Perfluoroether rubber composition, perfluoroether rubber as well as preparation method and application of perfluoroether rubber

By using peroxide vulcanizing agents and cage silsesquioxane and other additives in perfluoroether rubber, a vulcanized rubber with excellent high temperature resistance and chemical resistance is formed, which solves the problem of high temperature problems of perfluoroether rubber in the existing technology. and seal failure problems in acidic environments, achieving long-term stability and performance improvement under extreme conditions.

CN118834484AActive Publication Date: 2024-10-25CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310439596.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-25
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

Existing perfluoroether rubber cannot meet the requirements of high temperature resistance and chemical resistance at the same time, and is prone to sealing failure especially in extreme high temperatures and acidic environments.

Method used

A perfluoroether rubber composition containing a peroxide vulcanizing agent, a specific co-vulcanizing agent such as caged silsesquioxane (POSS) and an antioxidant is used to form a perfluoroether rubber composition with excellent high temperature resistance and anti-aging properties through free radical reaction and cross-linking reaction. Vulcanized rubber with chemical resistance.

Benefits of technology

Perfluoroether rubber has been realized for long-term use in high-temperature and harsh environments, meeting the needs of rubber sealing parts and improving mechanical properties and anti-aging properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118834484A_ABST
    Figure CN118834484A_ABST
Patent Text Reader

Abstract

The invention relates to the field of fluorine-containing high polymer materials, in particular to a perfluoroether rubber composition, perfluoroether rubber and a preparation method and application thereof. The perfluoroether rubber composition is characterized in that the perfluoroether rubber composition comprises the following components in parts by weight: 100 parts of perfluoroether rubber, 1-5 parts of a vulcanizing agent, 1-10 parts of an auxiliary vulcanizing agent, 1-10 parts of an anti-aging agent, 1-5 parts of a processing aid and 1-30 parts of filler, wherein the vulcanizing agent is a peroxide vulcanizing agent; the general formula of the auxiliary vulcanizing agent is (RSiO3 / 2) n, n is 6, 8, 10 or 12, R is alkenyl of C2-C10, # imgabs0 # R1 is hydrogen or alkyl of C1-C4, R2 is (CH2) m, and m is an integer of 1-10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fluorine-containing polymer materials, and in particular to a perfluoroether rubber composition, a perfluoroether rubber, and a preparation method and application thereof. Background Art

[0002] With the increasing demand for energy and the near exhaustion of easily exploitable oil and natural gas resources, hot dry rock has become a hot spot for development as a new type of geothermal resource, and oil and gas exploration and development are moving towards deeper strata. The extremely high underground temperature environment has put forward extremely stringent requirements on the performance of the materials used. The temperature of hot dry rock is generally greater than 230℃, and the use of conventional high-temperature resistant rubber materials is very likely to cause sealing failure under such extreme high temperature conditions. The development of high-temperature resistant rubber has become one of the technical bottlenecks restricting effective underground mining and development.

[0003] Perfluoroether rubber is mainly obtained by copolymerizing tetrafluoroethylene and perfluoroalkyl vinyl ether as main monomers with vulcanization point monomers. All hydrogen atoms on all carbon atoms in perfluoroether rubber are replaced by fluorine atoms, and it has excellent high temperature resistance and chemical corrosion resistance. During the vulcanization process of perfluoroether rubber, its vulcanization system is composed of a vulcanizing agent and a vulcanizing agent. The vulcanizing agent is mainly allyl isocyanurate (TAIC) or triallyl cyanurate (TAC), etc., which makes the cross-linked structure of the vulcanized rubber contain amide groups. Amide groups will undergo decomposition reactions in an acidic environment, which will reduce the mechanical properties of perfluoroether rubber and cause sealing failure.

[0004] At present, there are many commercial products of perfluoroether rubber, which can work for a long time in the high temperature field of 300℃. Perfluoroether rubber has been widely used in aerospace, chemical industry, semiconductor and other fields. The perfluoroelastomer with bromine or iodine curing point is cured with peroxide. The perfluoroelastomer after curing has good chemical resistance. An important advantage of the iodide curing system is that it does not contain metal oxides or other metal catalysts, which makes the elastomer not easy to be corroded in water or acidic environment, but sacrifices some thermal stability. The upper limit temperature of its continuous use is 218℃. It is impossible to meet the requirements of high temperature resistance and chemical resistance at the same time. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that perfluoroether rubber in the prior art cannot have both high temperature resistance and chemical resistance, and to provide a perfluoroether rubber composition, a perfluoroether rubber and a preparation method and application thereof. The perfluoroether rubber prepared from the rubber composition not only has high temperature aging resistance, but also has excellent chemical resistance and can be used for a long time in harsh environments.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a perfluoroether rubber composition, characterized in that the perfluoroether rubber composition comprises: 100 parts by weight of perfluoroether rubber, 1-5 parts by weight of a vulcanizing agent, 1-10 parts by weight of a co-vulcanizing agent, 1-10 parts by weight of an antioxidant, 1-5 parts by weight of a processing aid and 1-30 parts by weight of a filler;

