Rubber composition for tires

By using solution polymerized styrene-butadiene rubber with a low glass transition temperature, white filler and thermoplastic resin in the tire rubber composition, combined with a specific silane coupling agent, the problem of high tire rolling resistance in a wide temperature range is solved. Improved wear resistance and wet performance.

CN118829682APending Publication Date: 2024-10-22THE YOKOHAMA RUBBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023108.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-16
Filing Date
2023-03-14
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing rubber compositions for tires cannot effectively reduce rolling resistance in a wider temperature range, and have insufficient wear resistance and wet performance.

Method used

A white filler, a thermoplastic resin, and a specific silane coupling agent are mixed with a diene rubber containing solution-polymerized styrene-butadiene rubber with a glass transition temperature of -50°C or lower to ensure that the glass of the diene rubber and thermoplastic resin The chemical transition temperature difference is below 10°C, resulting in excellent wear resistance and wet performance, and maintaining low rolling resistance in a wide temperature range.

Benefits of technology

A tire rubber composition with low rolling resistance, high wear resistance and excellent wet performance in a wide temperature range has been realized to meet the needs of summer tires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005076550000131
    Figure BDA0005005076550000131
  • Figure BDA0005005076550000141
    Figure BDA0005005076550000141
  • Figure BDA0005005076550000161
    Figure BDA0005005076550000161
Patent Text Reader

Abstract

Provided is a rubber composition for tires, which has excellent wear resistance and wet performance, while having low rolling resistance and temperature dependence thereof. The rubber composition is characterized in that 30 parts by mass or more but less than 100 parts by mass of a white filler and 15 parts by mass or more of a thermoplastic resin are blended with 100 parts by mass of a diene rubber containing 55% by mass or more of a solution-polymerized styrene-butadiene rubber having a glass transition temperature of-50 DEG C or less. A silane coupling agent represented by a specific average composition formula is blended in an amount of 3-20% by mass relative to the mass of the white filler, and a mixture obtained by blending the diene rubber and the thermoplastic resin at a mass ratio of 1: 1, the difference (Tga-Tgm) between a theoretical value (Tga) of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and a measured value (Tgm) of the glass transition temperature of the mixture is 10 DEG C or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rubber composition for a tire that is excellent in wear resistance and wet performance and can obtain good low rolling resistance in a wide temperature range. Background Art

[0002] Summer tires are required to have high levels of wear resistance, wet performance, and low rolling resistance. As a rubber composition for a tire with improved wet performance and low rolling resistance, it is proposed to mix silica and various resin components in modified styrene-butadiene rubber (see, for example, Patent Documents 1 and 2).

[0003] However, in recent years, there is a demand for excellent low rolling resistance in a wider temperature range. Therefore, the inventions described in Patent Documents 1 and 2 are not necessarily sufficient to reduce the temperature dependency of rolling resistance and obtain low rolling resistance in a wider temperature range.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 5376008

[0007] Patent Document 2: Japanese Patent No. 6641300 Summary of the invention

[0008] Problems to be solved by the invention

[0009] An object of the present invention is to provide a rubber composition for a tire which is excellent in wear resistance and wet performance and has low rolling resistance and temperature dependence.

[0010] Means for solving problems

[0011] The tire rubber composition of the present invention for achieving the above-mentioned object is characterized in that 30 parts by mass or more and less than 100 parts by mass of a white filler and 15 parts by mass or more of a thermoplastic resin are mixed with 100 parts by mass of a diene rubber containing 55% by mass or more of a solution-polymerized styrene-butadiene rubber having a glass transition temperature of -50°C or less, and 3 to 20% by mass of a silane coupling agent represented by the average composition formula of the following formula (1) is mixed with the diene rubber and the thermoplastic resin in a mixture obtained by mixing the diene rubber and the thermoplastic resin in a mass ratio of 1:1, and the difference Tga-Tgm between a theoretical value Tga of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and a measured value Tgm of the glass transition temperature of the mixture is 10°C or less.

[0012] (A) a (B)b (C) c (D) d (R 1 ) e SiO (4-2a-b-c-d-e) / 2 (1)

[0013] (In formula (1), A represents a divalent organic group containing a thioether group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, and R 1 It represents a monovalent hydrocarbon group having 1 to 4 carbon atoms, and a to e satisfy the relationship of 0≤a<1, 0<b<1, 0<c<3, 0<d<1, 0≤e<2, 0<2a+b+c+d+e<4. )

[0014] Effects of the Invention

[0015] The tire rubber composition of the present invention has excellent wear resistance and wet performance and can reduce rolling resistance in a wide temperature range because a specific thermoplastic resin, silica and a specific silane coupling agent are mixed with a diene rubber containing a specific solution-polymerized styrene-butadiene rubber.

[0016] The maximum value of the loss tangent tanδ of the tire rubber composition at -40°C to 60°C in the relationship between the tire rubber composition B and a rubber composition having the same composition as the tire rubber composition except that all the thermoplastic resin is replaced by oil is MAXA , and the maximum value of the loss tangent tanδ of the rubber composition B at -40°C to 60°C MAXB The following formula (2) can be satisfied.

