Method for producing transparent porous film

By controlling the change rate and viscosity of the solid component concentration of the transparent porous film coating, combined with appropriate dispersion media and particles, the problems of reduced transparency and uneven thickness during the spraying process are solved, and excellent transparency and thickness are achieved on optical components. Transparent porous membrane with precise thickness.

CN118829905APending Publication Date: 2024-10-22NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025978.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-23
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing transparent porous films are prone to problems such as reduced transparency or uneven thickness during the spraying process, making it difficult to form a film with excellent transparency and thickness accuracy on optical components.

Method used

By controlling the solid content concentration change rate of the transparent porous coating to be between 1.3 ≤ and 60, the solid content concentration at 10 seconds after spraying is between 3.7 mass% and 6.5 mass%, and the viscosity of the coating film is adjusted to satisfy 0.0549e1 In the range of .2x ≤ to 0.0549e3.3x, use a dispersion medium with a boiling point less than 150°C and silicon compound porous particles to ensure the stability and transparency of the coating film.

Benefits of technology

It achieves excellent transparency and thickness accuracy of the transparent porous film after spraying, suppresses the shaking and void formation on the surface of the coating film, and improves the transparency and thickness uniformity of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031160800000141
    Figure BDA0005031160800000141
Patent Text Reader

Abstract

Provided is a method for producing a transparent porous film with which it is possible to produce a transparent porous film having excellent transparency and excellent thickness accuracy by spray coating. A method for producing a transparent porous film according to an embodiment of the present invention comprises a step for forming a coating film by spraying a transparent porous forming coating material, which contains particles and a dispersion medium in which the particles are dispersed, onto a substrate such that the rate of change in solid content concentration satisfies formula (1). 1.3 < = rate of change in solid content concentration < = 60 (1) (In formula (1), the rate of change in solid content concentration represents the ratio of the solid content concentration in the coating film 10 seconds after spray coating to the solid content concentration in the transparent porous forming coating material before spray coating).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a transparent porous film. Background Art

[0002] It is known that a transparent porous film having a refractive index lower than that of the optical component is provided on various optical components to arbitrarily control the optical properties of an optical product containing these optical components and the transparent porous film. Such a transparent porous film is manufactured by, for example, applying an organic silica sol coating containing a pulverized product of a gel-like silicon compound and a dispersion medium to a substrate (for example, refer to patent document 1). In the past, from the viewpoint of manufacturing efficiency, such a transparent porous film was manufactured by die coating on a long strip substrate, and was attached to the optical component after being peeled off from the substrate for use. However, in recent years, the use of optical products has been diversified, and research is being conducted on forming a transparent porous film directly on an optical component. Optical components may have various shapes (special shapes, sheets, etc.) corresponding to their uses, so it is ideal to spray the coating on the object to form a transparent porous film. However, if the organic silica sol coating described in patent document 1 is used for spraying, sometimes the transparency of the transparent porous film will decrease, or sometimes the accuracy of the thickness of the transparent porous film will decrease.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-25277 Summary of the invention

[0006] Problems to be solved by the invention

[0007] The present invention has been made to solve the above-mentioned conventional technical problems, and its main object is to provide a method for producing a transparent porous film, which can produce a transparent porous film having excellent transparency and excellent thickness accuracy by spraying.

[0008] Solutions for solving problems

[0009] The method for producing a transparent porous film according to an embodiment of the present invention includes the step of spraying a transparent porous-forming coating material including particles and a dispersion medium in which the particles are dispersed onto a substrate so that the solid content concentration change rate satisfies the following formula (1) to form a coating film.

[0010] 1.3≤Solid content concentration change rate≤60……(1)

[0011] (In the formula (1), the solid content concentration change rate represents the solid content concentration in the coating film at 10 seconds after spraying relative to the solid content concentration in the transparent porous forming coating material before spraying.)

[0012] In one embodiment, the solid content concentration of the transparent porous forming coating before spraying is 0.1 mass % to 6.0 mass %, and the solid content concentration of the coating film 10 seconds after spraying is 3.7 mass % to 6.5 mass %.

[0013] In one embodiment, the viscosity of the coating film at 10 seconds after the spraying satisfies the following formula (2).

[0014] 0.0549e 1.2x ≤Viscosity of the coating at 10 seconds after spraying≤0.0549e 3.3x ……(2)

[0015] (In formula (2), e represents the Napier number; x represents the solid content concentration in the coating film at 10 seconds after spraying.)

