturated hydrocarbon solvents and hydrogenated products of monocyclic monoterpenes. In a preferred embodiment of the present invention, at least one second solvent comprises one or more selected from cyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane, C10-C15 tetraalkylcyclohexane, cyclooctane, C9-C15 monoalkylcyclooctane, C10-C15 dialkylcyclooctane, C11-C15 trialkylcyclooctane, C12-C15 tetraalkylcyclooctane, n-octane and n-decane. In another preferred embodiment of the present invention, at least one second solvent comprises C9 alkylcyclohexane and / or C10 alkylcyclohexane. As a solvent comprising C9 alkylcyclohexane and / or C10 alkylcyclohexane, SWACLEAN150 produced by Maruzen Petrochemical Co., Ltd. can be used, for example.

[0130] In certain embodiments of the present invention, as the first solvent, a solvent having a boiling point of 50°C or more and a flash point of 400°C or more can be used. The flash point is preferably 410°C or more, more preferably 420°C or more, and further preferably 430°C or more. In addition, the upper limit of the boiling point and the upper limit of the flash point are not particularly limited, and preferably, for example, the boiling point is below 150°C and the flash point is below 470°C. By using a solvent having a high boiling point and a flash point, the devolatilization extrusion process can be carried out efficiently. As such a solvent, methyl isobutyrate, ethyl acetate, butyl acetate, and methyl propionate can be cited.

[0131] In certain embodiments of the present invention, the second solvent has a boiling point of 80°C or more and a flash point of 230°C or more. The flash point is preferably 250°C or more, more preferably 280°C or more, and further preferably 300°C or more. In addition, the upper limit of the boiling point and the upper limit of the flash point are not particularly limited, and preferably, for example, the boiling point is below 150°C and the flash point is below 470°C. By using a solvent having a high boiling point and a flash point, the devolatilization extrusion process can be efficiently performed. As such solvents, cyclohexane, cyclopentane, methylcyclohexane, n-heptane, 2,2,4-trimethylpentane, cyclooctane, 1,3-dimethylcyclohexane, ethylcyclohexane, 1,2,4-trimethylcyclohexane, decalin (cis, trans-decalin) and SWACLEAN 150 can be cited. Among them, the approximate value of the flash point of the mixed solvent containing the first solvent and the second solvent can be obtained by the weighted average of the flash point values ​​of each solvent. That is, when a first solvent w1 parts by weight having a flash point x1°C and a second solvent w2 parts by weight having a flash point x2°C are mixed, the flash point x°C of the mixed solvent can be estimated by the following formula.

[0132] x=x1×w1 / (w1+w2)+x2×w2 / (w1+w2)

[0133] (Hydrogenation Catalyst)

[0134] As the active ingredient of the hydrogenation catalyst used in certain embodiments of the present invention, metal elements with contact hydrogenation performance (hereinafter referred to as "specific metal components") can be cited. As specific metal components, for example, nickel, cobalt, iron, ruthenium, rhodium, palladium, platinum, iridium, copper, silver, molybdenum, tungsten, chromium and rhenium can be cited. As long as the specific metal component exhibits hydrogenation performance, it can be either a metallic state or a cationic state. Among these, the hydrogenation performance of the metallic state is usually strong and stable under a reducing environment, so the metallic state is preferred. The specific metal component can be used in a state in which a single one or a combination of two or more is contained in a solid catalyst. In the case of using two or more specific metal components, their combination, mixing ratio and form are not particularly limited, and can be used in the form of a mixture of each metal, or an alloy or an intermetallic compound. In certain embodiments of the present invention, the hydrogenation catalyst is preferably a solid catalyst supported by one or more selected from palladium, platinum, ruthenium, rhodium and nickel, and is particularly preferably a solid catalyst supported by palladium.

[0135] The raw materials of these specific metal components are not particularly limited, and materials used as raw materials when preparing catalysts according to methods known in the prior art can be used. Examples of such raw materials include hydroxides, oxides, fluorides, chlorides, bromides, iodides, sulfates, nitrates, acetates, ammine compounds and carbonyl complexes of various metal elements. These can be used alone or in combination of two or more.

[0136] The hydrogenation catalyst used in certain embodiments of the present invention may also use a specific metal component alone or in combination with a metal that does not have contact hydrogenation performance as a metal component. Examples thereof include: catalysts such as palladium black and platinum black composed of fine metal powders of the specific metal component; and sponge catalysts made by forming an alloy with the specific metal component, aluminum and a small amount of additives, and then leaching all or part of the aluminum.

[0137] In addition, in order to further improve the activity, selectivity and physical properties of the catalyst, compounds of one or more elements selected from lithium, sodium, potassium, rubidium and cesium as alkali metal elements, magnesium, calcium, strontium and barium as alkaline earth metal elements, fluorine, chlorine, bromine and iodine as halogen elements, and mercury, lead, bismuth, tin, tellurium and antimony as auxiliary additive elements (hereinafter referred to as specific additive components) may be added to the catalyst together with the above-mentioned specific metal components.

[0138] The raw materials of these specific additives are not particularly limited, and materials used as raw materials when preparing catalysts by existing known methods can be used. As such raw materials, for example, hydroxides, oxides, fluorides, chlorides, bromides, iodides, sulfates, nitrates, acetates and ammonia compounds of various metal elements can be cited. They can be used alone or in combination of two or more. In addition, there are no particular restrictions on the method of adding the specific additives and the ratio of the specific additives to the specific metal components.

[0139] In the hydrogenation catalyst used in some embodiments of the present invention, non-metallic substances can also be used in combination with specific metal components. As non-metallic substances, mainly include elemental simple substance, carbide, nitride, oxide, hydroxide, sulfate, carbonate and phosphate (hereinafter referred to as "specific non-metallic components"). As its specific example, for example, graphite, diamond, activated carbon, silicon carbide, silicon nitride, aluminum nitride, boron nitride, boron oxide, aluminum oxide (alumina), silicon dioxide (silica), titanium oxide, zirconium oxide, hafnium oxide, lanthanum oxide, cerium oxide, yttrium oxide, niobium oxide, magnesium silicate, calcium silicate, magnesium aluminate, calcium aluminate, zinc oxide, chromium oxide, aluminum silicate, aluminum silicophosphate, aluminum phosphate, boron phosphate, magnesium phosphate, calcium phosphate, strontium phosphate, hydroxyapatite (hydroxy calcium phosphate), apatite chloride, apatite fluoride, calcium sulfate, barium sulfate and barium carbonate can be mentioned. Specific non-metallic components can be used alone or in combination of two or more. When two or more compounds are used in combination, there are no particular restrictions on the combination, mixing ratio, or form, and the compounds may be used in the form of a mixture, a complex, or a complex salt.