[0017] tanδ MAXA / tanδ MAXB > 0.8 (2)

[0018] At least one terminal of the solution-polymerized styrene-butadiene rubber may be modified with a functional group. Furthermore, the amount of oil extension in the solution-polymerized styrene-butadiene rubber may be 10 parts by mass or less relative to 100 parts by mass of the solution-polymerized styrene-butadiene rubber.

[0019] The glass transition temperature of the thermoplastic resin may be 40°C to 120°C, and may be at least one selected from a resin containing at least one selected from terpene, terpene phenol, rosin, rosin ester, C5 component, C9 component, and a resin in which at least a part of the double bonds of these resins are hydrogenated.

[0020] A tire having a tread portion formed from the above-mentioned tire rubber composition is particularly suitable as a summer tire, is excellent in wear resistance and wet performance, and can reduce rolling resistance over a wide temperature range. DETAILED DESCRIPTION

[0021] The rubber component of the tire rubber composition of the present invention is made of diene rubber, and contains 55% by mass or more of solution-polymerized styrene-butadiene rubber having a glass transition temperature (hereinafter sometimes referred to as "Tg") of -50°C or less in 100% by mass of the diene rubber. By containing a solution-polymerized styrene-butadiene rubber having a Tg of -50°C or less, the dispersibility of silica is improved, abrasion resistance and low rolling resistance are ensured, and the temperature dependence of rolling resistance is reduced. The solution-polymerized styrene-butadiene rubber having a Tg of -50°C or less can be 55% by mass or more in 100% by mass of the diene rubber, preferably 55 to 80% by mass, and more preferably 60 to 75% by mass. If the solution-polymerized styrene-butadiene rubber is less than 55% by mass, the effect of improving the dispersibility of silica cannot be fully obtained, and the temperature dependence of rolling resistance cannot be reduced.

[0022] If the Tg of the solution-polymerized styrene-butadiene rubber is higher than -50°C, the temperature dependence of the rolling resistance cannot be reduced. Tg may preferably be -50°C to -65°C, more preferably -50°C to -60°C. The Tg of the solution-polymerized styrene-butadiene rubber can be measured from a thermal analysis diagram obtained by differential scanning calorimetry (DSC) at a heating rate of 20°C / min as the temperature of the midpoint of the transition region. In addition, when the diene rubber is an oil-extended product, it is the Tg of the diene rubber in a state that does not contain the oil-extending component (oil).

[0023] At least one end of the solution-polymerized styrene-butadiene rubber having a Tg of -50°C or less can be modified with a functional group, thereby making the dispersibility of silica good and making the rolling resistance of the tire smaller. Examples of the functional group include epoxy, carboxyl, amino, hydroxyl, alkoxy, silyl, alkoxysilyl, amide, oxysilyl, silanol, isocyanate, isothiocyanate, carbonyl, aldehyde, etc., and preferably a functional group having a polyorganosiloxane structure or an aminosilane structure can be used. By containing a functional group having a polyorganosiloxane structure or an aminosilane structure, the dispersibility of silica can be good, and the wet road performance and low rolling resistance can be excellent.

[0024] The styrene content of the solution polymerized styrene butadiene rubber is not particularly limited, but may be preferably 5 to 30% by mass, more preferably 8 to 25% by mass. By setting the styrene content within such a range, it is preferred that the tire has low rolling resistance. The styrene content of the solution polymerized styrene butadiene rubber may be adjusted by 1 Determined by H-NMR.

[0025] The vinyl content of the solution-polymerized styrene-butadiene rubber is not particularly limited, but can be preferably 9 to 45 mol%, more preferably 20 to 45 mol%, further preferably 25 to 45 mol%, and particularly preferably 28 to 42 mol%. By making the vinyl content within such a range, the dispersibility of silica can be improved, the temperature dependence of rolling resistance can be reduced, and wear resistance can be ensured, which is preferred. Regarding the vinyl content of the solution-polymerized styrene-butadiene rubber, the vinyl content of the solution-polymerized styrene-butadiene rubber can be determined by 1 Determined by H-NMR.

[0026] The solution polymerized styrene butadiene rubber may contain an oil-filled component. The amount of the oil-filled component may be preferably 10 parts by mass or less relative to 100 parts by mass of the solution polymerized styrene butadiene rubber. By making the amount of the oil-filled component 10 parts by mass or less, the reduction in the grip performance of the tire after aging can be suppressed. The amount of the oil-filled component may be more preferably 8 parts by mass or less, and further preferably 5 parts by mass or less.

[0027] The tire rubber composition may contain other diene rubbers other than solution-polymerized styrene-butadiene rubber as its rubber component. As other diene rubbers, for example, solution-polymerized styrene-butadiene rubber, natural rubber, isoprene rubber, butadiene rubber, butyl rubber, emulsion-polymerized styrene-butadiene rubber, halogenated butyl rubber, nitrile rubber, and modified rubbers to which functional groups are added, etc., having a Tg exceeding -50°C, can be exemplified. These other diene rubbers can be used alone or as any admixture. The content of other diene rubbers can be preferably 45% by mass or less, more preferably 20 to 45% by mass, and further preferably 25 to 40% by mass in 100% by mass of the diene rubber.

