Method for producing ultra-thick silicon steel with thickness of 1.0 mm or above on continuous annealing coating line
By adjusting the welding, loop tension, cleaning, annealing and cooling steps on the continuous annealing coating line, various technical problems in the production of ultra-thick silicon steel are solved, ensuring high-quality continuous production of silicon steel with a thickness of more than 1.0mm and avoiding run-out Problems such as deviation, tearing, and burning damage are eliminated, which improves production efficiency and product quality.
Patent Information
- Application Number
- CN202411006017.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-25
AI Technical Summary
When producing ultra-thick silicon steel with a thickness of more than 1.0mm on a continuous annealing coating line, there are problems such as welding tail drift, tearing caused by looper tension, scratches caused by deviation in the cleaning section, burning wrinkles caused by heating of the annealing furnace, and insufficient cooling capacity. The existing technology cannot effectively solve problems such as the rubber roller being burned and the winding speed being too fast, causing the roll to collapse.
Use 0.5~0.8mm strip steel lap welding, the loop tension is set to 15~18N/mm2, the cleaning section uses a squeeze roller instead of a brush roller, the annealing furnace temperature is controlled at 850-880°C, and the maximum opening of the cooling fan is 80% , the coiling speed is controlled at 10-20m/min, and the coiling tension is between 19-21N/mm2. These steps ensure the stability and quality of the strip during the production process.
It effectively avoids the deviation, squeezing, tearing, collapse and contusion of the strip during the production process, ensures the smooth continuous production of ultra-thick silicon steel, and improves product quality and production efficiency.
Smart Images

Figure CN118832384A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultra-thick silicon steel production, and in particular relates to a method for producing ultra-thick silicon steel with a thickness of more than 1.0 mm on a continuous annealing coating line. Background Art
[0002] The CEPC accelerator consists of a linear accelerator, an intensifier, a collider, and a beam transport line. At present, most of the international circular accelerator dipole magnets work under medium and high magnetic fields. The magnets use solid pure iron cores or high stacking coefficient silicon steel sheets stacked cores. The magnetic field design and processing and manufacturing processes are very mature. However, high-precision alternating low-field dipole magnets, especially high-precision dipole magnets with a minimum working magnetic field of 94Gs, require an iron dipole magnet solution manufactured using core dilution technology to meet the design requirements of high-precision low fields. The iron core is made of stacked steel and aluminum sheets, and the thickness of the steel and aluminum sheets is 1mm, so silicon steel sheets with a thickness of 1mm or more are required.
[0003] However, the following problems will be encountered in the production process of the continuous annealing line for ultra-thick silicon steel with a thickness of more than 1.0 mm: 1) Welding: Due to its own thickness, it is easy to deviate during welding tail swing, the welding parameters fluctuate too much, and the weld is easy to crack. 2) Loop: Due to its own weight, the ultra-thick silicon steel sheet with a thickness of 1.0 mm must increase its tension, otherwise the large sleeve will collapse easily, but when the tension is too large, it will tear due to its own hidden cracks; 3) Cleaning section: Due to the alkali solution and squeeze rollers in the cleaning section, the thick strip is prone to deviation and scratches during operation, resulting in squeezing and tearing; 4) Annealing furnace heating: The strip is too thick, and the strip speed cannot be too fast on the production line, but slow speed can easily cause the strip to burn and wrinkle. 5) Cooling section in the rear area of the annealing furnace: Insufficient cooling capacity can easily cause the rubber roller to be burned and the strip surface to produce color difference. 6) Coiling: The flying shear will not be able to cut continuously, and the strip head is prone to arching when it is transported to the coiler, and the coil will not be tight and collapsed after coiling. The above conditions will lead to strip wrinkles, deviation, poor weld quality, strip breakage, burning, coil collapse after coiling, and bruising.
[0004] However, the prior art does not disclose that the above problems will occur when producing ultra-thick silicon steel with a thickness of 1.0 mm on a continuous annealing line, nor does it provide an effective solution to the above problems.