[0140] From the perspective of industrial use, it is preferred that the specific non-metallic component can be obtained simply and cheaply. As such a specific non-metallic component, preferably a zirconium compound, an aluminum compound and an apatite compound, more preferably a zirconium compound and an apatite compound. Among them, zirconium oxide and hydroxyapatite (calcium hydroxyphosphate) are particularly preferred. In addition, the above-mentioned specific additives can also be used to modify or ion-exchange some or all of these specific non-metallic components.

[0141] In addition, as the specific non-metallic component, carbides, nitrides, oxides, etc. of specific metal components can also be used. However, once these compounds are exposed to a hydrogen reduction environment, they are partially reduced to metals. Therefore, in this case, part of them is used as the specific metal component and the rest is used as the non-metallic component. As such examples, oxides such as nickel oxide, iron oxide, cobalt oxide, molybdenum oxide, tungsten oxide, and chromium oxide can be cited.

[0142] As the hydrogenation catalyst used in certain embodiments of the present invention, a specific metal component can be used alone, or a specific metal component can be used in combination with a specific non-metal component. Depending on the circumstances, specific additional components other than these can also be included. The method for manufacturing the hydrogenation catalyst used in certain embodiments of the present invention is not particularly limited, and existing known methods can be used. As examples thereof, there can be cited: a method in which a raw material compound of a specific metal component is impregnated on a specific non-metal component (supporting method); a method in which a raw material compound of a specific metal component and a raw material compound of a specific non-metal component are dissolved together in an appropriate solvent and then precipitated simultaneously using an alkaline compound or the like (coprecipitation method); a method in which a raw material compound of a specific metal component and a specific non-metal component are uniformly mixed in an appropriate proportion (mixing method), etc.

[0143] According to the composition of the hydrogenation catalyst or the conditions of the catalyst preparation method, it is also possible to perform a reduction treatment after preparing a specific metal component in a cationic state to form a metallic state. As the reduction method and reducing agent used for this purpose, existing known methods and substances can be used without special limitation. As reducing agents, for example, reducing inorganic gases such as hydrogen, carbon monoxide gas, ammonia, hydrazine, phosphine and silane, low-level oxygen-containing compounds such as methanol, formaldehyde and formic acid, hydrides such as sodium borohydride and lithium aluminum hydride can be cited. By performing a reduction treatment on a specific metal component in a cationic state in the gas phase or liquid phase in the presence of these reducing agents, the specific metal component is converted into a metallic state. The reduction treatment conditions at this time can be set to appropriate conditions according to the type and amount of the specific metal component and the reducing agent. The reduction treatment operation can be performed by using a catalytic reduction device separately before the hydrogenation reduction in the manufacturing method of certain embodiments of the present invention, or it can be performed in the reactor used in the manufacturing method of certain embodiments of the present invention before the start of the reaction or simultaneously with the reaction operation.

[0144] In addition, the metal content and shape of the hydrogenation catalyst used in certain embodiments of the present invention are not particularly limited. The shape can be powdery or a molded product, and the shape and molding method during molding are not particularly limited. For example, spherical products, tablet molded products, and extruded molded products can be appropriately selected and used, and they can be crushed into shapes of appropriate sizes.

[0145] A particularly preferred specific metal component is palladium, and a catalyst using the specific metal component is described in detail below. When the specific metal component is palladium, considering that palladium is a precious metal, from the perspective of economic efficiency, it is preferred that the amount used is small and the palladium can be effectively utilized. Therefore, it is preferred that the palladium is dispersed and supported on a catalyst carrier for use.

[0146] The palladium compound as a raw material of palladium is preferably a palladium compound that can be dissolved in water or an organic solvent. As such a palladium compound, for example, palladium chloride, tetrachloropalladium salt, tetraammine palladium salt, palladium nitrate and palladium acetate can be cited. Among them, palladium chloride is preferred because of its high solubility in water or an organic solvent and its ease of use for industrial purposes. Palladium chloride can be dissolved in a sodium chloride aqueous solution, dilute hydrochloric acid, ammonia water, etc. for use.

[0147] By adding a solution of a palladium compound to a catalyst support or impregnating the catalyst support into a solution of a palladium compound, palladium or a palladium compound is fixed on the catalyst support. The fixing method generally includes adsorption on the support, crystallization by distillation to remove the solvent, precipitation and deposition of reducing substances and / or alkaline substances acting on the palladium compound, and a suitable method can be used as appropriate. The palladium content in the hydrogenation catalyst obtained by this type of method is preferably 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, and further preferably 0.5 to 5% by mass relative to the total amount of the hydrogenation catalyst in terms of metal palladium conversion. Due to the palladium content of more than 0.01% by mass, a more sufficient hydrogenation rate can be obtained, and the conversion rate of the aromatic vinyl compound-based polymer is further improved. On the other hand, when the palladium content is less than 20% by mass, the dispersion efficiency of palladium in the hydrogenation catalyst becomes higher, so palladium can be used more effectively.

[0148] Depending on the conditions of the palladium compound and the catalyst preparation method, palladium is sometimes supported on the carrier in a cationic state rather than in a metallic state. In this case, the supported cationic palladium (for example, in the form of a palladium compound) can also be used after being reduced to metallic palladium. The reduction method and reducing agent used for this purpose can use existing known methods and products without special restrictions. As a reducing agent, for example: reducing inorganic gases such as hydrogen, carbon monoxide gas, ammonia and hydrazine, low-level oxygen-containing compounds such as methanol, formaldehyde and formic acid, hydrocarbon compounds such as ethylene, propylene, benzene and toluene, hydrides such as sodium borohydride and lithium aluminum hydride. By contacting the cationic palladium with the reducing agent in the gas phase or in the liquid phase, it can be easily reduced to metallic palladium. The reduction treatment conditions at this time can be set to appropriate conditions according to the type and amount of the reducing agent. The reduction treatment operation can be performed using a catalytic reduction device separately before the hydrogenation reduction in the manufacturing method of this embodiment, or it can be performed in the reactor used in the manufacturing method of this embodiment before the start of the reaction or simultaneously with the reaction operation.

[0149] As a specific non-metal component used together with a specific metal component, a zirconium compound is one of the preferred components, and a hydrogenation catalyst containing the compound is described in detail below. The zirconium compound used in certain embodiments of the present invention is preferably selected from zirconium oxide, zirconium hydroxide, zirconium carbonate, alkaline earth zirconate, rare earth zirconate and zircon, either alone or in combination of two or more thereof.