[0016] In one embodiment, the dispersion medium includes a first dispersion medium having a boiling point lower than 150°C.

[0017] In one embodiment, the content ratio of the first dispersion medium in the dispersion medium is 30 mass % to 100 mass %.

[0018] In one embodiment, the particles are porous particles of a silicon compound.

[0019] Effects of the Invention

[0020] According to the embodiment of the present invention, a transparent porous film having excellent transparency and excellent thickness accuracy can be manufactured by spray coating. DETAILED DESCRIPTION

[0021] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0022] A. Overview of the method for producing a transparent porous film

[0023] A method for producing a transparent porous film according to one embodiment of the present invention includes spraying a transparent porous coating material containing particles and a dispersion medium in which the particles are dispersed onto a substrate so that the solid content concentration change rate satisfies the following formula (1) to form a coating film.

[0024] 1.3≤Solid content concentration change rate≤60……(1)

[0025] (In the formula (1), the solid content concentration change rate represents the solid content concentration in the coating film at 10 seconds after spraying relative to the solid content concentration in the transparent porous forming coating material before spraying.)

[0026] When the solid content concentration change rate satisfies the above formula (1), the state of the coating formed on the substrate can be stabilized. Therefore, the coating surface can be suppressed from shaking due to the influence of spraying, and the generation of coarse voids in the coating can be suppressed. As a result, the thickness of the transparent porous film can be reduced, and the transparency of the transparent porous film can be improved. The solid content concentration change rate is preferably 1.5 or more and 55 or less.

[0027] The solid content concentration of the transparent porous forming coating material before spraying is, for example, 0.1 mass % or more, preferably 1.0 mass % or more, more preferably 2.0 mass % or more, and for example, 6.0 mass % or less, preferably 3.5 mass % or less.

[0028] The solid content concentration in the coating film at 10 seconds after spraying is the solid content concentration in the coating film at 10 seconds after the spraying of the coating from the nozzle stops, for example, 3.7% by mass or more, preferably 4.5% by mass or more, for example, 6.5% by mass or less. These solid content concentrations can be measured, for example, by spraying the substrate and measuring the mass change before and after drying.

[0029] In one embodiment, the viscosity [mPa·s] of the coating film at 10 seconds after spraying satisfies the following formula (2).

[0030] 0.0549e 1.2x ≤Viscosity of the coating at 10 seconds after spraying≤0.0549e 3.3x ……(2)

[0031] (In formula (2), e represents the Napier number; x represents the solid content concentration in the coating film at 10 seconds after spraying.)

[0032] When the viscosity of the coating film satisfies the above formula (2), both improvement in transparency and reduction in thickness unevenness of the transparent porous film can be sufficiently achieved.

[0033] Hereinafter, the transparent porous forming paint used for spray coating and the spray coating conditions will be specifically described.

[0034] B. Transparent porous coating

[0035] As described above, the transparent porous forming coating material contains particles and a dispersion medium in which the particles are dispersed.

[0036] B-1. Particles

[0037] The particles are made of any material suitable for manufacturing a transparent porous film. As the material constituting the particles, for example, the materials described in International Publication No. 2004 / 113966, Japanese Patent Publication No. 2013-254183, Japanese Patent Publication No. 2012-189802, and Japanese Patent Publication No. 2017-25277 can be used. As the material, there can be two types of inorganic and organic substances.

[0038] Examples of the inorganic substance constituting the particles include silicon compounds containing Si, magnesium compounds containing Mg, aluminum compounds containing Al, titanium compounds containing Ti, zinc compounds containing Zn, and zirconium compounds containing Zr.

[0039] Examples of the organic substance constituting the particles include organic polymers; polymerizable monomers (eg, (meth)acrylic monomers and styrene monomers); and curable resins (eg, (meth)acrylic resins, fluorine-containing resins, and polyurethane resins).

[0040] These materials constituting the particles can be used alone or in combination. Among such materials, inorganic substances are preferred, and silicon compounds are more preferred. Specific examples of silicon compounds include: silicon dioxide compounds; hydrolyzable silanes and their partial hydrolyzates and dehydrated condensates; silicon compounds containing silanol groups; and active silica obtained by contacting silicates with acids and ion exchange resins. Among silicon compounds, silicon compounds containing silanol groups are preferred.