[0005] Chinese patent CN 117900258 A discloses a method for producing ultra-thin silicon steel with a thickness of less than 0.15 mm on a continuous annealing coating line, the method comprising the following steps: uncoiling → head shearing → welding → cleaning → annealing → coating → drying → cooling → coiling. This patent is aimed at ultra-thin silicon steel with a thickness of less than 0.15 mm, and is only applicable to the production of ultra-thin silicon steel with a thickness of less than 0.15 mm. The production of ultra-thick silicon steel is actually different from ultra-thin silicon steel. The method in this patent cannot smoothly produce ultra-thick silicon steel with a thickness of more than 1.0 mm. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for producing ultra-thick silicon steel with a thickness of more than 1.0 mm on a continuous annealing line. The method can smoothly produce ultra-thick silicon steel with a thickness of more than 1.0 mm, and during the production process, there will be no strip wrinkling, deviation, poor weld quality, strip breakage, burning, coil collapse after coiling, and bruising. The quality of the produced silicon steel is good.
[0007] The technical solution adopted by the present invention is as follows:
[0008] The present invention provides a method for producing ultra-thick silicon steel with a thickness of more than 1.0 mm on a continuous annealing coating line, the method comprising the following steps: uncoiling → strip head shearing → welding → cleaning → annealing → cooling → coiling;
[0009] In the welding step, 0.5-0.8 mm strip steel overlaps 0.5-0.8 mm strip steel and is welded;
[0010] In the cleaning step, the squeeze roller is put into use normally, and the brush roller is not put into use;
[0011] In the annealing step, the temperature of the annealing furnace is controlled at 850-880°C, and the temperature of the steel strip and the rubber roller out of the annealing furnace is below 100°C;
[0012] In the cooling step, the maximum opening of the RJC variable frequency fan shall not be less than 80%, and the FJC constant speed cooling fan shall be fully opened;
[0013] In the winding step, the winding speed is not higher than 20 m / min.
[0014] In the unwinding step, the strip head is manually pulled with a tool or the gap between the rubber rollers is blocked with a steel plate by welding when winding; when unwinding the tail, the tail is manually flicked to correct the strip position when the strip deviates or gets stuck.
[0015] In the welding step, the welding current is 15000-17000A, the welding force is 280-600kN, and the welding speed is 3000-4100mm / min.
[0016] During the process from welding to cleaning, the strip passes through the looper, and the tension of the looper is set to 15-18N / mm 2 The speed of the loop filling is controlled within 20m / min, and the maximum amount of loop filling is controlled at 60%.
[0017] In the cleaning step, the pressure on both sides of the squeeze roller is guaranteed to be between 0.2 and 0.3 MPa, and the pressure difference on both sides is within ±0.01 MPa.
[0018] In the annealing step, the steel strip enters the annealing furnace at a conveying speed of 60-80 m / min.
[0019] In the annealing step, the temperatures of the RTF and SF sections are controlled at 855-865° C. and 865-875° C., respectively.
[0020] In the coiling step, the coiling speed of the silicon steel strip is controlled at 10-20 m / min.
[0021] In the winding step, the winding tension is controlled at 19-21N / mm 2 between.
[0022] When the rolled strip is rolled up, due to its large thickness and weight, the strip head is easily inserted into the gap between the rubber rollers. Therefore, when rolling up, it is necessary to manually pull the strip head with tools or weld the gap with steel plates; at the same time, 0.5-0.8mm strip steel is overlapped with 0.5-0.8mm strip steel for welding, with a welding current of 15000-17000A, a welding force of 280-600kN, and a welding speed of 3000-4100mm / min. The quality of the weld after welding has been verified many times and there is no problem, which can meet the process requirements.
[0023] When the thickness of the ultra-thick strip steel is 1.0mm or above, the plate shape collapses greatly and the deviation is serious when the looper is used for a large amount of looping. In order to solve this problem, the tension of the looper is set to 15-18N / mm in the entrance looper of the present invention. 2 The filling speed of the loop is controlled within 20m / min, and the maximum looping amount is controlled at 60%. After adopting this method, the loop runs stably.