[0150] A particularly preferred zirconium compound is zirconium oxide, and its preparation method is not particularly limited. For example, a method in which an aqueous solution of a soluble zirconium salt is decomposed with an alkaline substance to form zirconium hydroxide or zirconium carbonate, and then prepared by thermal decomposition, etc., is a generally known method. The raw material of the zirconium compound at this time is not limited, and examples thereof include zirconium oxychloride, zirconium oxynitrate, zirconium chloride, zirconium sulfate, tetraalkoxy zirconium, zirconium acetate, and zirconium acetylacetonate. They can be used alone or in combination of two or more. In addition, as alkaline substances for decomposition, examples thereof include ammonia, alkylamines, ammonium carbonate, ammonium bicarbonate, sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, potassium bicarbonate, magnesium hydroxide, calcium hydroxide, lanthanum hydroxide, yttrium hydroxide, and cerium hydroxide, and they can be used alone or in combination of two or more.

[0151] When zirconium oxide is used as the specific non-metal component, there are no particular restrictions on its physical properties, shape, etc. In addition, there are no particular restrictions on the purity of zirconium oxide, and zirconium oxide of purity grades ranging from commercially available general-purpose products to high-purity products can be appropriately used.

[0152] When a specific non-metal component represented by a zirconium compound is used as a catalyst carrier, there are no particular restrictions on the shape, particle size, porosity and other physical properties of these carriers, as well as the method of supporting the metal component. The shape, carrier physical properties, supporting method, etc. corresponding to the reaction mode and conditions can be appropriately selected and used.

[0153] (Other reaction conditions)

[0154] During the ring hydrogenation reaction, the concentration of the copolymer (aromatic polymer + ring hydrogenated polymer) in the solution is usually 1 to 50% by weight, preferably 3 to 30% by weight, and more preferably 5 to 25% by weight. By setting the upper limit of the concentration of the copolymer to a value below the specified value, it is possible to avoid handling inconveniences caused by a decrease in reaction rate or an increase in solution viscosity. In addition, from the perspective of productivity and / or economic benefits, it is preferred to set the lower limit of the concentration to a value above the specified value.

[0155] The hydrogenation (hydrogenation) reaction in the manufacturing method of certain embodiments of the present invention is carried out using a raw material liquid in which an aromatic vinyl compound polymer is dissolved in a solvent, but any one of a suspended bed or a fixed bed can be used for reaction, and known methods such as intermittent reaction or continuous flow reaction can also be used. In the case of using a suspended bed for reaction, the carrier particle size is usually in the range of 0.1 to 1000 μm, preferably 1 to 500 μm, more preferably 5 to 200 μm. By setting the particle size to a specified size or more, the catalyst separation after the hydrogenation reaction is easily achieved, and by setting the upper limit of the particle size to below the specified value, the reaction rate can be prevented from decreasing.

[0156] Preferred reaction conditions are a temperature of 60 to 250°C, a hydrogen pressure of 3 to 30 MPa, and a reaction time of 3 to 30 hours. By setting the reaction temperature to a predetermined temperature or higher, the reaction rate is accelerated; by setting the upper limit of the reaction temperature to a predetermined temperature or lower, side reactions such as polymer decomposition and solvent hydrogenation cracking can be suppressed. In addition, although the reaction rate can be accelerated by setting the hydrogen pressure to a predetermined value or higher, from the perspective of economic benefits, the upper limit is preferably about 30 MPa.

[0157] By separating the hydrogenation catalyst and volatile components (solvent, etc.) from the polymer solution after the hydrogenation reaction, a ring-hydrogenated polymer can be obtained. The catalyst can be separated by known techniques such as filtration or centrifugal separation. Considering coloration, the effect on mechanical properties, etc., the residual catalyst metal concentration in the polymer is preferably as small as possible, preferably 10 ppm or less, more preferably 1 ppm or less.

[0158] As a method for separating volatile components such as solvent from the obtained ring hydrogenated polymer solution after catalyst separation to purify the polymer, the following methods can be used: 1) a method of continuously removing the solvent from the polymer solution to form a concentrated solution, and extruding it in a molten state while heating to granulate it (also called devolatilization extrusion method); 2) a method of evaporating the solvent from the polymer solution to obtain a block, and then granulating it; 3) a method of adding a polymer solution to a poor solvent or adding a poor solvent to the polymer solution to precipitate it, and then granulating it; 4) a method of contacting with hot water to obtain a block, and then granulating it, etc. The manufacturing method of a preferred embodiment of the present invention includes a step of forming a polymer resin by devolatilization extrusion after the hydrogenation reaction. Devolatilization extrusion can be carried out, for example, by maintaining or heating the polymerization solution obtained in the polymerization tank to 120°C to 180°C, and introducing it into a devolatilization extruder equipped with a vent in this state to remove volatile components. The manufacturing method of another preferred embodiment of the present invention also includes a concentration step between the hydrogenation reaction and the devolatilization extrusion.

[0159] When performing catalyst separation and volatile component separation, it is preferred to operate in an inert gas or non-oxidizing gas environment. As the inert gas and non-oxidizing gas, hydrogen or nitrogen, helium, argon can be used, but it is preferred to operate in an environment of industrially cheap nitrogen or hydrogen as a reaction gas.

[0160] The hydrogenation rate (ring hydrogenation rate) of the hydrogenated polymer obtained by the method of certain embodiments of the present invention is not particularly limited, but is preferably 95% or more, more preferably 97% or more, and even more preferably 98% or more. As described in the Examples, the hydrogenation rate can be determined by UV spectrometry before and after the hydrogenation reaction.

[0161] The glass transition temperature (Tgm) of the hydrogenated polymer obtained by the method of certain embodiments of the present invention is not particularly limited, but is preferably 70 to 180° C., more preferably 100 to 160° C. In this specification, the glass transition temperature is a value obtained by differential scanning calorimetry (DSC).

[0162] The hydrogenated polymer obtained by the method of certain embodiments of the present invention can be appropriately mixed with additives such as antioxidants, colorants, release agents, surfactants, antibacterial agents, etc. to form an optical material composition. Since the obtained optical material composition has thermoplasticity, it can be used to manufacture precise and cost-effective optical products through various thermoforming processes such as extrusion molding or injection molding, secondary processing molding of sheet molded bodies, etc. As specific uses of optical products, various light guide plates or light guides, display front panels, plastic lens substrates, filters, optical films, lighting covers, lighting signs, etc. can be cited.

[0163] Example

[0164] The present invention will be described in more detail below by way of examples, but the present invention is not particularly limited by the following examples. The evaluation method of the resin is as follows.

[0165] (1) The ring hydrogenation rate is obtained by UV spectrum measurement before and after the hydrogenation reaction. That is, the resin is dissolved in tetrahydrofuran (THF) as a solvent, and the absorption spectrum at 260 nm is measured using a quartz cuvette. The copolymer resin before the ring hydrogenation reaction is used for calibration to calculate the ratio of unhydrogenated aromatic rings. The instrument used for the measurement is a UV-visible spectrophotometer "GENESYS10S" manufactured by Thermo, but it is not particularly limited to this, as long as it is an equivalent device.