[0041] In an embodiment of the present invention, the shape of the "particles" (for example, the porous particles described later) is not particularly limited, and may be, for example, spherical or other shapes. The particles may take any appropriate shape. Examples of the shape of the particles include: spherical, plate-like, needle-like, string-like, and grape cluster-like. Examples of string-like particles include: particles in which a plurality of particles having a spherical, plate-like, or needle-like shape are connected to form a rosary-like shape, short-fiber particles (for example, short-fiber particles described in Japanese Patent Gazette No. 2001-188104), and combinations thereof. String-like particles may be linear or branched. Examples of grape cluster-like particles include: particles in which a plurality of spherical, plate-like, and needle-like particles are agglomerated to form a grape cluster-like shape. The shape of the particles may be confirmed, for example, by observation using a transmission electron microscope.

[0042] The particles preferably have voids (pores). More preferred examples of the particles include hollow particles (hollow nano-silica / nano hollow sphere particles) and porous particles, and even more preferred examples include porous particles.

[0043] In one embodiment, the particles are porous particles of silicon compounds. According to such a structure, a transparent porous film having desired optical properties can be stably manufactured. The porous particles of silicon compounds are preferably a pulverized body of a gel-like silicon compound obtained by pulverizing a gel-like silicon compound in a medium (typically a hydrophilic medium). The pulverized body will be described in detail later.

[0044] In one embodiment, the volume average particle size of the particles (representatively the pulverized body) is, for example, 0.05 μm or more, preferably 0.10 μm or more, more preferably 0.20 μm or more, and further preferably 0.40 μm or more, for example, 2.00 μm or less, preferably 1.50 μm or less, and more preferably 1.00 μm or less. The volume average particle size represents the particle size deviation of the particles (pulverized material) in the transparent porous forming coating, and can be measured, for example, by a particle size distribution evaluation device such as a dynamic light scattering method and a laser diffraction method, and an electron microscope such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM).

[0045] In one embodiment, in the particle size distribution of particles (representatively pulverized bodies), particles with a particle size of 0.4 μm to 1 μm are, for example, 50% to 99.9% by mass, preferably 80% to 99.8% by mass, more preferably 90% to 99.7% by mass, and particles with a particle size of 1 μm to 2 μm are, for example, 0.1% to 50% by mass, preferably 0.2% to 20% by mass, more preferably 0.3% to 10% by mass. The particle size distribution represents the particle size deviation of the particles (pulverized bodies) in the transparent porous coating, and can be measured, for example, by a particle size distribution evaluation device or an electron microscope.

[0046] The content ratio of such particles can be adjusted in a manner such that the solid content concentration in the transparent porous coating before spraying becomes the above-mentioned range. The content ratio of the particles is, for example, more than 0.1 mass parts, preferably more than 0.5 mass parts, for example, less than 50 mass parts, preferably less than 30 mass parts, relative to 100 mass parts of the dispersion medium.

[0047] The concentration of the particles in the transparent porous forming coating material is, for example, 0.1 mass % or more, preferably 1.0 mass % or more, more preferably 2.0 mass % or more, and for example, 6.0 mass % or less, preferably 3.5 mass % or less.

[0048] B-2. Dispersion medium

[0049] The dispersion medium has any appropriate composition capable of dispersing the above particles. The dispersion medium typically includes a first dispersion medium having a boiling point of less than 150° C. The boiling point of the first dispersion medium is a boiling point at one atmospheric pressure, preferably 130° C. or less, more preferably 110° C. or less, for example 80° C. or more, preferably 90° C. or more.

[0050] As the first dispersion medium, for example, alcohols such as ethanol, isopropanol, butanol, tert-butyl alcohol, isobutyl alcohol, and 2-methoxyethanol (methyl cellosolve) can be listed; esters such as ethyl acetate and butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; and aromatic hydrocarbons such as toluene. These first dispersion media can be used alone or in combination. Among these first dispersion media, alcohols are more preferably listed, and isobutyl alcohol is further preferably listed.

[0051] The content ratio of the first dispersion medium in the dispersion medium is, for example, 5% by mass or more, preferably 30% by mass or more, more preferably 40% by mass or more, for example, 100% by mass or less, preferably 95% by mass or less, more preferably 60% by mass or less. If the content ratio of the first dispersion medium is within the above range, the viscosity of the transparent porous coating can be stably adjusted to a range suitable for spraying.