[0007] Wherein, the vulcanizing agent is a peroxide vulcanizing agent; the general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n , n is 6, 8, 10 or 12, R is C 2 -C 10 The alkenyl group, R 1 is hydrogen or C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 10.

[0008] The second aspect of the present invention provides a method for preparing perfluoroether rubber, characterized in that the method comprises: mixing and vulcanizing the components in the perfluoroether rubber composition provided by the present invention.

[0009] The third aspect of the present invention provides a perfluoroether rubber prepared by the method of the present invention.

[0010] A fourth aspect of the present invention provides use of the perfluoroether rubber composition or perfluoroether rubber of the present invention in the manufacture of rubber sealing components.

[0011] Through the above technical scheme, the perfluoroether rubber composition, perfluoroether rubber and the preparation method and application thereof provided by the present invention achieve the following beneficial effects:

[0012] The perfluoroether rubber composition provided by the present invention contains components of specific types and amounts, and the components cooperate and coordinate with each other, so that the vulcanized rubber prepared therefrom has excellent high temperature aging resistance and chemical resistance.

[0013] Furthermore, the perfluoroether rubber provided by the present invention can be used in high-temperature and harsh environments to meet the requirements of rubber sealing components. DETAILED DESCRIPTION

[0014] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0015] The first aspect of the present invention provides a perfluoroether rubber composition, characterized in that the perfluoroether rubber composition comprises: 100 parts by weight of perfluoroether rubber, 1-5 parts by weight of a vulcanizing agent, 1-10 parts by weight of a co-vulcanizing agent, 1-10 parts by weight of an antioxidant, 1-5 parts by weight of a processing aid, and 1-30 parts by weight of a filler;

[0016] Wherein, the vulcanizing agent is a peroxide vulcanizing agent; the general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n The compound wherein n is 6, 8, 10 or 12, and R is C 2 -C 10 The alkenyl group, R 1 is hydrogen or C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 10.

[0017] In the present invention, the fluorine content of the perfluoroether rubber is ≥75wt%, which can achieve free radical reaction with the above-mentioned co-vulcanizing agent and then cross-linking reaction with the vulcanizing agent, so that the obtained perfluoroether rubber has excellent high temperature resistance and chemical resistance.

[0018] In the present invention, a cage-type silsesquioxane (POSS) structure is introduced into perfluoroether rubber as a crosslinking agent. Multiple active sites are utilized. This chemical structure is relatively stable in water, and the side chain has a highly active carbon-carbon double bond to generate free radicals, which can be used to initiate a crosslinking reaction. The free radicals can react with free radicals in the perfluoroether rubber and then react with a vulcanizing agent to generate a crosslinking reaction. The POSS cage-type structure is introduced into the rubber crosslinking network, thereby improving the mechanical properties of the perfluoroether rubber.

[0019] Furthermore, the use of the above-mentioned specific weight portion of POSS as a vulcanizing agent can make the vulcanized perfluoroether rubber have excellent high temperature aging resistance and chemical resistance. When the POSS content is too much, agglomeration will occur, affecting the above-mentioned properties of the rubber.

[0020] In the present invention, the specific weight parts of perfluoroether rubber, vulcanizing agent, co-vulcanizing agent, antioxidant, processing aid and filler in the perfluoroether rubber composition are coordinated to make the prepared vulcanized perfluoroether rubber meet the requirements of high temperature aging resistance and chemical resistance.

[0021] According to the present invention, the perfluoroether rubber composition comprises: 100 parts by weight of perfluoroether rubber, 1-5 parts by weight of a vulcanizing agent, 3-8 parts by weight of a co-vulcanizing agent, 1-5 parts by weight of an antioxidant, 1-5 parts by weight of a processing aid, and 10-30 parts by weight of a filler;

[0022] Wherein, the vulcanizing agent is a peroxide vulcanizing agent, and the general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n , n is 6, 8, 10 or 12, R is R 1 is hydrogen or C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 4.