[0166] (2) The weight average molecular weight (Mw) was determined by gel permeation chromatography (GPC). A differential refractive index (RI) detector was used as the detector, THF was used as the solvent, and calibration was performed using standard polystyrene. The instrument used for the measurement was a high-speed liquid chromatography system "Elite LaChrom" manufactured by Shimadzu Scientific Co., Ltd., but it is not particularly limited thereto, and any equivalent equipment may be used.

[0167] (3) The glass transition temperature (Tgm) of the resin was determined by differential scanning calorimetry (DSC). The instrument used for the measurement was DSC7020 manufactured by SII (currently Hitachi High-Technologies Corporation), but the instrument is not particularly limited thereto and any equivalent equipment may be used.

[0168] (4) Method for obtaining HSP of mixed solvent

[0169] The HSP of each solvent is obtained from the data included in the dedicated software (HSPiP). The values ​​not included in the software are calculated by the Y-MB method. The HSP of the mixed solvent is obtained based on the volume average of each solvent. That is, when the d component (δd) of the London dispersion force of the mixed solvent with a volume ratio of solvent A to solvent B of 9:1 is obtained, AB ), the δd of solvents A and B are set to δd A and δd B According to the calculation formula "δd AB =0.9×δd A +0.1×δd B "Figure it out.

[0170] (5) Calculation of Hansen Solubility Parameter (HSP) and Hansen Sphere of Resin Before and After Hydrogenation

[0171] The solubility of the resin is studied by dissolving it in a variety of solvents (about 10 to 30 solvents), and the obtained results are plotted on a three-dimensional space (Hansen space) consisting of a δd axis, a δp axis, and a δh axis, thereby obtaining the Hansen sphere of the resin before and after hydrogenation. The Hansen solubility parameter (HSP) value of each resin is obtained based on the central coordinates of the Hansen sphere thus obtained. The specific method is shown in the following preparation example.

[0172] Preparation Example 1 (Hansen Spheres of Polystyrene (PS))

[0173] The solubility of polystyrene (resin 1) (GPPS HF-77 manufactured by PS Japan) with a weight average molecular weight of 200,000 in each of the 21 solvents listed in Table 3 (solvents indicated by "○" in Table 3) was studied. At this time, granular resin 1 was added to each solvent at room temperature so that the concentration of resin 1 relative to each solvent was 10% by weight, and it was determined whether it was dissolved after stirring. The solvents were neither heated nor cooled. The judgment standard adopted the compensation function method, with compensation factors of "complete dissolution" being 1 point, "uniform dispersion" being 2 points, "residual undissolved particles" being 3 points, and "white turbidity / precipitation" being 4 points. When the resin is insoluble, it is scored as 0 points to distinguish it from samples that have dissolved. That is, after distinguishing the insoluble case as 0 points, for samples that have dissolved other than this, the closer to complete dissolution, the smaller the compensation factor.

[0174] The solubility data obtained from these 21 solvents were input into a dedicated software (HSPiP), and the points of the HSP value of each solvent were plotted on the Hansen space to obtain a Hansen sphere including the points of the solvent that dissolved Resin 1. The HSP value of each solvent adopts the value obtained based on the data included in the dedicated software (HSPiP). After the solubility data of the 21 solvents were input, the Hansen sphere no longer changed, so the solubility test was terminated. The center coordinates of the Hansen sphere were used as the HSP value of Resin 1. The radius of the Hansen sphere was also calculated. The results obtained are shown in Table 4.

[0175] Preparation Example 2 (Hansen Spheres of Hydrogenated Polystyrene (PS-H))

[0176] Resin 1 is hydrogenated to obtain hydrogenated polystyrene (resin 2). The hydrogenation is carried out according to the method described in Example 1 described later. The solubility of resin 2 in each of the 21 solvents described in Table 3 (solvents indicated by "○" in Table 3) is studied under the same conditions as in Preparation Example 1. After the solubility data of the 21 solvents are input, the Hansen sphere no longer changes, so the solubility test is terminated. In addition, the HSP value and the radius of the Hansen sphere of resin 2 are calculated under the same conditions as in Preparation Example 1. The results obtained are shown in Table 4.

[0177] Preparation Example 3 (Hansen Spheres of Styrene-Maleic Anhydride Copolymer (SMA) Resin)

[0178] The solubility of a styrene-maleic anhydride copolymer (SMA) resin (resin 3) (XIBOND120 manufactured by POLYSCOPE POLYMERS BV) having a weight average molecular weight of 160,000 in each of the 33 solvents listed in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data for the 33 solvents were input, the Hansen sphere no longer changed, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of Resin 3 were determined under the same conditions as in Preparation Example 1. The results are shown in Table 4. Preparation Example 4 (Hansen sphere of hydrogenated styrene-maleic anhydride copolymer (SMA-H) resin)

[0179] Resin 3 was hydrogenated to obtain a styrene-maleic anhydride copolymer (resin 4). The hydrogenation was carried out according to the method described in Example 1 described later, except that the resin was changed from PS to SMA. The solubility of resin 4 in each of the 26 solvents described in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data of the 26 solvents were input, the Hansen sphere no longer changed, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of resin 4 were calculated under the same conditions as in Preparation Example 1. The results are shown in Table 4.

[0180] Preparation Example 5 (Hansen Spheres of Methyl Methacrylate-Styrene Copolymer (MS200) Resin)

[0181] The solubility of methyl methacrylate-styrene copolymer (MS200) resin (resin 5) (MS200 manufactured by Toyo Styrene Co., Ltd.) having a weight average molecular weight of 220,000 in each of the 24 solvents listed in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data of the 24 solvents were input, the Hansen sphere did not change, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of Resin 5 were obtained under the same conditions as in Preparation Example 1. The obtained results are shown in Table 4.

[0182] Preparation Example 6 (Hansen Spheres of Hydrogenated Methyl Methacrylate-Styrene Copolymer (MS200-H) Resin)

[0183] Resin 5 was hydrogenated to obtain a hydrogenated methyl methacrylate-styrene copolymer (resin 6). The hydrogenation was carried out according to the method described in Example 2 described later, except that the resin was changed from PS to MS200. The solubility of resin 6 in each of the 24 solvents described in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data of the 24 solvents were input, the Hansen sphere no longer changed, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of resin 6 were calculated under the same conditions as in Preparation Example 1. The results obtained are shown in Table 4.

[0184] Preparation Example 7 (Hansen Spheres of Methyl Methacrylate-Styrene Copolymer (MS750) Resin)

[0185] The solubility of methyl methacrylate-styrene copolymer (MS750) resin (resin 7) (MS750 manufactured by Toyo Styrene Co., Ltd.) having a weight average molecular weight of 120,000 in each of the 23 solvents listed in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data of the 23 solvents were input, the Hansen sphere did not change, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of Resin 7 were obtained under the same conditions as in Preparation Example 1. The obtained results are shown in Table 4.