[0024] During cleaning, the strip is prone to deviation, scratches, wrinkles or strip breakage; in the present invention, in the cleaning step, the squeezing roller in the cleaning section is normally put into use, between 0.2-0.3MPa, and the pressure difference on both sides is within ±0.01MPa, and the brush roller is not put into use, otherwise the strip is very likely to deviate in the cleaning section or scrape the edge due to the speed difference of the squeezing roller, causing strip breakage. The experiment was conducted without squeezing roller or with squeezing roller and brush roller, and the problem of 1-3cm deviation and scraping on the transmission side was found at 5#CPC in the cleaning section, and the machine stopped or broke the strip.
[0025] For extra-thick strip steel with a thickness of 1.0mm or above, its thickness is large and its own temperature is high. The daily RJC and FJC cooling capacity is insufficient, which can easily cause the rubber rollers to be burned and cause color difference on the strip surface. The power of the RJC variable frequency fan is adjusted to 80% or above, and the maximum opening shall not be less than 80%. All FJC constant speed cooling fans are turned on to ensure that the temperature of the strip steel and rubber rollers leaving the annealing furnace is below 100℃ to meet the strip cooling requirements.
[0026] If the temperature of the annealing furnace is too high, the strip will wrinkle, and when passing through the squeeze roller after the furnace, it will wrinkle and deform, causing scrap. Therefore, in the present invention, the temperature of the RTF and SF sections of the annealing furnace is controlled at 855-865°C and 865-875°C respectively during production, and the speed of the process section is controlled at 60-80m / min. If it is lower than 60m / min, the machine is stopped in time to prevent the strip from wrinkling.
[0027] When coiling at the exit, the strip is prone to slipping and wrinkling due to the high coiling speed, resulting in loose coiling. When unloading, the coil is prone to collapse and the strip surface rubs against each other, causing contusion. When coiling, the speed is controlled within 20m / min. If slipping occurs, it can be corrected in time with the help of tools. At the same time, the coiling unit tension is increased to 19-21N / mm 2 In between, it avoids the phenomenon of loose roll and collapsed roll.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The method for producing ultra-thick silicon steel with a thickness of 1.0 mm on a continuous annealing coating line provided by the present invention can smoothly complete the continuous production of ultra-thick silicon steel with a thickness of more than 1.0 mm on the continuous annealing coating line, solves the technical problems of uncoiling, welding, continuous shearing, coiling, etc. in the production of ultra-thick silicon steel with a thickness of more than 1.0 mm, effectively avoids production failures such as deviation, wrinkling, shaking and tearing, coil collapse and contusion of the strip during the production process, solves the problem of smooth production of ultra-thick silicon steel in batches, and enables ordinary continuous annealing coating lines to also have the production capacity of ultra-thick silicon steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1It is a schematic diagram of the composition of a continuous annealing furnace and a coating drying furnace, in which 01-inlet sealed chamber, 2-heating section (1RTF), 3-1st furnace throat (1FTH), 4-soaking furnace (1SF), 5-1st separator (1SEP), 6-heating section (2RTF), 7-2nd furnace throat (2FTH), 8-soaking furnace (2SF), 9-2nd separator (2SEP), 10-3rd furnace throat (3FTH), 11-tube cooling section (CTF), 12-4th furnace throat (4FTH), 13-circulating gas jet cooling slow cooling section (SJC), 14-5th furnace throat (5FTH), 15-circulating gas jet cooling fast cooling section (RJC), 16-exit sealed chamber, 17-FJC, 18-drying furnace (DF-DS), 19-sintering furnace (DF-BS), 20-air jet cooling section (AJC);
[0031] Figure 2 This is a picture of the ultra-thin silicon steel with a thickness of 1.0 mm produced in Example 1;
[0032] Figure 3 This is a picture of the poor quality of the weld of the ultra-thick strip steel in Comparative Example 1;
[0033] Figure 4 This is a picture of the belt being squeezed and broken in the cleaning section in Comparative Example 2;
[0034] Figure 5 This is a picture of the wrinkles in the annealing furnace of the ultra-thick strip steel in Comparative Example 3;
[0035] Figure 6 This is a photo of the color difference of the rubber roller caused by insufficient cooling of the ultra-thick strip in Comparative Example 4;
[0036] Figure 7 This is a picture of the ultra-thick silicon steel in comparative example 5 when the looper collapses;
[0037] Figure 8 This is a picture of the collapse of the ultra-thick silicon steel coil in Comparative Example 6;
[0038] Fig. 9 This is a photo of the surface damage of the ultra-thick strip steel in Comparative Example 7. DETAILED DESCRIPTION
[0039] The present invention provides a method for producing ultra-thick silicon steel with a thickness of more than 1.0 mm on a continuous annealing coating line, the method comprising the following steps: uncoiling → strip head shearing → welding → cleaning → annealing → cooling → coiling;
[0040] In the unwinding step, the strip head is manually pulled with a tool or the gap between the rubber rollers is blocked with a steel plate by welding when winding; when unwinding the tail, the tail is manually flicked to correct the strip position when the strip deviates or gets stuck.