[0023] According to the present invention, the general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n , n is 8, R is R 1 C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 4.

[0024] In the present invention, POSS containing both carbon-carbon double bonds and acyloxy groups is used as a co-crosslinking agent, which not only improves the mechanical properties, but also enhances the anti-aging properties of the rubber.

[0025] Preferably, R 1 is methyl or ethyl, R 2 for (CH 2 ) m , m is an integer from 1 to 3.

[0026] According to the present invention, the co-vulcanizing agent is selected from methacryloxypropyl cage silsesquioxane and / or acryloxy cage silsesquioxane.

[0027] According to the present invention, the co-vulcanizing agent is methacryloxypropyl cage silsesquioxane and acryloxy cage silsesquioxane.

[0028] In the present invention, methacryloxypropyl cage silsesquioxane (MAPOSS) and acryloxy cage silsesquioxane (AOPOSS) are used together. According to the principle of similar compatibility of polarity, methacryloxypropyl cage silsesquioxane and perfluoroether rubber are both polar, and the two have excellent compatibility. The presence of methyl activates the acryloxypropyl group, which improves the free radical reaction activity of POSS. In addition, the two materials used together are used as co-crosslinking agents, and the molecules are hybridized cage structures. Specifically, the carbon atoms connected to the propylene group are sp2 hybridized, the other carbon atom is sp3 hybridized, and the acyloxy group is sp2 hybridized. The above hybrid cage structure combines the advantages of organic groups and inorganic groups and the hollow cage structure to improve the mechanical properties of perfluoroether rubber.

[0029] According to the present invention, the weight ratio of the methacryloxypropyl cage silsesquioxane to the acryloxy cage silsesquioxane is 0.25-4:1, preferably 1.5-4:1.

[0030] In the present invention, MAPOSS and AOPOSS in a specific weight ratio are used as co-vulcanizing agents, and the anti-aging performance of the perfluoroether rubber is more excellent.

[0031] According to the present invention, the vulcanizing agent is a peroxide vulcanizing agent, preferably one of dicumyl peroxide, di(tert-butylperoxide isopropyl)benzene, dibenzoyl peroxide, di(2,4-dichlorobenzoyl)benzoyl peroxide, and 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane.

[0032] In the present invention, a specific weight portion of a peroxide vulcanizing agent is used. If the amount used is too small, the number of crosslinking points produced is small and the rubber performance is poor; if the amount used is too large, the rubber is over-crosslinked, which will have an adverse effect on the performance of the prepared perfluoroether rubber, and the residues of the peroxide decomposition will affect the performance of the perfluoroether rubber.

[0033] Furthermore, dicumyl peroxide is selected as a vulcanizing agent, and there is no large-area foaming on the rubber surface after high-temperature vulcanization.

[0034] According to the present invention, the filler is hard carbon black.

[0035] According to the present invention, the antioxidant is selected from quinoline antioxidants and / or benzimidazole antioxidants.

[0036] According to the present invention, the quinoline antioxidant is 2,2,4-trimethyl-1,2-dihydroquinoline, and the benzimidazole antioxidant is 2-mercaptobenzimidazole zinc salt.

[0037] According to the present invention, the antioxidants are 2-mercaptobenzimidazole and 2,2,4-trimethyl-1,2-dihydroquinoline.

[0038] Preferably, the weight ratio of the 2-mercaptobenzimidazole to the 2,2,4-trimethyl-1,2-dihydroquinoline is 1:1-2.

[0039] According to the present invention, the processing aid is stearate, preferably sodium stearate.

[0040] The second aspect of the present invention provides a method for preparing perfluoroether rubber, characterized in that the method comprises: mixing and vulcanizing the components in the perfluoroether rubber composition provided by the present invention.

[0041] According to the present invention, the method comprises:

[0042] (1) mixing perfluoroether rubber, a vulcanizing agent, a filler, an antioxidant, a vulcanizing agent and a processing aid to obtain a rubber mixture;

[0043] (2) vulcanizing the rubber mixture to obtain the perfluoroether rubber.

[0044] According to the present invention, the vulcanization comprises: performing a first-stage vulcanization on the rubber mix in a flat vulcanizer, and then performing a second-stage vulcanization in an oven.

[0045] According to the present invention, the vulcanization temperature is 160-180° C., the vulcanization pressure is 5-20 MPa, and the vulcanization time is 10-30 min.

[0046] According to the present invention, the conditions of the two-stage vulcanization include: a vulcanization temperature of 200-240° C. and a vulcanization time of 6-24 hours.