[0186] Preparation Example 8 (Hansen Spheres of Hydrogenated Methyl Methacrylate-Styrene Copolymer (MS750-H) Resin)

[0187] Resin 7 was hydrogenated to obtain a hydrogenated methyl methacrylate-styrene copolymer (resin 8). The hydrogenation was carried out according to the method described in Comparative Example 1 described later, except that the resin was changed from PS to MS750. The solubility of Resin 8 in each of the 23 solvents described in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data of the 23 solvents were input, the Hansen sphere no longer changed, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of Resin 8 were calculated under the same conditions as in Preparation Example 1. The results obtained are shown in Table 4.

[0188] Preparation Example 9 (Hansen Spheres of Styrene-Butadiene Copolymer (SBC) Resin)

[0189] The solubility of a styrene-butadiene copolymer (SBC) resin (resin 9) (CLEAREN 530L manufactured by Denka Co., Ltd.) having a weight average molecular weight of 130,000 in each of the 15 solvents listed in Table 3 (solvents indicated by "○" in Table 3) was investigated under the same conditions as in Preparation Example 1. After the solubility data of the 15 solvents were input, the Hansen sphere did not change, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of Resin 9 were determined under the same conditions as in Preparation Example 1. The obtained results are shown in Table 4.

[0190] Preparation Example 10 (Hansen Spheres of Hydrogenated Styrene-Butadiene Copolymer (SBC-H) Resin)

[0191] Resin 9 was hydrogenated to obtain a hydrogenated styrene-butadiene copolymer (resin 10). The hydrogenation was carried out according to the method described in Example 2 described later, except that the resin was changed from PS to SBC. The solubility of resin 10 in each of the 15 solvents described in Table 3 (solvents indicated by "○" in Table 3) was studied under the same conditions as in Preparation Example 1. After the solubility data of the 15 solvents were input, the Hansen sphere no longer changed, so the solubility test was terminated. In addition, the HSP value and the radius of the Hansen sphere of resin 10 were calculated under the same conditions as in Preparation Example 1. The results obtained are shown in Table 4.

[0192] [Table 3]

[0193] Table 3: Solvents used to determine the HSP values ​​of each resin

[0194] No. PS PS-H SMA SMA-H MS200 MS200-H MS750 MS750-H SBC SBC-H 1 acetone ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 2 Acetonitrile ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 3 1-Butanol ○ ○ ○ ○ ○ 4 Butyl acetate ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 5 γ-Butyrolactone ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 6 Chloroform ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 7 Cyclohexane ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 8 Cyclohexanol ○ ○ ○ ○ 9 Diacetone Alcohol ○ ○ ○ ○ ○ 10 Diethylene glycol ○ 11 DMF ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 12 DMSO ○ ○ ○ ○ 13 1,4-Dioxane ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 14 Ethanol ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 15 Ethyl acetate ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 16 MEK ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 17 MIBK ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 18 N-Methyl-2-pyrrolidone ○ ○ ○ ○ ○ ○ ○ ○ 19 Dichloromethane ○ ○ ○ ○ ○ ○ ○ ○ 20 Decalane ○ ○ ○ ○ ○ ○ ○ ○ 21 Styrene ○ ○ ○ ○ ○ ○ 22 Ethylene dichloride ○ ○ ○ ○ ○ ○ ○ ○ 23 IBM ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 24 Toluene ○ ○ ○ ○ ○ ○ ○ ○ ○ ○ 25 Meta-Xylene ○ ○ ○ ○ ○ ○ ○ ○ 26 Acetic anhydride ○ 27 aniline ○ 28 Nitrobenzene ○ ○ ○ ○ ○ 29 Propylene carbonate ○ 30 Cyclohexanone ○ ○ ○ ○ 31 Cyclohexylamine ○ ○ 32 2-Methyl-1,3-dioxolane ○ ○ 33 Piperidine ○ ○ 34 Cyclohexene ○ ○

[0195] [Table 4]

[0196] Table 4: HSP and HSP value of each resin

[0197] PS PS-H SMA SMA-H MS200 MS200-H MS750 MS750-H SBC SBC-H London dispersion force (δd) 18.7 18.3 18.9 18.0 18.2 18.0 19.04 19.06 20.46 17.26 Inter-dipole force (δp) 7.5 0.5 8.5 2.5 8.4 2.1 3.07 3.30 3.87 1.57 Hydrogen bond (δh) 4.1 0.8 4.6 0.8 5.2 2.5 8.39 8.36 7.99 2.54 HSP value (δTot) 20.6 18.3 21.2 17.6 20.7 18.1 21.0 21.1 22.3 17.8 Hansen sphere radius 8.6 3.6 8.3 4.0 8.1 5.0 9.5 9.3 11.3 3.4

[0198] Preparation Example 11: Preparation of a mixed solvent for dissolving resin before and after hydrogenation

[0199] Methyl isobutyrate (IBM) and cyclohexane (CH) were mixed to prepare 11 levels of solvents and mixed solvents at a weight ratio of IBM:CH of 10:0 to 0:10, and the HSP at each ratio was calculated. The results are shown in Table 5. The HSP at each ratio was obtained based on the volume average value of each solvent. That is, the δd of the mixed solvent having a weight ratio of IBM to CH of 9:1 was calculated based on the specific gravity of each solvent (IBM: 0.89, CH: 0.778) and the volume ratio (10.1:1.3) was calculated, and then calculated using the following calculation formula.

[0200]

[0201] [Table 5]

[0202] Table 5: HSP at various ratios of mixed solvents

[0203] IBM: CH 10∶0 9∶1 8∶2 7∶3 6∶4 5∶5 4∶6 3∶7 2∶8 1∶9 0∶10 δd 15.6 15.7 15.9 16.0 16.1 16.2 16.4 16.5 16.6 16.7 16.8 δp 5.1 4.5 4.0 3.4 2.9 2.4 1.9 1.4 0.9 0.5 0 δh 6.1 5.4 4.8 4.2 3.5 3.0 2.4 1.8 1.3 0.7 0.2

[0204] Whether a certain solvent falls into the Hansen sphere of a certain resin is determined by whether the Hansen solubility parameter (HSP) value of the solvent (the coordinates in the three-dimensional space determined by δd, δp and δh) exists inside the Hansen sphere of the resin. That is, it is determined by whether the Hansen solubility parameter (HSP) value of the solvent exists within the radius of the Hansen sphere from the center coordinate of the Hansen sphere of the resin. The distance between the coordinates in the three-dimensional space determined by δd, δp and δh of a certain solvent and the center coordinates of the Hansen sphere can be calculated by the following formula.

