A kind of degradable plastic and preparation method thereof

By combining polyester with modified bamboo lignin, a biodegradable plastic was prepared, which solved the problem of difficult degradation of petroleum-based plastics, achieved biodegradability and performance improvement, and reduced environmental pollution.

CN118834512BActive Publication Date: 2024-11-29RUGAO HENGXIANG PLASTIC CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411331370.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-29
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

Existing petroleum-based plastics are difficult to degrade, resulting in environmental pollution and ecosystem damage, and lack of efficient and degradable materials.

Method used

Modified polyester is prepared by reacting polyester with 4-amino-2,2,6,6-tetramethylpiperidine, and modified bamboo lignin reacts with 3-mercaptopropanol to produce modified bamboo Lignin, combined with melt plasticization and calendering, produces a biodegradable plastic.

Benefits of technology

The biodegradability, flame retardant properties, mechanical properties and anti-aging properties of degradable plastics have been improved, and can quickly decompose in nature and reduce environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a degradable plastic and a preparation method thereof, and relates to the technical field of polymer materials. When preparing the degradable plastic, the present invention performs melt polycondensation on diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol, and 1,4-butene glycol to obtain polyester; the polyester is reacted with 4-amino-2,2,6,6-tetramethylpiperidine to obtain a modified polyester; the bamboo alkali lignin is purified and reacted with melamine to obtain pre-treated bamboo lignin; the pre-treated bamboo lignin is reacted with diethyl phosphite to obtain pre-modified bamboo lignin; the pre-modified bamboo lignin is reacted with 3-mercaptopropanol to obtain modified bamboo lignin; the modified polyester and the modified bamboo lignin are melt-plasticized and then calendered to obtain a degradable plastic. The degradable plastic prepared by the present invention has excellent flame retardancy, anti-aging, degradability and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a degradable plastic and a preparation method thereof. Background Art

[0002] As a new type of chemical material, plastic has developed rapidly since the 1950s due to its advantages of low cost, light weight, good performance, complete variety, convenient processing and wide application. It is widely used in food packaging, textiles, automobiles, electronics, medical equipment and other fields. As plastic products are used more and more widely in human life and production, they have also caused a series of problems for the environment: the plastic products currently used are generally petroleum-based plastics, which have a low recycling rate and are difficult to degrade or have a long degradation period in nature, which can easily cause "white pollution", cause a series of damages to the soil and environment, and seriously damage the ecological environment system.

[0003] In order to cope with the increasingly serious environmental problems, more and more researchers have begun to explore and develop a green and environmentally friendly material that can be degraded in a short time. Biodegradable materials have very important research value and broad market prospects because of their good degradability and environmental protection. Summary of the invention

[0004] The purpose of the present invention is to provide a degradable plastic and a preparation method thereof to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A degradable plastic is prepared by reacting polyester with 4-amino-2,2,6,6-tetramethylpiperidine to obtain modified polyester; reacting pre-modified bamboo lignin with 3-mercaptopropanol to obtain modified bamboo lignin; and calendering the modified polyester and the modified bamboo lignin after melt plasticization.

[0007] As an optimization, the polyester is prepared by melt polycondensation of diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol.

[0008] As an optimization, the pre-modified bamboo lignin is prepared by reacting pre-treated bamboo lignin with diethyl phosphite.

[0009] As an optimization, the pretreated bamboo lignin is prepared by reacting the purified bamboo alkali lignin with melamine.

[0010] A method for preparing a degradable plastic comprises the following steps:

[0011] (1) Diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol were mixed in a molar ratio of 1:(0.4-0.6):1:(0.4-0.6), and tetrabutyl titanate (0.05-0.07 times the mass of diethyl terephthalate) was added. In a nitrogen atmosphere, the mixture was stirred at 175-185°C and 300-500 r / min for 2-3 h. The mixture was heated to 220-230°C and heated at 3-5 Pa and 300-50 0r / min, continue stirring the reaction for 6-8h, cool to room temperature to obtain a crude product, and purify the crude product to obtain polyester; mix polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform in a mass ratio of 1:(0.4-0.6):(0.4-0.6):(20-24), stir and react at 45-55°C, 300-500r / min for 3-4h, and dry at 5-7Pa, 40-50°C for 20-24h to obtain modified polyester;