[0041] In the welding step, 0.5-0.8 mm strip steel is overlapped with 0.5-0.8 mm strip steel for welding; the welding current is 15000-17000 A, the welding force is 280-600 kN, and the welding speed is 3000-4100 mm / min.
[0042] During the process from welding to cleaning, the strip passes through the looper, and the tension of the looper is set to 15-18N / mm 2 The speed of loop filling is controlled within 20m / min, and the maximum looping volume is controlled at 60%.
[0043] In the cleaning step, the squeeze roller is put into use normally, the brush roller is not put into use, the pressure on both sides of the squeeze roller is guaranteed to be between 0.2 and 0.3 MPa, and the pressure difference on both sides is within ±0.01 MPa;
[0044] In the annealing step, the temperature of the annealing furnace is controlled at 850-880°C at a strip conveying speed of 60-80m / min, wherein the temperatures of the RTF and SF sections are controlled at 855-865°C and 865-875°C, respectively; the maximum opening of the RJC variable frequency fan shall not be less than 80%, the FJC constant speed cooling fan is fully opened, and the temperature of the strip and rubber roller out of the annealing furnace is below 100°C;
[0045] In the coiling step, the coiling speed of the silicon steel strip is controlled at 10-20 m / min; the coiling tension is controlled at 19-21 N / mm 2 between.
[0046] The present invention is described in detail below with reference to the embodiments.
[0047] Example 1
[0048] A method for producing ultra-thick silicon steel with a thickness of 1.0 mm on a continuous annealing line, the method comprising the following steps: uncoiling → strip head shearing → welding → cleaning → annealing → cooling → coiling;
[0049] During rolling, the thickness of the head and tail of the strip steel is controlled at 0.65mm and 0.5mm respectively, and then the strip is unrolled, the head is sheared and welded. During welding, 0.65mm overlaps 0.5mm, the welding current is 15500A, the welding force is 300kN, the welding speed is 4000mm / min, the weld is fully penetrated and the quality is qualified. In the entrance looper, the tension of the looper is set to 16N / mm 2 , the looper filling speed is controlled within 20m / min, the maximum looping volume is controlled at 60%, and the looper runs stably;
[0050] In the cleaning step, the squeeze roller is put into use normally, the brush roller is not put into use, the pressure on both sides of the squeeze roller is adjusted to 0.25MPa, the strip steel in the cleaning section runs smoothly, there is no scraping edge on both sides of the strip steel, and there is no scratch on the surface, which is normal;
[0051] In the annealing step, the process speed is 80m / min, the furnace temperatures of the RTF and SF sections are controlled at 855°C and 865°C respectively, and the strip steel leaves the annealing furnace without burn wrinkles or yellowing, meeting the surface quality requirements;
[0052] In the cooling step, the fan opening of the RJC cooling section is set to 85%, and the three constant speed fans of the FJC are all turned on. The strip temperature out of the FJC cooling section is 81°C, which meets the process and rubber roller temperature requirements;
[0053] In the winding step, the winding speed is controlled at 20m / min and the winding tension is set at 21N / mm 2 There was no slippage or coil collapse during coiling, and there was no scratch on the upper and lower surfaces of the strip. 100XW-PEC grade silicon steel with a thickness of 1.0 mm was successfully produced. Figure 2 shown.