[0028] It is preferred that the tire rubber composition improves wet road performance by mixing a solution-polymerized styrene-butadiene rubber having a Tg exceeding -50°C. The solution-polymerized styrene-butadiene rubber having a Tg exceeding -50°C may preferably account for 10 to 25% by mass, more preferably 10 to 15% by mass, of 100% by mass of the diene rubber. As the solution-polymerized styrene-butadiene rubber having a Tg exceeding -50°C, substances commonly used in tire rubber compositions may be used.

[0029] The tire rubber composition can reduce the temperature dependence of rolling resistance by mixing natural rubber. The natural rubber may preferably account for 5 to 40% by mass, more preferably 15 to 30% by mass, of 100% by mass of the diene rubber. As the natural rubber, materials commonly used in tire rubber compositions may be used.

[0030] In addition, the abrasion resistance is improved by mixing with butadiene rubber, which is preferred. The butadiene rubber may be preferably 5 to 20% by mass, more preferably 5 to 15% by mass, in 100% by mass of the diene rubber. As the butadiene rubber, those commonly used in tire rubber compositions may be used.

[0031] The tire rubber composition is mixed with 30 parts by mass or more and less than 100 parts by mass of a white filler in 100 parts by mass of a diene rubber. By mixing the white filler, wet road performance and low rolling resistance can be excellent. As a white filler, for example, silicon dioxide, calcium carbonate, magnesium carbonate, talc, clay, aluminum oxide, aluminum hydroxide, titanium oxide, and calcium sulfate can be cited. They can be used alone or in combination of two or more. Among them, silicon dioxide is preferably used, which can make wet road performance and low heat generation more excellent. If the white filler is less than 30 parts by mass, the wet road performance and / or low rolling resistance are insufficient. If the white filler is more than 100 parts by mass, the low rolling resistance is worsened. The white filler can be preferably mixed with more than 40 parts by mass and less than 100 parts by mass, and more preferably mixed with more than 45 parts by mass and less than 100 parts by mass. As silica, those commonly used in tire rubber compositions can be used, for example, wet-process silica, dry-process silica, carbon-silica (two-phase filler) in which silica is supported on the surface of carbon black, silica surface-treated with a compound reactive or compatible with both silica and rubber, such as a silane coupling agent or polysiloxane, etc. Among them, wet-process silica having hydrated silicic acid as a main component is preferred.

[0032] Furthermore, it is preferred that a silane coupling agent represented by the average composition formula (1) below is blended together with silica, because the dispersibility of silica is improved, and wet performance and low rolling resistance are further improved.

[0033] (A) a (B) b (C) c (D) d (R 1 ) e SiO (4-2a-b-c-d-e) / 2 (1)

[0034] (In formula (1), A represents a divalent organic group containing a thioether group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, and R 1 It represents a monovalent hydrocarbon group having 1 to 4 carbon atoms, and a to e satisfy the relationship of 0≤a<1, 0<b<1, 0<c<3, 0<d<1, 0≤e<2, 0<2a+b+c+d+e<4. )

[0035] The silane coupling agent represented by the above formula (1) preferably has a polysiloxane skeleton. The polysiloxane skeleton may be linear, branched, or three-dimensional, or a combination thereof.

[0036] In the above formula (1), the hydrocarbon group B is a monovalent hydrocarbon group having 5 to 10 carbon atoms, preferably a monovalent hydrocarbon group having 6 to 10 carbon atoms, and more preferably a monovalent hydrocarbon group having 8 to 10 carbon atoms. Examples thereof include hexyl, octyl, and decyl. This can protect the mercapto group and prolong the Mooney scorch time, thereby making the processability (scorch resistance) more excellent and making the low rolling resistance more excellent. The subscript b of the hydrocarbon group B can be greater than 0, and preferably 0.10≤b≤0.89.

[0037] In the above formula (1), the organic group A represents a divalent organic group containing a thioether group (hereinafter, also referred to as "the organic group containing a thioether group"). By having the organic group A containing a thioether group, low heat generation and processability (particularly, maintenance / extension of Mooney scorch time) are further improved. Therefore, the subscript a of the organic group A containing a thioether group may be greater than 0, and more preferably 0<a≤0.50. The organic group A containing a thioether group may have a hetero atom such as an oxygen atom, a nitrogen atom, or a sulfur atom.

[0038] Among them, the sulfide group-containing organic group A is preferably a group represented by the following formula (3).

[0039] *-(CH2) n -Sx-(CH2) n -*(3)

[0040] (In the above formula (3), n represents an integer of 1 to 10, x represents an integer of 1 to 6, and * represents a bonding position.)

[0041] Specific examples of the sulfide group-containing organic group A represented by the general formula (3) include *-CH2-S2-CH2-*, *-C2H4-S2-C2H4-*, *-C3H6-S2-C3H6-*, *-C4H8-S2-C4H8-*, *-CH2-S4-CH2-*, *-C2H4-S4-C2H4-*, *-C3H6-S4-C3H6-*, *-C4H8-S4-C4H8-*, etc.