[0047] The third aspect of the present invention provides perfluoroether rubber prepared by the preparation method of the present invention.

[0048] A fourth aspect of the present invention provides use of the perfluoroether rubber composition or perfluoroether rubber of the present invention in the manufacture of rubber sealing components.

[0049] The present invention will be described in detail below by way of examples. In the following examples,

[0050] The mechanical properties (hardness, tensile strength, elongation at break) of perfluoroether rubber were measured using the GB / T528-2009 method;

[0051] The high temperature aging resistance of perfluoroether rubber was measured in a hydrothermal reactor under the aging conditions of 300℃, 15MPa, and 48h.

[0052] The high temperature chemical (acid, alkali, oil) resistance of perfluoroether rubber is measured in a hydrothermal reactor at a temperature of 300°C, a total pressure of 15MPa, an aging time of 48h, and aging conditions of 20% NaOH, 20% HCl or hydraulic oil;

[0053] Mass change rate = (mass increase of perfluoroether rubber after aging test / mass of perfluoroether rubber before aging) * 100. The smaller the value, the better the aging resistance of perfluoroether rubber.

[0054] The perfluoroether rubber is PM 3000 produced by Asahi Glass.

[0055] The vulcanizing agent is industrial grade dicumyl peroxide (DCP) and sulfur powder produced by Shijiazhuang Fate Chemical Technology Co., Ltd.

[0056] The curing agent POSS is methacryloyloxypropyl cage silsesquioxane (MAPOSS, n is 8, R 1 is methyl, R 2 is propylene), acryloxy cage silsesquioxane (AOPOSS, n is 8, R 1 is hydrogen, R 2 is propylene), cage-type octavinyl polysilsesquioxane (OVPOSS, n is 8, R is vinyl), octahydrogen cage-type silsesquioxane (Octa H-POSS, n is 8, R is hydrogen).

[0057] The filler is N550 from Cabot Chemical (Tianjin) Co., Ltd.

[0058] The antioxidants are 2-mercaptobenzimidazole and 2,2,4-trimethyl-1,2-dihydroquinoline from Shanghai Lanrun Chemical Co., Ltd., and N-phenyl-N ’ -cyclohexyl-p-phenylenediamine (4040NA), N,N-di-n-butyldithiocarbamate nickel (NBC) from Shanghai Lanrun Chemical Co., Ltd.

[0059] The processing aid is sodium stearate from Aladdin Reagent (Shanghai) Co., Ltd.

[0060] The formulations of the perfluoroether rubber compositions A1-A8 and D1-D2 provided in Examples 1-8 and Comparative Examples 1-2 are shown in Table 1.

[0061] Table 1 (parts by weight)

[0062]

[0063] Preparation Example

[0064] According to the formula shown in Table 1, the components were mixed to obtain a rubber compound; the rubber compound was subjected to a first-stage vulcanization in a vulcanizer, and the conditions for the first stage vulcanization were: temperature 170°C, pressure 10MPa, and vulcanization time 10min; the second stage vulcanization was carried out in an oven, and the vulcanization conditions were 220°C×12h. The obtained rubber products S1-S8 and DS1-DS2 were tested for their properties, and the test results are shown in Tables 2-5.

[0065] Table 2

[0066]

[0067]

[0068] Table 3

[0069]

[0070] Table 4

[0071]

[0072] Table 5

[0073]

[0074]

[0075] It can be seen from the results of Tables 2-5 that the perfluoroether rubber prepared by the perfluoroether rubber composition provided by Examples 1-8 of the present invention has excellent high temperature resistance (300°C), chemical resistance and aging resistance compared with the comparative example, and can be used to make rubber sealing components. In particular, in Table 2, after high-temperature aging, the perfluoroether rubber prepared by the perfluoroether rubber composition provided by Examples 1-8 of the present invention will undergo further cross-linking, and the tensile strength is greater than that before the aging treatment.

[0076] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A perfluoroether rubber composition, It is characterized in that The perfluoroether rubber composition comprises: 100 parts by weight of perfluoroether rubber, 1-5 parts by weight of a vulcanizing agent, 1-10 parts by weight of a co-vulcanizing agent, 1-10 parts by weight of an antioxidant, 1-5 parts by weight of a processing aid and 1-30 parts by weight of a filler; Wherein, the vulcanizing agent is a peroxide vulcanizing agent; the general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n , n is 6, 8, 10 or 12, R is C 2 -C 10 The alkenyl group, R 1 is hydrogen or C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 10.