[0054] Example 2
[0055] A method for producing ultra-thick silicon steel with a thickness of 1.2 mm on a continuous annealing line, the method comprising the following steps: uncoiling → strip head shearing → welding → cleaning → annealing → cooling → coiling;
[0056] During rolling, the thickness of the head and tail of the strip steel is controlled at 0.72 and 0.65 mm respectively, and then the strip is uncoiled, the head is sheared and welded. During welding, 0.72 mm overlaps 0.65 mm, the welding current is 16200A, the welding force is 400kN, the welding speed is 3500mm / min, the weld is fully penetrated and the quality is qualified. In the entrance looper, the tension of the looper is set to 16N / mm 2 , the looper filling speed is controlled within 20m / min, the maximum looping volume is controlled at 60%, and the looper runs stably;
[0057] In the cleaning step, the squeeze roller is put into use normally, the brush roller is not put into use, the pressure on both sides of the squeeze roller is adjusted to 0.28MPa, the strip steel in the cleaning section runs smoothly, there is no scraping edge on both sides of the strip steel, and there is no scratch on the surface, which is normal;
[0058] In the annealing step, the process speed is 70m / min, the furnace temperatures of the RTF and SF sections are controlled at 860°C and 870°C respectively, and the strip steel leaves the annealing furnace without burn wrinkles or yellowing, meeting the surface quality requirements;
[0059] In the cooling step, the fan opening of the RJC cooling section is set to 88%, and the three constant speed fans of the FJC are all turned on. The strip temperature out of the FJC cooling section is 90°C, which meets the process and rubber roller temperature requirements;
[0060] In the winding step, the winding speed is controlled at 17m / min and the winding tension is set at 20N / mm 2 There was no slippage or coil collapse during coiling, and there was no scratch on the upper and lower surfaces of the strip. Silicon steel with a thickness of 1.2mm and a grade of 120XW-PEC was successfully produced.
[0061] In this embodiment, during the production process of silicon steel, there is no strip wrinkling, deviation, poor weld quality, strip breakage, burning, coil collapse after coiling, or bruising.
[0062] Example 3
[0063] A method for producing ultra-thick silicon steel with a thickness of 1.5 mm on a continuous annealing line, the method comprising the following steps: uncoiling → strip head shearing → welding → cleaning → annealing → cooling → coiling;
[0064] During rolling, the thickness of the head and tail of the strip steel is controlled at 0.8mm and 0.72mm respectively, and then the strip is unrolled, the head is sheared and welded. During welding, 0.8mm overlaps 0.72mm, the welding current is 17000A, the welding force is 500kN, the welding speed is 3000mm / min, the weld is fully penetrated and the quality is qualified. In the entrance looper, the tension of the looper is set to 16N / mm 2 , the looper filling speed is controlled within 20m / min, the maximum looping volume is controlled at 60%, and the looper runs stably;
[0065] In the cleaning step, the squeeze roller is put into use normally, the brush roller is not put into use, the pressure on both sides of the squeeze roller is adjusted to 0.30 MPa, the strip steel in the cleaning section runs smoothly, there is no scraping edge on both sides of the strip steel, and there is no scratch on the surface, which is normal;
[0066] In the annealing step, the process speed is 60m / min, the furnace temperatures of the RTF and SF sections are controlled at 865°C and 875°C respectively, and the strip steel leaves the annealing furnace without burn wrinkles or yellowing, meeting the surface quality requirements;
[0067] In the cooling step, the fan opening of the RJC cooling section is set to 90%, and all three FJC constant speed fans are turned on. The strip temperature out of the FJC cooling section is 75°C, which meets the process and rubber roller temperature requirements;
[0068] In the winding step, the winding speed is controlled at 15m / min and the winding tension is set at 19N / mm 2There was no slippage or coil collapse during coiling, and there was no scratch on the upper and lower surfaces of the strip. 150XW-PEC grade silicon steel with a thickness of 1.5mm was successfully produced.
[0069] In this embodiment, during the production process of silicon steel, there is no strip wrinkling, deviation, poor weld quality, strip breakage, burning, coil collapse after coiling, or bruising.
[0070] Comparative Example 1
[0071] The other parts are the same as in Example 1. During rolling, the thickness of the strip head and tail is controlled at 1.0 mm. The head and tail are 1.0 mm overlapped and welded. The weld is not fully penetrated. During operation, tearing occurs. Figure 3 shown.