[0205]

[0206] (where δd R Indicates the δd value of the resin, δp R Indicates the δp value of the resin, δh R Indicates the δh value of the resin,

[0207] δd S Indicates the δd value of the solvent, δp S represents the δp value of the solvent, δh S Indicates the δh value of the solvent. )

[0208] When the distance between coordinates obtained by the above formula is less than the radius of the Hansen sphere, it can be said that the Hansen solubility parameter (HSP) value of the solvent (coordinates in the three-dimensional space determined by δd, δp and δh) exists inside the Hansen sphere of the resin. The values ​​of the distance between coordinates in the Hansen space of the mixed solvent of methyl isobutyrate and cyclohexane and each resin obtained using the above formula are shown in the following Table 6. The range surrounded by the black frame in the table is the range where the distance between coordinates in the Hansen space is less than the radius of the Hansen sphere both before and after hydrogenation.

[0209] [Table 6]

[0210] Table 6: Distances between coordinates of mixed solvent of methyl isobutyrate and cyclohexane and each resin in Hansen space

[0211]

[0212] According to the above table, it can be understood that when hydrogenating polystyrene (PS, resin 1), by using a mixed solvent of methyl isobutyrate and cyclohexane with a weight ratio of IBM:CH of 5:5 to 1:9, the reaction can be completed without precipitation of the resin before and after the hydrogenation. Based on this information, the mixed solvent was used for the hydrogenation reaction in the following examples.

[0213] Example 1

[0214] 0.5 parts of polystyrene (resin 1) (GPPS HF-77 manufactured by PS Japan) having a weight average molecular weight of 200,000 was dissolved in 2.75 parts of methyl isobutyrate (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter referred to as IBM) (specific gravity: 0.89, δd: 15.6, δp: 5.1, δh: 6.1), and then the amount of water was reduced from the polymer solution by distillation operation (0.5 parts were removed by azeotropic distillation). 2.25 parts of SWACLEAN 150 (manufactured by Maruzen Petrochemical Co., Ltd., a C9C10 alkylcyclohexane mixture, hereinafter referred to as SWC) (specific gravity: 0.79, δd: 15.6, δp: 0.1, δh: 0.1) were added to the polymer solution after distillation and dehydration to prepare a hydrogenation reaction raw material polymer solution. The HSP of SWC is an inferred value based on the HSP of trimethylcyclohexane and tetramethylcyclohexane. The raw polymer solution and 0.10 parts of 5.0 wt% Pd / ZrO2 were added to a reaction vessel equipped with a stirring device, and a hydrogenation reaction was carried out for 24 hours under the conditions of a hydrogen pressure of 9 MPa and a temperature of 180°C. After the reaction, the hydrogen environment was maintained to filter the catalyst, and IBM / SWC was removed by heating and distillation, and the reaction solution was concentrated until the polymer concentration reached 43 wt%. The concentrated solution was introduced into a devolatilization extruder equipped with a vent under a nitrogen environment to remove the volatile components, and the strands were cut to obtain pellets. The ring hydrogenation rate of the ring hydrogenated polymer was 99.5%, the weight average molecular weight Mw was 140,000, and the Tgm was 136°C.

[0215] Example 2

[0216] 0.5 parts of resin 1 are dissolved in 2.75 parts of IBM, and then the water content is reduced from the polymer solution by distillation (0.5 parts are removed by azeotropic distillation). 2.25 parts of cyclohexane (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter referred to as CH) (specific gravity: 0.78, δd: 16.8, δp: 0, δh: 0.2) are added to the polymer solution after distillation and dehydration to prepare a hydrogenation reaction raw polymer solution. The obtained hydrogenation reaction raw polymer solution is subjected to a hydrogenation reaction for 10 hours under the same conditions as in Example 1. After the hydrogenation reaction, the catalyst is removed from the polymer solution after the hydrogenation reaction by filtration, and then the reaction solution is added dropwise to an excess of isopropanol to precipitate the resin. The obtained resin powder is dried under reduced pressure to obtain a dry resin powder. The obtained resin has a ring hydrogenation rate of 99.7%, a weight average molecular weight of 154,000, and a Tgm of 136°C.

[0217] Example 3

[0218] A raw polymer solution for hydrogenation reaction was prepared in the same manner as in Example 2. A hydrogenation reaction was carried out for 24 hours in the same manner as in Example 1 except that the obtained raw polymer solution was added together with 0.05 parts of 5.0 wt% Pd / ZrO2 into a reaction vessel equipped with a stirring device. The obtained resin had a ring hydrogenation rate of 98.9%, a weight average molecular weight of 153,000, and a Tgm of 136°C.

[0219] Example 4

[0220] 0.5 parts of resin 1 was dissolved in 2.75 parts of butyl acetate (specific gravity: 0.88, δd: 15.8, δp: 5.1, δh: 6.1), and then the water content was reduced by distillation from the polymer solution (0.5 parts by azeotropic distillation). The hydrogenation reaction was carried out for 24 hours under the same conditions as in Example 2 except that 2.25 parts of SWACLEAN 150 were added to the polymer solution after distillation. The obtained resin had a ring hydrogenation rate of 98.8%, a weight average molecular weight of 153,000, and a Tgm of 136°C.

[0221] Example 5

[0222] 0.5 parts of resin 1 was dissolved in 1.85 parts of methyl propionate (specific gravity: 0.92, δd: 15.5, δp: 6.5, δh: 7.7), and then the water content was reduced by distillation from the polymer solution (0.5 parts by azeotropic distillation). The same operation as in Example 4 was performed except that 3.15 parts of SWACLEAN 150 were added to the polymer solution after distillation and dehydration. The obtained resin had a ring hydrogenation rate of 98.9%, a weight average molecular weight of 153,000, and a Tgm of 136°C.

[0223] Example 6

[0224] The hydrogenation reaction was carried out for 24 hours under the same conditions as in Example 2 except that 0.5 parts of resin 1 was replaced by 0.5 parts of resin 3. The obtained resin had a ring hydrogenation rate of 97.8%, a weight average molecular weight of 142,000, and a Tgm of 140°C.

[0225] Example 7

[0226] The same procedure as in Example 6 was carried out except that 0.5 parts of Resin 3 was dissolved in 2.75 parts of butyl acetate. The obtained resin had a ring hydrogenation rate of 97.8%, a weight average molecular weight of 142,000, and a Tgm of 139°C.

[0227] Example 8

[0228] 0.5 parts of resin 5 was dissolved in 4.10 parts of IBM, and then the water content was reduced by distillation from the polymer solution (0.5 parts by azeotropic distillation). The hydrogenation reaction was carried out for 24 hours under the same conditions as in Example 2 except that 0.81 parts of CH were added to the polymer solution after distillation. The obtained resin had a ring hydrogenation rate of 99.7%, a weight average molecular weight of 202,000, and a Tgm of 131°C.

[0229] Example 9

[0230] The hydrogenation reaction was carried out for 24 hours under the same conditions as in Example 2 except that 0.5 parts of resin 1 was replaced by 0.5 parts of resin 9. The obtained resin had a ring hydrogenation rate of 99.8%, a weight average molecular weight of 104,000, and a Tgm of 142°C.