[0052] The dispersion medium may be composed of only the first dispersion medium, or may contain a second dispersion medium in addition to the first dispersion medium. In one embodiment, the dispersion medium further contains a second dispersion medium having a boiling point of 150° C. or more in addition to the first dispersion medium described above. The boiling point of the second dispersion medium is preferably 155° C. or more, more preferably 165° C. or more, for example, 200° C. or less, preferably 190° C. or less.

[0053] Examples of the second dispersion medium include: dimethyl sulfoxide (DMSO); esters such as ethylene glycol monoethyl ether acetate and ethyl lactate; ethers such as diethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol monomethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol butyl methyl ether, tripropylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol monobutyl ether, ethylene glycol monophenyl ether, triethylene glycol monomethyl ether, diethylene glycol dibutyl ether, triethylene glycol butyl methyl ether, polyethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and polyethylene glycol monomethyl ether.

[0054] These second dispersion media may be used alone or in combination. Among these second dispersion media, preferably esters and ethers are used, and more preferably diethylene glycol ethyl methyl ether is used.

[0055] In one embodiment, the content ratio of the second dispersion medium in the dispersion medium is, for example, 0% by mass or more, preferably 5% by mass or more, more preferably 40% by mass or more, for example, 95% by mass or less, preferably 70% by mass or less, more preferably 60% by mass or less. According to such a structure, the viscosity of the transparent porous coating can be more stably adjusted to a range suitable for spraying, and the transparency of the transparent porous film manufactured by spraying can be further improved.

[0056] C. Method for producing transparent porous coating material

[0057] Next, a method for producing a transparent porous coating is described. The method for producing a transparent porous coating includes the following steps: a step of pulverizing a pulverized object in a hydrophilic medium to prepare a sol solution in which particles are dispersed in the hydrophilic medium; and a step of replacing the hydrophilic medium contained in the sol solution with the above-mentioned dispersion medium and adjusting the concentration of the particles to the above-mentioned range. When the solvent is replaced after the pulverized object is pulverized in this way, the dispersibility of the particles can be maintained.

[0058] In the method, first, a pulverized material as a raw material of the particles is prepared. As a method for preparing the pulverized material, for example, the method described in Japanese Patent Publication No. 2017-25277 can be cited. All the records in the publication are cited as references in this specification. More specifically, a precursor of the material of the above particles (representatively a silicon compound) is gelled in a hydrophilic medium.

[0059] Examples of the hydrophilic medium include isopropyl alcohol (IPA), ethanol, methanol, butanol, acetone, dimethylformamide (DMF), and dimethyl sulfoxide (DMSO), preferably IPA and DMSO. The hydrophilic medium may be used alone or in combination. In addition, the hydrophilic medium may be mixed with water.

[0060] Thus, a pulverized product (typically a gel-like silicon compound) composed of the material of the above-mentioned particles is prepared. The pulverized product (typically a gel-like silicon compound) is aged in a hydrophilic medium at, for example, 20° C. to 50° C. for 10 hours or more.

[0061] Next, the object to be pulverized (representatively a gel-like silicon compound) is pulverized in a hydrophilic medium by any appropriate method. It should be noted that the hydrophilic medium may be a mixed medium mixed with water. The pulverization method is not particularly limited. When the object to be pulverized is a gel-like silicon compound, a high-pressure medium-free pulverization method using a homogenizer is preferably used.

[0062] Thus, a sol solution in which the above-mentioned particles are dispersed in a hydrophilic medium is prepared.

[0063] Next, the hydrophilic medium contained in the sol solution is replaced with the above-mentioned dispersion medium by any appropriate method. The replacement method of the solvent is not particularly limited, and for example, decantation, cross-flow filtration, and dynamic filter can be listed. These replacement methods are preferably implemented multiple times. It should be noted that, as required, the concentration of the particles is adjusted to the above-mentioned range using the above-mentioned dispersion medium. In addition, when the hydrophilic medium is a mixed medium mixed with water, the hydrophilic medium can be replaced with the above-mentioned dispersion medium after replacing the mixed medium with a hydrophilic medium (representatively, alcohols with a carbon number of less than 3).

[0064] In the above manner, a transparent porous coating material containing the above particles and the above dispersion medium is produced.