[0042] The silane coupling agent composed of the polysiloxane represented by the average composition formula of the general formula (1) has a hydrolyzable group C, thereby making the affinity and / or reactivity with silica excellent. Based on the reasons that low heat generation, processability (scorch resistance) are better, and the dispersibility of silica is better, the subscript c of the hydrolyzable group C in the general formula (1) can be 1.2≤c≤2.0. As specific examples of the hydrolyzable group C, for example, alkoxy, phenoxy, carboxyl, alkenyloxy, etc. can be mentioned. As the hydrolyzable group C, from the viewpoint of making the dispersibility of silica good and the processability (scorch resistance) better, the group represented by the following general formula (4) is preferred.

[0043] *-OR 2 (4)

[0044] In the above general formula (4), * represents a binding position. 2 It represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 6 to 10 carbon atoms (arylalkyl) or an alkenyl group having 2 to 10 carbon atoms, and among them, an alkyl group having 1 to 5 carbon atoms is preferred.

[0045] Specific examples of the alkyl group having 1 to 20 carbon atoms include, for example, methyl, ethyl, propyl, butyl, hexyl, octyl, decyl, octadecyl, etc. Specific examples of the aryl group having 6 to 10 carbon atoms include, for example, phenyl, tolyl, etc. Specific examples of the aralkyl group having 6 to 10 carbon atoms include, for example, benzyl, phenylethyl, etc. Specific examples of the alkenyl group having 2 to 10 carbon atoms include, for example, ethenyl, propenyl, pentenyl, etc.

[0046] The silane coupling agent composed of the polysiloxane represented by the average composition formula of the general formula (1) can interact and / or react with the diene rubber by having an organic group D containing a mercapto group, thereby making the low heat generation excellent. The subscript d of the organic group D containing a mercapto group can be 0.1≤d≤0.8. As the organic group D containing a mercapto group, from the viewpoint of making the dispersibility of silica good and the processability (scorch resistance) more excellent, it is preferably a group represented by the following general formula (5).

[0047] *-(CH2) m -SH(5)

[0048] In the above general formula (5), m represents an integer of 1 to 10, and preferably an integer of 1 to 5. In the formula, * represents a bonding position.

[0049] Specific examples of the group represented by the general formula (5) include *-CH2SH, *-C2H4SH, *-C3H6SH, *-C4H8SH, *-C5H 10SH, *-C6H 12 SH, *-C7H 14 SH, *-C8H 16 SH, *-C9H 18 SH, *-C 10 H 20 SH.

[0050] In the above general formula (1), R 1 represents a monovalent hydrocarbon group having 1 to 4 carbon atoms. 1 , for example, a methyl group, an ethyl group, a propyl group, and a butyl group can be mentioned.

[0051] The silane coupling agent can be mixed in an amount of 3 to 20% by mass relative to the mass of silica, preferably 5 to 15% by mass. When the amount of the silane coupling agent mixed is less than 3% by mass of the mass of silica, the effect of improving the dispersibility of silica cannot be fully obtained. In addition, if the silane coupling agent exceeds 20% by mass, the diene rubber component tends to gel easily, so the desired effect cannot be obtained.

[0052] The tire rubber composition can be mixed with fillers other than the white filler to increase the strength of the rubber composition and ensure tire durability. Examples of other fillers include inorganic fillers such as carbon black, mica, alumina, and barium sulfate, and organic fillers such as cellulose, lecithin, lignin, and dendritic molecules.

[0053] Among them, by mixing carbon black, the strength of the rubber composition can be excellent. As carbon black, furnace black, acetylene black, thermal black, channel black, graphite and other carbon blacks can be mixed. Among them, furnace black is preferred, and as its specific example, SAF, ISAF, ISAF-HS, ISAF-LS, IISAF-HS, HAF, HAF-HS, HAF-LS, FEF and the like can be cited. These carbon blacks can be used alone or in combination of two or more. In addition, surface-treated carbon blacks in which these carbon blacks are chemically modified with various acid compounds can also be used.

[0054] The tire rubber composition can adjust the temperature dependence of its dynamic viscoelasticity by mixing a specific thermoplastic resin. The specific thermoplastic resin is mixed with 15 parts by mass or more relative to 100 parts by mass of the diene rubber, preferably 20 parts by mass or more, and more preferably 25 parts by mass or more. If the thermoplastic resin is less than 15 parts by mass, the purpose of the present invention of excellent wear resistance and wet road performance and small rolling resistance and temperature dependence cannot be achieved. In addition, the specific thermoplastic resin can be preferably 75 parts by mass or less relative to 100 parts by mass of the diene rubber, and more preferably 60 parts by mass or less. If the specific thermoplastic resin exceeds 75 parts by mass, the wear resistance may be reduced.