[0231] Example 10

[0232] 0.5 parts of resin 9 was dissolved in 3.65 parts of IBM, and then the water content was reduced by distillation from the polymer solution (0.5 parts by azeotropic distillation). The same operation as in Example 8 was performed except that 1.35 parts of CH were added to the polymer solution after distillation. The obtained resin had a ring hydrogenation rate of 99.7%, a weight average molecular weight of 104,000, and a Tgm of 142°C.

[0233] Embodiment 11

[0234] 0.5 parts of resin 9 were dissolved in 2.75 parts of IBM, and then the water content was reduced from the polymer solution by distillation (0.5 parts were removed by azeotropic distillation). The same method as in Example 1 was used, except that 2.25 parts of CH were added to the polymer solution after distillation and dehydration. After the reaction, the catalyst was removed and concentrated in the same manner as in Example 1, and the concentrated solution was introduced into a devolatilization extruder equipped with a vent under a nitrogen atmosphere to devolatilize the volatile components, and the strands were cut to obtain pellets. The obtained resin had a ring hydrogenation rate of 98.5%, a weight average molecular weight of 104,000, and a Tgm of 142°C.

[0235] Example 12

[0236] 0.5 parts of styrene-maleic anhydride copolymer (SMA) resin (resin 11) having a weight average molecular weight of 140,000 (XIBOND140 manufactured by POLYSCOPE POLYMERS BV, styrene / maleic anhydride molar ratio = 85 / 15) was dissolved in 3.65 parts of butyl acetate, and then the water content was reduced by distillation operation (0.5 parts were removed by azeotropic distillation). A hydrogenation reaction was carried out for 24 hours under the same conditions as in Example 2 except that 1.35 parts of SWACLEAN 150 were added to the polymer solution after distillation and dehydration. The obtained resin had a ring hydrogenation rate of 98.4%, a weight average molecular weight of 120,000, and a Tgm of 149°C. The HSP of resin 11 before hydrogenation was δd: 19.3, δp: 5.2, and δh: 3.5, respectively, and the HSP of resin 11 after hydrogenation was δd: 18.3, δp: 4.4, and δh: 1.6, respectively. The Hansen sphere radius of the resin 11 before hydrogenation was 8.5, and the Hansen sphere radius of the resin 11 after hydrogenation was 4.1.

[0237] Example 13

[0238] 0.5 parts of resin 11 was dissolved in 3.65 parts of butyl acetate, and then the water content was reduced by distillation from the polymer solution (0.5 parts by azeotropic distillation). The same operation as in Example 11 was performed except that 1.35 parts of CH were added to the polymer solution after distillation. The obtained resin had a ring hydrogenation rate of 98.5%, a weight average molecular weight of 120,000, and a Tgm of 149°C.

[0239] Comparative Example 1

[0240] After dissolving 0.5 parts of polystyrene (resin 1) (GPPS HF-77 manufactured by PS Japan) with a weight average molecular weight of 200,000 in 5.0 parts of IBM, the water content was reduced by distillation from the polymer solution (0.5 parts were removed by azeotropic distillation). The obtained hydrogenation reaction raw polymer solution after distillation and dehydration was subjected to hydrogenation reaction under the same conditions as in Example 1. When the inside of the reaction vessel was opened and confirmed after the reaction, the hydrogenated polymer precipitated in the IBM solvent and was difficult to separate from the catalyst. The ring hydrogenation rate of the obtained resin was 97.5%.

[0241] Comparative Example 2

[0242] The hydrogenation reaction was carried out for 16 hours under the same conditions as in Comparative Example 1 except that 0.5 parts of Resin 1 was dissolved in 5.0 parts of CH. When the interior of the reaction vessel was opened after the reaction and checked for safety, the hydrogenated polymer was precipitated in the solvent and was difficult to separate from the catalyst. The ring hydrogenation rate of the obtained resin was 98.3%.

[0243] Comparative Example 3

[0244] The same procedure as in Comparative Example 1 was followed except that 0.5 parts of Resin 3 was dissolved in 5.0 parts of methyl propionate. After the reaction, the interior of the reaction vessel was opened and checked for safety. Hydrogenated polymer was found to be precipitated in the methyl propionate solvent and difficult to separate from the catalyst. The ring hydrogenation rate of the obtained resin was 14.2%.

[0245] Comparative Example 4

[0246] The same procedure as in Comparative Example 1 was followed except that 0.5 parts of Resin 5 was dissolved in 5.0 parts of IBM. After the reaction, the interior of the reaction vessel was opened and checked for safety. Hydrogenated polymer was precipitated in the IBM solvent and was difficult to separate from the catalyst. The ring hydrogenation rate of the obtained resin was 99.6%.

[0247] Comparative Example 5

[0248] The same procedure as in Comparative Example 1 was followed except that 0.5 parts of Resin 11 was dissolved in 5.0 parts of IBM. After the reaction, the interior of the reaction vessel was opened and checked for safety. Hydrogenated polymer was precipitated in the IBM solvent and was difficult to separate from the catalyst. The ring hydrogenation rate of the obtained resin was 93.8%.

[0249] Reference Example 1

[0250] 0.5 parts of polystyrene (resin 1) (GPPS HF-77 manufactured by PS Japan) with a weight average molecular weight of 200,000 was dissolved in 5.0 parts of cyclohexane, and then the water content was reduced by distillation from the polymer solution (0.5 parts were removed by azeotropic distillation). The obtained hydrogenation reaction raw polymer solution after distillation and dehydration was hydrogenated under the same conditions as in Example 1. The ring hydrogenation rate of the obtained resin was 99.7%. However, since only cyclohexane (flashing point: 268°C) was used as a solvent, it was not possible to devolatilize the volatile components using a devolatilization extruder.

[0251] Reference Example 2

[0252] 0.5 parts of resin 3 were dissolved in 5.0 parts of cyclohexane, and then the water content was reduced from the polymer solution by distillation (0.5 parts were distilled out by azeotropic distillation). The obtained hydrogenation reaction raw polymer solution after distillation and dehydration was subjected to a hydrogenation reaction for 63 hours under the same conditions as in Example 1. After removing the catalyst from the polymer solution after the hydrogenation reaction by filtration, the reaction solution was added dropwise to an excess of isopropanol to precipitate the resin. The obtained resin powder was dried under reduced pressure to obtain a dry resin powder. The ring hydrogenation rate of the obtained resin was 98.0%.