[0065] D.Spraying

[0066] The transparent porous coating material can be preferably sprayed. In the spraying, the transparent porous coating material is sprayed onto a substrate (typically an optical component such as an optical film) as an object to form a coating film on the substrate. The shape of the substrate is not particularly limited. As the shape observed from the thickness direction of the substrate, for example, polygons such as rectangles; circles; ellipses; irregular shapes with concave and / or convex portions can be listed. In addition, the surface shape of the substrate is not particularly limited.

[0067] During spraying, as described above, the substrate is sprayed so that the solid content concentration change rate in the transparent porous forming coating material satisfies the above formula (1). In addition, it is preferred that the viscosity [mPa·s] of the coating film at 10 seconds after spraying satisfies the above formula (2).

[0068] The viscosity of the coating film at 10 seconds after spraying is specifically 30 mPa·s or more, preferably 100 mPa·s or more, more preferably 300 mPa·s or more, further preferably 400 mPa·s or more, particularly preferably 500 mPa·s or more, for example, 4500 mPa·s or less, preferably 3000 mPa·s or less, more preferably 1000 mPa·s or less, particularly preferably 700 mPa·s or less. If the viscosity of the coating film is within the above range, the transparency and thickness accuracy of the transparent porous film can be further improved.

[0069] The viscosity of the transparent porous forming coating before spraying is, for example, 0.1 mPa·s or more, preferably 1.0 mPa·s or more, and for example, 2000 mPa·s or less, preferably 200 mPa·s or less. These viscosities can be calculated using a rheometer manufactured by Anton-Paar.

[0070] During spraying, the distance (coating distance) between the nozzle and the substrate from which the transparent porous coating is sprayed in a mist can be appropriately adjusted. If the distance between the nozzle and the substrate increases, the above-mentioned solid component concentration change rate may increase, and if the distance between the nozzle and the substrate decreases, the above-mentioned solid component concentration change rate may decrease. The distance (coating distance) between the nozzle and the substrate is, for example, more than 50 mm, preferably more than 100 mm, for example, less than 500 mm, preferably less than 300 mm.

[0071] In one embodiment, in the spraying, the nozzle moves in the surface direction of the substrate while spraying the transparent porous forming coating in a mist form. The atomization pressure of the spraying is, for example, 100 kPa to 1000 kPa, the coating amount of the spraying is, for example, 0.1 mL / min to 20 mL / min, and the moving speed of the nozzle during the spraying is, for example, 1 mm / sec to 1000 mm / sec.

[0072] Thus, a coating film is formed on the substrate, and the coating film forms a void structure as a precursor of a porous layer (void layer). It should be noted that the following mainly describes the case where the particles are pulverized products of gel-like compounds. However, in the case where the particles are other than pulverized products of gel-like compounds, a coating film can also be formed in the same manner. In the case where the particles are pulverized products of gel-like compounds, the reasons for forming an appropriate void structure in the coating film are, for example, inferred as follows. However, the inference does not limit the formation method of the transparent porous film.

[0073] The above-mentioned particles (porous particles) are obtained by crushing a gel-like silicon compound, so the three-dimensional structure of the gel-like silicon compound before crushing is in a state of being dispersed into a three-dimensional basic structure. Moreover, in the above-mentioned method, a precursor of a porous structure based on a three-dimensional basic structure is formed by spraying the crushed material of the gel-like silicon compound on a substrate. That is, according to the above-mentioned method, a new porous structure (three-dimensional basic structure) formed by spraying the crushed material, which is different from the three-dimensional structure of the gel-like silicon compound, is formed. Therefore, in the transparent porous film finally obtained, for example, a low refractive index that functions to the same extent as an air layer can be achieved.

[0074] In one embodiment, the method for producing a transparent porous film further comprises a step of heating and drying the coating film on the substrate. The heating temperature is, for example, 60° C. or higher, preferably 70° C. or higher, more preferably 80° C. or higher, for example, 200° C. or lower, preferably 120° C. or lower, more preferably 100° C. or lower. The heating time is not particularly limited as long as the coating film can be fully dried.

[0075] In one embodiment, in the process, a cross-linking reaction occurs between the plurality of particles contained in the coating film, so that the three-dimensional basic structure is fixed. Thus, although the transparent porous film finally obtained has a structure with voids, it can maintain sufficient strength and flexibility.

[0076] In the above manner, a transparent porous film is formed on the substrate.