[0055] The following relationship is satisfied between a specific thermoplastic resin and a diene rubber. That is, in a mixture obtained by mixing the above-mentioned diene rubber and thermoplastic resin in a mass ratio of 1:1, the difference Tga-Tgm between the theoretical value Tga of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and the measured value Tgm of the glass transition temperature of the mixture is 10°C or less. By making the difference Tga-Tgm below 10°C, the wear resistance and wet road performance are excellent, and the rolling resistance can be made small, and the temperature dependence is small. The difference Tga-Tgm can be preferably below 7°C, and more preferably below 5°C. It can be considered that if the difference Tga-Tgm is below 10°C, the diene rubber and the thermoplastic resin are in a compatible relationship, and by mixing the thermoplastic resin in a relatively large amount, the tensile strength at break of the rubber composition is large, which helps to improve the viscoelastic properties such as tanδ. In this specification, the theoretical value Tga of the glass transition temperature of the mixture can be calculated as a weighted average value from the glass transition temperatures and mass ratios of the diene rubber and the thermoplastic resin. In addition, the glass transition temperatures of the diene rubber and the thermoplastic resin, and the glass transition temperature Tgm of the mixture are measured by measuring a thermogram by differential scanning calorimetry (DSC) at a temperature increase rate of 20°C / min, and are measured as the temperature of the midpoint of the transition region. In addition, when the thermogram has a plurality of transition regions, the midpoint in the largest transition region is set as the glass transition temperature Tgm of the mixture.

[0056] The so-called thermoplastic resin is a resin that is usually mixed with a tire rubber composition, has a molecular weight of about several hundred to several thousand, and has the function of imparting adhesion to the tire rubber composition. As a thermoplastic resin, it is preferably a resin made of at least one selected from a resin containing at least one selected from terpene, modified terpene, rosin, rosin ester, C5 component, C9 component, and a resin obtained by hydrogenating at least a part of the double bonds of these resins. For example, natural resins such as terpene resins, modified terpene resins, rosin resins, and rosin ester resins, synthetic resins such as petroleum resins containing C5 components and C9 components, coal resins, phenolic resins, and xylene resins, and hydrogenated resins obtained by hydrogenating at least a part of the double bonds of these natural resins and synthetic resins.

[0057] Examples of the terpene resin include α-pinene resin, β-pinene resin, limonene resin, hydrogenated limonene resin, dipentene resin, terpene phenol resin, terpene styrene resin, aromatic modified terpene resin, hydrogenated terpene resin, etc. Examples of the rosin resin include gum rosin, tall oil rosin, wood distilled rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, modified rosins such as maleic rosin and fumaric rosin, ester derivatives of these rosins such as glycerol ester, pentaerythritol ester, methyl ester and triethylene glycol ester, and rosin-modified phenolic resins.

[0058] Examples of petroleum-based resins include aromatic hydrocarbon resins or saturated or unsaturated aliphatic hydrocarbon resins, such as C5 petroleum resins (aliphatic petroleum resins obtained by polymerizing fractions such as isoprene, 1,3-pentadiene, cyclopentadiene, methylbutene, and pentene), C9 petroleum resins (aromatic petroleum resins obtained by polymerizing fractions such as α-methylstyrene, o-vinyltoluene, m-vinyltoluene, and p-vinyltoluene), C5C9 copolymer petroleum resins, and resins obtained by hydrogenating these resins.

[0059] The glass transition temperature (Tg) of the thermoplastic resin may be preferably 40°C to 120°C, preferably 45°C to 115°C, and more preferably 50°C to 110°C. It is preferred that the Tg of the thermoplastic resin be 40°C or higher, thereby improving wet road performance. It is also preferred that the Tg be 120°C or lower, thereby improving wear resistance. The Tg of the thermoplastic resin can be measured by the above method.

[0060] In the following description, the tire rubber composition of the present invention is referred to as rubber composition A, and a material having the same composition as rubber composition A except that all the thermoplastic resin contained in rubber composition A is replaced with oil is referred to as rubber composition B. In addition, the maximum value of the loss tangent of rubber composition A at -40°C to 60°C is referred to as tan δ MAXA The maximum value of the loss tangent of the rubber composition B at -40°C to 60°C is defined as tan δ MAXB In this case, tanδ is preferably MAXA and tanδ MAXB The relationship of the following formula (2) is satisfied.

[0061] tanδ MAXA / tanδ MAXB > 0.8 (2)

[0062] If the ratio of the maximum loss tangent to tanδ MAXA / tanδ MAXBWhen the tanδ of the rubber composition for tires of the present invention (rubber composition A) is greater than 0.8, the tensile strength at break of the rubber composition for tires of the present invention (rubber composition A) becomes greater, and the wear resistance of the tires made therefrom is more excellent, which is preferred. Rubber composition B has a tendency to have a high compatibility between the diene rubber and the oil contained therein and a high tensile strength at break. It is estimated that the tanδ of rubber composition A is MAXA is close to tanδ of rubber composition B MAXB When the value of tanδ is greater than tanδ, the viscoelastic behavior of the rubber composition is similar, the compatibility of the diene rubber and the thermoplastic resin is good, and the thermoplastic resin is inhibited from becoming the starting point of destruction, and the tensile strength at break increases. MAXA / tanδ MAXB It may be more preferably greater than 0.85, and even more preferably greater than 0.9. MAXA and tanδ MAXB The dynamic viscoelasticity of the cured products of rubber compositions A and B can be measured using a viscoelasticity spectrometer under the conditions of a tensile strain rate of 10±2%, a frequency of 20 Hz, and a temperature of -40°C to 60°C. A viscoelasticity curve with the measured temperature as the horizontal axis and the loss tangent (tanδ) as the vertical axis is obtained, and the maximum values ​​(peak values) of tanδ are respectively set as tanδ MAXA and tanδ MAXB .