2. The perfluoroether rubber composition according to claim 1, in, The perfluoroether rubber composition comprises: 100 parts by weight of perfluoroether rubber, 1-5 parts by weight of a vulcanizing agent, 3-8 parts by weight of a co-vulcanizing agent, 1-5 parts by weight of an antioxidant, 1-5 parts by weight of a processing aid, and 10-30 parts by weight of a filler; Wherein, the vulcanizing agent is a peroxide vulcanizing agent; the general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n , n is 6, 8, 10 or 12, R is R 1 is hydrogen or C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 4.

3. The perfluoroether rubber composition according to claim 1 or 2, in, The general formula of the co-vulcanizing agent is (RSiO 3 / 2 ) n , n is 8, R is R 1 C 1 -C 4 The alkyl group, R 2 for (CH 2 ) m , m is an integer from 1 to 4; Preferably, the co-vulcanizing agent is selected from methacryloxypropyl cage silsesquioxane and / or acryloxy cage silsesquioxane; More preferably, the co-vulcanizing agent is methacryloxypropyl cage silsesquioxane and acryloxy cage silsesquioxane.

4. The perfluoroether rubber composition according to any one of claims 1 to 3, in, The weight ratio of the methacryloxypropyl cage silsesquioxane to the acryloxy cage silsesquioxane is 0.25-4:1, preferably 1.5-4:

1.

5. The perfluoroether rubber composition according to any one of claims 1 to 4, in, The vulcanizing agent is selected from one of dicumyl peroxide, di(tert-butylperoxyisopropyl)benzene, dibenzoyl peroxide, di(2,4-dichlorobenzoyl)benzoyl peroxide, and 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane; Preferably, the filler is carbon black, preferably hard carbon black; Preferably, the processing aid is a stearate, preferably sodium stearate; Preferably, the antioxidant is selected from quinoline antioxidants and / or benzimidazole antioxidants; Preferably, the quinoline antioxidant is 2,2,4-trimethyl-1,2-dihydroquinoline, and the benzimidazole antioxidant is 2-mercaptobenzimidazole zinc salt; Preferably, the antioxidant is 2-mercaptobenzimidazole and 2,2,4-trimethyl-1,2-dihydroquinoline; Preferably, the weight ratio of the 2-mercaptobenzimidazole to the 2,2,4-trimethyl-1,2-dihydroquinoline is 1:1-2.

6. A method for preparing perfluoroether rubber, It is characterized in that The method comprises: mixing and vulcanizing the components in the perfluoroether rubber composition according to any one of claims 1 to 5.

7. The preparation method according to claim 6, in, The method comprises: (1) mixing perfluoroether rubber, a vulcanizing agent, a filler, an antioxidant, a vulcanizing agent and a processing aid to obtain a rubber mixture; (2) vulcanizing the rubber mixture to obtain the perfluoroether rubber.

8. The method according to claim 6 or 7, in, The vulcanization is a two-stage vulcanization; Preferably, the vulcanization comprises: performing a first-stage vulcanization on the rubber mix in a flat vulcanizer, and then performing a second-stage vulcanization in an oven; Preferably, the conditions of the one-stage vulcanization include: a vulcanization temperature of 160-180°C, a vulcanization pressure of 5-20MPa, and a vulcanization time of 10-30min; Preferably, the conditions of the two-stage vulcanization include: a vulcanization temperature of 200-240° C. and a vulcanization time of 6-24 hours.

9. Perfluoroether rubber obtained by the method according to any one of claims 6 to 8.

10. Use of the perfluoroether rubber composition according to any one of claims 1 to 5 or the perfluoroether rubber according to claim 9 in the manufacture of rubber sealing parts.

Citation Information

Patent Citations

  • Low-stress epoxy / organic silicon / POSS nano hybrid material, and preparation method and application thereof

    CN101974227A

  • Silicon rubber-fluorocarbon coating interpenetrating network structure polymer and preparation method thereof

    CN108192455A

  • Low-temperature-resistant perfluoroether rubber composition as well as preparation method and application thereof

    CN112457612A

  • Rubber composition

    JP2010024400A

Cited By

  • High-adhesion organic silicon electronic pouring sealant and preparation method thereof

    CN119161852A

  • High-adhesion organosilicon electronic potting glue and preparation method thereof

    CN119161852B

  • Plasma-resistant perfluoroether rubber and preparation method thereof

    CN119955239A

  • A plasma-resistant perfluoroether rubber and its preparation method

    CN119955239B