[0077] E. Transparent porous membrane

[0078] The transparent porous film can be, for example, an open-pore structure in which the pore structure is continuous. The open-pore structure refers to a state in which the pore structure is three-dimensionally connected, or it can be said that the internal voids of the pore structure are continuous. The transparent porous film has an open-pore structure, which can increase the porosity. The transparent porous film more preferably has an overall structure in which the open-pore structure includes a plurality of pores distributed. The overall structure refers to a hierarchical structure, which includes, for example, a structure in which nano-sized fine voids exist and an open-pore structure in which the nano voids are assembled. When the overall structure is formed, for example, the film strength can be imparted by the fine voids, and the high porosity can be imparted by the coarse open-pore voids, taking into account both the film strength and the high porosity.

[0079] The transparent porous membrane may be preferably a nanoporous membrane (specifically, a membrane having 90% or more of the pores having a diameter of 10 - 1 nm~10 3 nm range of transparent porous film).

[0080] The porosity of the transparent porous film is, for example, more than 10% by volume, preferably more than 20% by volume, more preferably more than 30% by volume, more preferably more than 35% by volume, for example, less than 60% by volume, preferably less than 55% by volume, more preferably less than 50% by volume, and more preferably less than 45% by volume. If the porosity is such a range, the refractive index of the transparent porous film can be set to an appropriate range, and the specified mechanical strength can be ensured. The porosity is a value calculated using the Lorentz-Lorenz formula according to the value of the refractive index measured with an ellipsometry spectrometer.

[0081] The size of the void (pore) in the transparent porous film refers to the diameter of the long axis of the void (pore) and the diameter of the short axis. The size of the void (pore) is, for example, 2nm to 500nm. The size of the void (pore) is, for example, more than 2nm, preferably more than 5nm, more preferably more than 10nm, and further preferably more than 20nm. On the other hand, the size of the void (pore) is, for example, less than 500nm, preferably less than 200nm, and more preferably less than 100nm. The range of the size of the void (pore) is, for example, 2nm to 500nm, preferably 5nm to 500nm, more preferably 10nm to 200nm, and further preferably 20nm to 100nm. The size of the void (pore) can be adjusted to the desired size according to the purpose and use.

[0082] The size of the voids (pores) can be quantified by the BET test method. Specifically, 0.1 g of the sample (the void layer formed) is put into the capillary of the specific surface area measuring device (made by Micromeritics: ASAP2020), and then it is dried under reduced pressure at room temperature for 24 hours to degas the gas in the void structure. Then, the adsorption isotherm is drawn by adsorbing nitrogen on the above sample to obtain the pore distribution. In this way, the void size can be evaluated.

[0083] The refractive index of the transparent porous film is, for example, 1.25 or less, preferably less than 1.20, more preferably 1.19 or less, further preferably 1.18 or less, and typically 1.10 or more. Unless otherwise specified, the refractive index refers to the refractive index measured at a wavelength of 550 nm.

[0084] The transparent porous film has excellent transparency. The total light transmittance of the transparent porous film is, for example, 85% to 99%, preferably 87% to 98%, and more preferably 89% to 97%. The haze of the transparent porous film is, for example, less than 5%, preferably less than 3%, and more preferably less than 1%. On the other hand, the haze is, for example, 0.1% or more. The haze can be measured, for example, by the following method.

[0085] The transparent porous film was cut into a size of 50 mm×50 mm and mounted on a haze meter (HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd.) to measure the haze. The haze value was calculated according to the following formula.

[0086] Haze (%) = [diffuse transmittance (%) / total transmittance (%)] × 100 (%)

[0087] The average thickness of the transparent porous film is, for example, 30 nm to 5 μm, preferably 200 nm to 4 μm, more preferably 400 nm to 3 μm, and further preferably 600 nm to 2 μm. If the thickness of the transparent porous film is within this range, the transparent porous film can effectively exhibit a total reflection function for light in the visible to infrared regions.

[0088] The transparent porous film has excellent thickness accuracy. The thickness unevenness of the transparent porous film is, for example, less than ±300 nm, preferably less than ±100 nm, and more preferably less than ±80 nm. The thickness unevenness of the transparent porous film can be measured, for example, by an Optical NanoGauge film thickness meter manufactured by Hamamatsu Photonics.