[0253] [Table 7]

[0254] Table 7

[0255] unit Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Resin 1 Weight 0.5 0.5 0.5 0.5 0.5 Resin 3 Weight 0.5 0.5 IBM Weight 2.75 2.75 2.75 2.75 Butyl acetate Weight 2.75 2.75 Methyl propionate Weight 1.85 SWC Weight 2.25 2.25 3.15 CH Weight 2.25 2.25 2.25 2.25 catalyst Weight 0.1 0.1 0.05 0.1 0.1 0.1 0.1 Reaction time Hour 24 10 24 24 24 24 24 Reaction temperature ℃ 180 180 180 180 180 180 180 Hydrogenation rate % 99.5 99.7 98.9 98.8 98.9 97.8 97.8 Refining method Devolatilization Extrusion Reprecipitation Reprecipitation Reprecipitation Reprecipitation Reprecipitation Reprecipitation

[0256] Note: 0.5 parts by weight of each of the added IBM, butyl acetate and methyl propionate were distilled out due to azeotropy.

[0257] [Table 8]

[0258] Table 8

[0259] unit Example 8 Example 9 Example 10 Embodiment 11 Example 12 Embodiment 13 Resin 5 Weight 0.5 Resin 9 Weight 0.5 0.5 0.5 Resin 11 Weight 0.5 0.5 IBM Weight 4.10 2.75 3.65 2.75 Butyl acetate Weight 3.65 3.65 SWC Weight 1.35 CH Weight 0.81 2.25 1.35 2.25 1.35 catalyst Weight 0.1 0.1 0.1 0.1 0.1 0.1 Reaction time Hour 24 24 24 24 24 24 Reaction temperature ℃ 180 180 180 180 180 180 Hydrogenation rate % 99.7 99.8 99.7 98.5 98.4 98.5 Refining method Reprecipitation Reprecipitation Reprecipitation Devolatilization Extrusion Reprecipitation Reprecipitation

[0260] Note: 0.5 parts by weight of each of the IBM and butyl acetate added were distilled out due to azeotropy.

[0261] [Table 9]

[0262] Table 9

[0263] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Reference Example 1 Reference Example 2 Resin 1 Weight 0.5 0.5 0.5 Resin 3 Weight 0.5 0.5 Resin 5 Weight 0.5 Resin 11 Weight 0.5 IBM Weight 5.0 5.0 5.0 Methyl propionate Weight 5.0 CH Weight 5.0 5.0 5.0 catalyst Weight 0.1 0.1 0.1 0.1 0.1 0.1 0.1 Reaction time Hour 24 16 24 24 24 24 63 Reaction temperature ℃ 180 180 180 180 180 180 180 Hydrogenation rate % 97.5 98.3 14.2 99.6 93.8 99.7 98.0

[0264] Note: 0.5 parts by weight of the solvent added in the comparative example and the reference example were distilled off due to azeotropy.

Claims

1. A method for producing a hydrogenated polymer, by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer, the production method is characterized in that Including the step of performing a hydrogenation reaction using the aromatic vinyl compound-based polymer, solvent and hydrogenation catalyst, The solvent is a mixed solvent comprising at least one first solvent and at least one second solvent, Hansen solubility parameter (HSP) value of the mixed solvent 1) Fall into Hansen spheres in three-dimensional space composed of δd axis, δp axis and δh axis of the aromatic vinyl compound-based polymer before hydrogenation, and 2) Fall into the Hansen sphere in three-dimensional space composed of the delta d axis, delta p axis and delta h axis of the hydrogenated aromatic vinyl compound polymer.

2. A method for producing a hydrogenated polymer, by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer, the production method is characterized in that Including the step of performing a hydrogenation reaction using the aromatic vinyl compound-based polymer, solvent and hydrogenation catalyst, The solvent is a mixed solvent comprising at least one first solvent and at least one second solvent, The Hansen solubility parameters (HSPs) of the first solvent of the at least one are as follows, δd: 10~20, δp: 1~15, δh: 1~25, The HSPs of the at least one second solvent are as follows, δd: 10~20, δp: greater than 0 and less than 1, δh: 0~2, The weight ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:1, The first solvent is a solvent selected from the group consisting of an ester solvent, an aromatic solvent, a monocyclic monoterpene and a dioxane.

3. The manufacturing method according to claim 1, characterized in that The weight ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:

1.

4. The manufacturing method according to claim 1 or 3, characterized in that The steps of obtaining Hansen spheres of the aromatic vinyl compound-based polymer before hydrogenation and Hansen spheres of the aromatic vinyl compound-based polymer after hydrogenation are also included.

5. The manufacturing method according to any one of claims 1 to 4, characterized in that The HSP of the mixed solvent is as follows: δd: 15.6~16.7 δp: 0.3~4.7 δh: 0.5~5.

8.

6. The manufacturing method according to any one of claims 1 to 5, characterized in that The first solvent of the at least one comprises more than one selected from the group consisting of methyl acetate, ethyl acetate, butyl acetate, methyl isobutyrate, methyl propionate and propylene glycol monomethyl ether acetate.

7. The manufacturing method according to any one of claims 1 to 6, characterized in that The second solvent of the at least one comprises more than one selected from the group consisting of a saturated hydrocarbon solvent and a monocyclic monoterpene.

8. The manufacturing method according to any one of claims 1 to 7, characterized in that The at least one second solvent comprises one or more selected from cyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane, C10-C15 tetraalkylcyclohexane, cyclooctane, C9-C15 monoalkylcyclooctane, C10-C15 dialkylcyclooctane, C11-C15 trialkylcyclooctane, C12-C15 tetraalkylcyclooctane, n-octane and n-decane.

9. The manufacturing method according to any one of claims 1 to 7, characterized in that The second solvent of the at least one comprises C9 alkylcyclohexane and / or C10 alkylcyclohexane.

10. The manufacturing method according to any one of claims 1 to 9, characterized in that The boiling point of the first solvent is above 50°C and the ignition point is above 400°C.

11. The manufacturing method according to any one of claims 1 to 10, characterized in that The boiling point of the second solvent is above 80°C and the ignition point is above 230°C.

12. The manufacturing method according to any one of claims 1 to 11, characterized in that The aromatic vinyl compound-based polymer includes at least one selected from the group consisting of copolymers of styrene and butadiene, copolymers of styrene and isoprene, copolymers of styrene and methyl methacrylate, copolymers of styrene and maleic anhydride, copolymers of styrene and vinyl acetate, and polystyrene.

13. The manufacturing method according to any one of claims 1 to 12, characterized in that The step of extruding the resin forming the polymer by devolatilization after the hydrogenation reaction is included.

14. The manufacturing method according to any one of claims 1 to 13, characterized in that The concentration process is also included between the hydrogenation reaction and the devolatilization extrusion.

15. The manufacturing method according to any one of claims 1 to 14, characterized in that The hydrogenation catalyst is a solid catalyst supported by one or more selected from palladium, platinum, ruthenium, rhodium and nickel.

Citation Information

Patent Citations

  • Hydrogenation method for aromatic polymers

    JP2001527095A

  • Hydrogenation method of aromatic polymers in the presence of branched hydrocarbons

    JP2002511501A