[0072] Comparative Example 2
[0073] The other parts are the same as in Example 1, except that the pressure of the squeeze roller is not finely adjusted during cleaning, and the pressure is in the range of 0.35-0.5MPa. The pressure deviation value on both sides of some squeeze rollers exceeds 0.03MPa. When producing 1.1mm thick silicon steel, the strip deviates, scrapes, wrinkles and breaks in the cleaning section. Figure 4 shown.
[0074] Comparative Example 3
[0075] The other parts are the same as in Example 2, except that the temperature in the SF section of the annealing furnace is 900°C, and the strip has obvious burn wrinkles when it comes out of the furnace, such as Figure 5 shown.
[0076] Comparative Example 4
[0077] The other parts are the same as in Example 2, except that the power of the RJC cooling fan on the production line is only set to 70% opening, the strip cooling capacity is insufficient, resulting in the rubber roller being burned, and the rubber roller color difference is obvious on the surface of the strip. Figure 6 shown.
[0078] Comparative Example 5
[0079] The rest is the same as in Example 3, except that the entrance looper is too large, 70% of the looper, and the entrance looper runs off the tower type parking, such as Figure 7 shown.
[0080] Comparative Example 6
[0081] The other parts are the same as in Example 3, except that the coiling speed is too fast, the coiling speed is 30m / min, and the steel coil collapses after unloading. Figure 8 shown.
[0082] Comparative Example 7
[0083] The other parts are the same as in Example 3, except that the winding tension is small during winding, and the winding tension is 18N / mm 2, when the coils were separated, serious bruises were found on the surface of the coils, such as Fig. 9 shown.
[0084] The above-mentioned detailed description of a method for producing ultra-thick silicon steel with a thickness of more than 1.0 mm on a continuous annealing coating line with reference to the embodiment is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for producing ultra-thick silicon steel with a thickness of more than 1.0 mm on a continuous annealing coating line, characterized in that: The method comprises the following steps: uncoiling→strip head shearing→welding→cleaning→annealing→cooling→coiling; In the welding step, 0.5-0.8 mm strip steel overlaps 0.5-0.8 mm strip steel for welding; In the cleaning step, the squeeze roller is put into use normally, and the brush roller is not put into use; In the annealing step, the temperature of the annealing furnace is controlled at 850-880°C, and the temperature of the steel strip and the rubber roller out of the annealing furnace is below 100°C; In the cooling step, the maximum opening of the RJC variable frequency fan shall not be less than 80%, and the FJC constant speed cooling fan shall be fully opened; In the winding step, the winding speed is not higher than 20 m / min.
2. The method according to claim 1, characterized in that In the unwinding step, the strip head is manually pulled with a tool or the gap between the rubber rollers is blocked with a steel plate by welding when winding; when unwinding the tail, the tail is manually flicked to correct the strip position when the strip deviates or gets stuck.
3. The method according to claim 1, characterized in that In the welding step, the welding current is 15000-17000A, the welding force is 280-600kN, and the welding speed is 3000-4100mm / min.
4. The method according to claim 1, characterized in that During the process from welding to cleaning, the strip passes through the looper, and the tension of the looper is set to 15-18N / mm 2 The speed of loop filling is controlled within 20m / min, and the maximum looping volume is controlled at 60%.
5. The method according to claim 1, characterized in that In the cleaning step, the pressure on both sides of the squeeze roller is guaranteed to be between 0.2 and 0.3 MPa, and the pressure difference on both sides is within ±0.01 MPa.
6. The method according to claim 1, characterized in that In the annealing step, the steel strip enters the annealing furnace at a conveying speed of 60-80 m / min.
7. The method according to claim 1, characterized in that In the annealing step, the temperatures of the RTF and SF sections are controlled at 855-865° C. and 865-875° C., respectively.
8. The method according to claim 1, characterized in that In the coiling step, the coiling speed of the silicon steel strip is controlled at 10-20 m / min.
9. The method according to claim 1, characterized in that: In the winding step, the winding tension is controlled at 19-21N / mm 2 between.
Citation Information
Patent Citations
Method for producing ultrathin silicon steel with thickness below 0.15 mm on continuous annealing coating line