[0089] Hereinafter, an example of a specific structure of a transparent porous film will be described. The transparent porous film of the present embodiment is composed of one or more structural units forming a fine void structure, and the structural units are chemically bonded to each other through catalysis. As the shape of the structural unit, for example, there can be listed: particle-shaped, fibrous, rod-shaped, and flat-plate-shaped. The structural unit can have only one shape, or it can have a combination of two or more shapes. Hereinafter, the case where the transparent porous film is a porous body formed by chemical bonding of the above-mentioned particles to each other is mainly described.

[0090] Such a transparent porous film can be formed, for example, by chemically bonding particles to each other in the above-mentioned drying process. In one embodiment, the transparent porous film contains a pulverized product of a gel-like compound, and the pulverized products are chemically bonded to each other. The form of the chemical bonding (chemical bond) between the pulverized products in the transparent porous film is not particularly limited, and examples thereof include: cross-linking bonds, covalent bonds, and hydrogen bonds. In the case of using a pulverized product of a gel-like silicon compound, the particles have a three-dimensional tree-like structure, so the tree-like particles settle and accumulate in the coating (a coating of a sol containing the pulverized product of the gel-like silicon compound), thereby easily forming an open-pore structure. In addition, in such a transparent porous film, for example, when the gel-like silicon compound is pulverized, an overall structure can be formed by controlling the particle size distribution of the pulverized particles to a desired size.

[0091] In addition, in the transparent porous film (void layer), for example, the silicon atoms contained therein are preferably siloxane-bonded. As a specific example, the proportion of unbonded silicon atoms (that is, residual silanol) in all silicon atoms contained in the void layer is, for example, less than 50%, preferably less than 30%, and more preferably less than 15%.

[0092] Example

[0093] The present invention will be described in detail below by way of examples, but the present invention is not limited to these examples. It should be noted that the measuring methods of the various properties are as follows. In addition, unless otherwise specified, the "%" and "part" in the examples are by mass.

[0094] (1) Determination of solid content concentration

[0095] In each of the Examples and Comparative Examples, the solid content concentration at the time of coating (solid content concentration in the coating film at 10 seconds after spraying) was calculated by the following formula (3).

[0096] Solid content concentration at the time of coating (mass %) = {(solid content of the coating applied to the substrate) / (total amount of the coating applied to the substrate)} × 100 = {(total mass of the substrate and the coating film after drying - mass of the substrate before coating) / (total mass of the substrate and the coating film 10 seconds after spray coating - mass of the substrate before coating)} × 100 ... (3)

[0097] It should be noted that the mass after drying refers to the mass after the coating film on the substrate is continuously dried at 90° C. until the mass no longer changes due to the volatilization of the solvent.

[0098] (2) Uneven thickness

[0099] In each example and each comparative example, the film thickness of the coating film applied on a 100 mm × 100 mm glass (alkali-free glass) was measured at 10 points in length × 10 points in width at 10 mm intervals, and the standard deviation was taken as the film thickness unevenness. The results are shown in Table 1.

[0100] [Example 1, Example 2 and Comparative Example 1, Comparative Example 2]

[0101] <Preparation of transparent porous coating material>

[0102] (1) Gelation of Silicon Compounds

[0103] 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare a mixed solution A. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution was added to the mixed solution A, and the mixture was stirred at room temperature (23° C.) for 30 minutes to hydrolyze MTMS, thereby generating a mixed solution B containing tri(hydroxy)methylsilane.

[0104] To 5.5 g of DMSO, 0.38 g of 28 mass % ammonia water and 0.2 g of pure water were added, and the mixed solution B was further added, followed by stirring at room temperature (23° C.) for 15 minutes to gel tri(hydroxy)methylsilane, thereby obtaining a mixed solution C containing a gel-like silicon compound.

[0105] (2) Aging treatment

[0106] The mixed solution C containing the gel-like silicon compound prepared as described above was incubated at 40° C. for 20 hours to perform an aging treatment.

[0107] (3) Crushing

[0108] Next, the gel-like silicon compound after the aging treatment as described above was subjected to a pulverization treatment (high-pressure medium-free pulverization). The pulverization treatment (high-pressure medium-free pulverization) was performed using a homogenizer (manufactured by SMT, trade name "UH-50"), and 1.85 g of the gel-like compound in the mixed solution C and 1.15 g of IPA were weighed in a 5 cc screw bottle, and then pulverized for 2 minutes under the conditions of 50 W and 20 kHz.