[0063] In the rubber composition for tires, in addition to the above-mentioned components, various compounding agents generally used in rubber compositions for tire treads, such as vulcanization or crosslinking agents, vulcanization accelerators, antioxidants, processing aids, plasticizers, liquid polymers, thermosetting resins, etc., can be mixed according to conventional methods. Such compounding agents can be mixed by a general method to form a rubber composition for vulcanization or crosslinking. The compounding amount of these compounding agents can be the general compounding amount in the past as long as it does not violate the purpose of the present invention. The rubber composition for tires can be prepared by mixing the above-mentioned components using a known rubber mixing machine such as a Banbury mixer, a kneading machine, a roller, etc.

[0064] The tire rubber composition is suitable for forming the tread and sidewall of a summer tire, and is particularly suitable for forming the tread of a summer tire. The summer tire obtained thereby has excellent wear resistance and wet performance, and can reduce rolling resistance and its temperature dependence to a level higher than the conventional level.

[0065] Hereinafter, the present invention will be further described by way of examples, but the scope of the present invention is not limited to these examples.

[0066] Example

[0067] When preparing 21 kinds of rubber compositions for tires (standard examples, examples 1 to 11, comparative examples 1 to 9) having the common additive formula shown in Table 3 and composed of the blends shown in Tables 1 and 2, the components other than sulfur and vulcanization accelerator were weighed respectively, and after mixing for 5 minutes in a 1.7-liter closed Banbury mixer, the masterbatch was released outside the mixer and cooled at room temperature. The masterbatch was supplied to the Banbury mixer, sulfur and vulcanization accelerator were added and mixed, and a rubber composition for tires was obtained. Regarding comparative example 9 in Table 1, SBR-4 is an oil-extended product of 25 parts by mass, so the blending amount without the oil-extending component is recorded in the brackets at the lower level. In addition, the additive formula of Table 3 is recorded in parts by mass relative to 100 parts by mass of the diene rubber recorded in Tables 1 and 2. In addition, the tire rubber compositions of Examples 1 to 11 and Comparative Examples 1 to 9 were respectively designated as rubber composition A, and rubber composition B was designated as a material having the same composition as that of each rubber composition A except that all the thermoplastic resins were replaced with oil, and the same preparation was performed as described above. Furthermore, a mixture was prepared by mixing the diene rubber and the thermoplastic resin constituting the tire rubber composition of each Example and Comparative Example at a mass ratio of 1:1, and the glass transition temperature (Tgm) of the mixture was measured by the above method, and the theoretical value Tga of the glass transition temperature was calculated, and the difference Tga-Tgm from the measured value Tgm of the glass transition temperature was calculated and recorded in Tables 1 and 2.

[0068] The tire rubber compositions obtained above were vulcanized in molds of a predetermined shape at 160° C. for 20 minutes to prepare evaluation samples. The obtained evaluation samples were used to measure dynamic viscoelasticity (loss tangent tan δ), wear resistance, wet performance, rolling resistance, and temperature dependence of rolling resistance by the following methods.

[0069] Dynamic viscoelasticity (loss tangent tanδ)

[0070] The dynamic viscoelasticity of the evaluation samples of the obtained tire rubber composition (rubber composition A) and rubber composition B was measured under the conditions of a tensile strain rate of 10±2%, a frequency of 20 Hz, and a temperature of -40°C to 60°C using a viscoelasticity spectrometer manufactured by Iwamoto Seisakusho Co., Ltd., and a viscoelasticity curve at -40°C to 60°C was prepared, and the maximum value (peak value) of tan δ of the rubber composition A and the rubber composition B was defined as tan δ MAXA and tanδ MAXB , calculate tanδ MAXA / tanδ MAXB The obtained results are recorded in Tables 1 and 2.

[0071] In addition, as an index of wet performance, the measured value of tan δ at 0°C of the tire rubber composition (rubber composition A) is used and recorded in the "Wet Performance" column of Tables 1 and 2 as an index with tan δ at 0°C of the standard example being 100. A larger index means better wet performance.

[0072] Wear resistance

[0073] The evaluation samples of the obtained tire rubber composition were measured for wear amount using a Lamborn wear tester (manufactured by Iwamoto Seisakusho Co., Ltd.) in accordance with JIS K6264 under the conditions of a load of 15.0 kg (147.1 N) and a sliding rate of 25%. The reciprocals of the obtained results were calculated and recorded in the "wear resistance" column of Tables 1 and 2 as an index with the reciprocal of the wear amount of the standard example being 100. The larger the wear resistance index, the better the wear resistance.

[0074] Rolling resistance

[0075] The rubber composition for tires obtained above was used for tread rubber of 17 inches of pneumatic tires by vulcanization molding. Each test tire was assembled on a wheel of standard rim size, mounted on a rolling resistance tester with a drum having a radius of 854 mm, and pre-traveled for 30 minutes under the conditions of air pressure 210 kPa, load 100 N, speed 80 km / h, and drum surface temperature 20°C, and the rolling resistance was measured under the same conditions. Regarding the evaluation results, the reciprocal of the measured value was used as an index with the standard example set to 100 and recorded in the "low rolling resistance" column of Tables 1 and 2. The larger the index value of rolling resistance, the smaller the rolling resistance and the better.

[0076] Temperature dependence of rolling resistance

[0077] Under the same conditions as the measurement conditions of the rolling resistance, the rolling resistance when the surface temperature of the tire was 20°C and the rolling resistance when it was 40°C were evaluated. The measured rolling resistance was plotted against the temperature, and the slope of the difference in rolling resistance at each temperature was evaluated as the temperature dependence of the rolling resistance. Here, the smaller the slope of the rolling resistance, the lower the temperature dependence of the rolling resistance. Regarding the evaluation results, the inverse of the temperature dependence of the rolling resistance (slope) is used as an index with the standard example set to 100 and recorded in the "Temperature Dependence of Low Rolling Resistance" column of Tables 1 and 2. The larger the index value of the temperature dependence of the rolling resistance, the smaller the temperature dependence of the rolling resistance and the better.

[0078]

[0079]

[0080] The types of raw materials used in Tables 1 and 2 are shown below.

[0081] NR: Natural rubber, TSR20, glass transition temperature is -65℃

[0082] SBR-1: a terminal-modified solution-polymerized styrene-butadiene rubber having a polyorganosiloxane structure, Nipol NS612 manufactured by Zeon Co., Ltd., Japan, with a glass transition temperature of -61°C, a styrene content of 15% by mass, a vinyl content of 31% by mole, and a non-oil-extended product.

[0083] SBR-2: a terminal-modified solution-polymerized styrene-butadiene rubber having a polyorganosiloxane structure, Nipol NS616 manufactured by Zeon Co., Ltd., Japan, with a glass transition temperature of -23°C, a styrene content of 22% by mass, a vinyl content of 67 mol%, and a non-oil-extended product.

[0084] SBR-3: a terminal-modified solution-polymerized styrene-butadiene rubber produced by batch polymerization, HPR850 manufactured by JSR Corporation, glass transition temperature -25°C, styrene content 27% by mass, vinyl content 59 mol%, non-oil-extended

[0085] SBR-4: Alkoxysilane-modified solution-polymerized styrene-butadiene rubber produced by continuous polymerization, M2520 manufactured by LG, glass transition temperature -48°C, styrene content 27% by mass, vinyl content 27 mol%, oil-filled content 25 parts by mass

[0086] BR: Butadiene rubber, Nipol BR1220 manufactured by Japan Zeon Co., Ltd., glass transition temperature is -105°C

[0087] ·Carbon black: Tokai Carbon Co., Ltd.'s Seto 7HM

[0088] Silica-1: Zeosil 1165MP manufactured by Solvay, nitrogen adsorption specific surface area: 159 m 2 / g

[0089] Silica-2: ULTRASIL 5000GR manufactured by Evonik, nitrogen adsorption specific surface area: 126 m 2 / g

[0090] · Coupling agent-1: A silane coupling agent containing a polysiloxane represented by the average composition formula of general formula (1), prepared by the production method described in WO2014 / 002750 pamphlet, with an average composition formula of (-C3H6-S4-C3H6-) 0.083 (-C8H 17 ) 0.667 (-OC2H5)1.50 (-C3H6SH) 0.167 SiO 0.75 The polysiloxane shown has an average molecular weight of 860

[0091] · Coupling agent-2: silane coupling agent, Si69 manufactured by Evonik Degussa

[0092] Resin-1: Aromatic modified terpene resin, HSR-7 manufactured by Yashara Chemical Co., Ltd., glass transition temperature: 72°C

[0093] Resin-2: Aromatic modified terpene resin, YS Resin TO-105 manufactured by Yashara Chemical Co., Ltd., glass transition temperature: 57°C

[0094] Resin-3: Indene resin, FMR0150 manufactured by Mitsui Chemicals, Inc., glass transition temperature: 89°C

[0095] Resin-4: Phenol-modified terpene resin, Tamanol 803L manufactured by Arakawa Chemical Industries, Ltd., glass transition temperature: 95°C

[0096] Resin-5: polyterpene resin, Sylvatraxx8115 manufactured by Kraton, glass transition temperature: 67°C

[0097] ・Oil: Sequoia Fluid No. 4 S manufactured by Semantec Co., Ltd.