[0109] By this pulverization treatment, the gel-like silicon compound in the mixed solution C is pulverized, and the mixed solution C becomes a sol solution D of the pulverized product.

[0110] Next, the dispersion medium shown in Table 1 was added to the sol solution D of the pulverized product, and after slight stirring, the solution was left to stand at room temperature (23° C.) for 6 hours to separate the dispersion medium and catalyst in the gel by decantation. The same decantation treatment was repeated three times to perform solvent replacement.

[0111] By the above method, a transparent porous coating was obtained. The concentration of the pulverized material in the coating (particle concentration) is shown in Table 1. The volume average particle size indicating the particle size deviation of the pulverized material contained in the coating was confirmed by a dynamic light scattering NANOTRAC particle size analyzer (manufactured by Nikkiso Co., Ltd., UPA-EX150 model), and the result was 0.50 to 0.70.

[0112] <Spraying>

[0113] Next, the transparent porous forming paint and the alkali-free glass as a substrate were installed in a spray coater (manufactured by Apeiros, product name: API-240 series). Table 1 shows the distance (coating distance) between the spray head (nozzle) and the alkali-free glass.

[0114] Next, a transparent porous coating was sprayed on the alkali-free glass under the following coating conditions to form a coating film on the alkali-free glass. The first step and the second step were repeatedly performed by spraying, wherein the first step was a step of spraying the coating in a mist form while the nozzle moved in the direction X of the first surface of the substrate, and the second step was a step of moving the nozzle in the direction Y of the second surface of the substrate.

[0115] Coating conditions: atomization pressure 100 kPa, coating amount 7 mL / min, nozzle speed in the first step 300 mm / sec, nozzle moving distance in the second step 15 mm.

[0116] Next, the coating film on the alkali-free glass was dried at 90° C. for 10 minutes, and then dried at 70° C. for 24 hours.

[0117] In the above manner, a transparent porous film is formed.

[0118] The average thickness of the transparent porous film was 1.00 μm, and the refractive index of the transparent porous film was 1.18.

[0119] [Table 1]

[0120]

[0121] It should be noted that the details of the abbreviations in the table are as follows.

[0122] IBA: isobutyl alcohol, manufactured by Tokyo Chemical Industry Co., Ltd.

[0123] EDM: diethylene glycol ethyl methyl ether, manufactured by Toho Chemical Industry Co., Ltd.

[0124] As can be seen from Table 1, according to the embodiments of the present invention, when the solid content concentration change rate satisfies the above formula (1), a transparent porous film with low haze and small thickness unevenness can be manufactured by spray coating.

[0125] Industrial Applicability

[0126] The transparent porous film produced by the method for producing a transparent porous film according to the embodiment of the present invention can be applied to various optical products.

Claims

1. A method for producing a transparent porous film, comprising the step of spraying a transparent porous coating material onto a substrate so that the solid content concentration change rate satisfies the following formula (1) to form a coating film, wherein the transparent porous coating material comprises particles and a dispersion medium in which the particles are dispersed. 1.3≤Solid content concentration change rate≤60……(1) In the formula (1), the solid content concentration change rate represents the solid content concentration in the coating film at 10 seconds after spraying relative to the solid content concentration in the transparent porous forming coating material before spraying.

2. The method for producing a transparent porous film according to claim 1, wherein: The solid content concentration of the transparent porous forming paint before spraying is 0.1 mass % to 6.0 mass %, The solid content concentration in the coating film at 10 seconds after the spraying is 3.7% by mass to 6.5% by mass.

3. The method for producing a transparent porous film according to claim 2, wherein: The viscosity of the coating film at 10 seconds after spraying satisfies the following formula (2): 0.0549e 1.2x ≤Viscosity of the coating at 10 seconds after spraying≤0.0549e 3.3x ……(2) In the formula (2), e represents the Napier number; and x represents the solid content concentration in the coating film at 10 seconds after spraying.

4. The method for producing a transparent porous film according to any one of claims 1 to 3, wherein: The dispersion medium includes a first dispersion medium having a boiling point of less than 150°C.

5. The method for producing a transparent porous film according to claim 4, wherein: The content ratio of the first dispersion medium in the dispersion medium is 30 mass % to 100 mass %.

6. The method for producing a transparent porous film according to any one of claims 1 to 5, wherein: The particles are porous particles of a silicon compound.