[0098] [Table 3]

[0099]

[0100] The types of raw materials used in Table 3 are shown below.

[0101] Antiaging agent: VULANOX 4020 manufactured by LANXESS

[0102] Wax: OZOACE-0015A manufactured by NIPPON SEIRO

[0103] ·Sulfur: Tsurumi Chemical Industry Co., Ltd. Sulfux 5

[0104] · Vulcanization accelerator: Noxelara TOT-N manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0105] From Table 2, it was clearly confirmed that the rubber compositions for tires of Examples 1 to 11 were excellent in wear resistance, wet performance, and low rolling resistance, and had low temperature dependence of rolling resistance.

[0106] As is clear from Table 1, the tire rubber composition of Comparative Example 1 has a difference Tga-Tgm exceeding 10° C., and therefore has poor wear resistance, and cannot reduce rolling resistance and its temperature dependency.

[0107] Since the rubber composition for a tire of Comparative Example 2 used a silane coupling agent (coupling agent-2) which could not be represented by the average composition formula of Formula (1), the rolling resistance became large.

[0108] The tire rubber composition of Comparative Example 3 cannot improve wear resistance, rolling resistance and their temperature dependence because the solution-polymerized styrene-butadiene rubber (SBR-1) having a Tg of -50°C or less is less than 55% by mass.

[0109] Since the rubber composition for a tire of Comparative Example 4 contained less than 30 parts by mass of silica, the wear resistance and wet performance could not be improved.

[0110] Since the rubber composition for a tire of Comparative Example 5 contained more than 100 parts by mass of silica, the rolling resistance and its temperature dependence were inferior.

[0111] The tire rubber composition of Comparative Example 6 is inferior in wear resistance, wet performance, low rolling resistance and temperature dependence of rolling resistance because the silane coupling agent (coupling agent-1) represented by the average composition formula (1) is less than 3% by mass of the silica mass.

[0112] The tire rubber composition of Comparative Example 7 had a difference Tga-Tgm exceeding 10° C., and therefore had poor wear resistance, and could not reduce rolling resistance and its temperature dependency.

[0113] The tire rubber composition of Comparative Example 8 was inferior in wear resistance, rolling resistance and temperature dependence thereof because the Tg of the solution-polymerized styrene-butadiene rubber (SBR-3) was higher than -50°C.

[0114] The rubber composition for a tire of Comparative Example 9 was inferior in rolling resistance and its temperature dependency because the Tg of the solution-polymerized styrene-butadiene rubber (SBR-4) was higher than -50°C.

Claims

1. A rubber composition for a tire, characterized in that: In 100 parts by mass of a diene rubber containing 55% by mass or more of a solution-polymerized styrene-butadiene rubber having a glass transition temperature of -50°C or less, 30 parts by mass or more and less than 100 parts by mass of a white filler and 15 parts by mass or more of a thermoplastic resin are mixed, and a silane coupling agent represented by an average composition formula of the following formula (1) is mixed in an amount of 3 to 20% by mass relative to the mass of the white filler, wherein in a mixture obtained by mixing the diene rubber and the thermoplastic resin in a mass ratio of 1:1, a difference Tga-Tgm between a theoretical value Tga of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and a measured value Tgm of the glass transition temperature of the mixture is 10°C or less, (A) a (B) b (C) c (D) d (R 1 ) e SiO (4-2a-b-c-d-e) / 2 (1) In formula (1), A represents a divalent organic group containing a thioether group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, and R 1 It represents a monovalent hydrocarbon group having 1 to 4 carbon atoms, and a to e satisfy the relationship of 0≤a<1, 0<b<1, 0<c<3, 0<d<1, 0≤e<2, 0<2a+b+c+d+e<4.

2. The tire rubber composition according to claim 1, characterized in that In relation to a rubber composition B having the same composition as the tire rubber composition except that all the thermoplastic resin is replaced with oil, the maximum value tanδ of the loss tangent at -40°C to 60°C of the tire rubber composition MAXA , and the maximum value of the loss tangent tanδ of the rubber composition B at -40°C to 60°C MAXB Satisfies the following formula (2): tanδ MAXA / tanδ MAXB > 0.8 (2)。 3. The tire rubber composition according to claim 1 or 2, characterized in that: At least one terminal of the solution-polymerized styrene-butadiene rubber is modified with a functional group.

4. The tire rubber composition according to any one of claims 1 to 3, characterized in that The glass transition temperature of the thermoplastic resin is 40°C to 120°C.

5. The tire rubber composition according to any one of claims 1 to 4, characterized in that The thermoplastic resin is at least one selected from a resin containing at least one selected from terpene, modified terpene, rosin, rosin ester, C5 component, C9 component, and a resin in which at least a part of double bonds of these resins are hydrogenated.

6. The rubber composition for a tire according to any one of claims 1 to 5, characterized in that The amount of oil extension in the solution-polymerized styrene-butadiene rubber is 10 parts by mass or less relative to 100 parts by mass of the solution-polymerized styrene-butadiene rubber. 7 . A tire comprising a tread portion formed from the rubber composition for a tire according to claim 1 .