[0012] (2) Purified bamboo lignin, melamine, and 1,4-dioxane aqueous solution were mixed at a mass ratio of 1:(0.3-0.4):(9-11), and acetic acid (1.4-1.6 times the mass of purified bamboo lignin) and formaldehyde aqueous solution (35-37% by mass) (0.2-0.3 times the mass of purified bamboo lignin) were added, and the mixture was stirred at 55-65°C and 300-500 r / min for 4-5 h. Deionized water (20-30 times the mass of purified bamboo lignin) was added and mixed evenly, and the mixture was centrifuged. The precipitate was dried at 5-7 Pa and 45-55°C for 6-7 h to obtain pretreated bamboo lignin. Pretreated bamboo lignin, diethyl phosphite, formaldehyde, and N,N-dimethylformamide were mixed at a mass ratio of 1:(0.2-0.3):(0.1-0 .2):(9~11) are mixed evenly, and the pH value is adjusted to 4.9~5.1 with a hydrochloric acid aqueous solution with a mass fraction of 11~13%, and the mixture is stirred at 65~75℃ and 300~500r / min for 4~5h, and dried at 5~7Pa and 50~60℃ for 7~8h to obtain pre-modified bamboo lignin; the pre-modified bamboo lignin, 3-mercaptopropanol, p-toluenesulfonic acid, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(0.4~0.6):(0.03~0.05):(12~14), and the mixture is stirred at 120~130℃ and 300~500r / min for 4~5h, and centrifuged, and the precipitate is washed with deionized water for 3~5 times, and dried at 5~7Pa and 50~60℃ for 7~8h to obtain modified bamboo lignin;

[0013] (3) Add the modified polyester and modified bamboo lignin in a mass ratio of 1:(0.2~0.3) into an internal mixer, stir at 150~160℃ and 300~500r / min for 8~10min, then add 0.01~0.03 times the mass of azobisisobutyronitrile of the modified polyester, mix well, place on a flat vulcanizer for calendering, and press into a film with a thickness of 0.9~1.1mm to obtain a biodegradable plastic.

[0014] As an optimization, the purification process of the crude product in step (1) is as follows: the crude product is mixed evenly with chloroform in a mass ratio of 1:(8-10) to completely dissolve the crude product, and then 20-30 times the mass of methanol of the crude product is added to mix evenly, allowed to stand for 6-8 hours, filtered, and dried at 5-7 Pa and 40-50° C. for 12-14 hours.

[0015] As an optimization, the purified bamboo lignin in step (2) is prepared by uniformly mixing bamboo alkali lignin with a sodium hydroxide aqueous solution having a molar concentration of 0.1 mol / L in a mass ratio of 1:(9-11), stirring at 10-30° C. and 300-500 r / min for 50-60 min, adjusting the pH to 3-3.2 with a hydrochloric acid aqueous solution having a mass fraction of 11-13%, centrifuging, washing the precipitate with deionized water for 3-5 times, and drying at 5-7 Pa and 50-60° C. for 7-8 h.

[0016] As an optimization, the 1,4-dioxane aqueous solution in step (2) is prepared by mixing deionized water and 1,4-dioxane in a volume ratio of 1:4-5.

[0017] As an optimization, the process parameters of the calendering molding in step (3) are: the pressure of the flat vulcanizer is 9-11 MPa, the temperature is 155-165°C, and the insulation time is 8-10 min.

[0018] As an optimization, the bamboo alkali lignin is derived from a kraft pulping process and purchased from Yibin Paper Co., Ltd.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] When preparing the degradable plastic, the present invention carries out melt polycondensation on diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol to obtain polyester; the polyester is reacted with 4-amino-2,2,6,6-tetramethylpiperidine to obtain modified polyester; the bamboo alkali lignin is purified and reacted with melamine to obtain pretreated bamboo lignin; the pretreated bamboo lignin is reacted with diethyl phosphite to obtain premodified bamboo lignin; the premodified bamboo lignin is reacted with 3-mercaptopropanol to obtain modified bamboo lignin; the modified polyester and the modified bamboo lignin are melt-plasticized and then calendered to obtain the degradable plastic.

[0021] Firstly, diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol are subjected to melt polycondensation to obtain polyester, aliphatic ester bonds and carbon-carbon double bonds are introduced into the main chain of the polyester molecule, and bromine atoms are introduced into the side chain; the aliphatic ester bonds introduced into the main chain of the polyester molecule are biodegradable and can give the degradable plastic excellent degradability; the carbon-carbon double bonds introduced into the main chain of the polyester molecule can undergo addition reaction with the thiol groups on the modified bamboo lignin to form a cross-linked network, inhibit the relative slip between the polyester molecular chains, and give the degradable plastic excellent mechanical properties; the polyester is reacted with 4-amino-2,2,6,6-tetramethylpiperidine to obtain the modified polyester, the bromine atoms on the side chain of the polyester molecule react with the amino groups on the 4-amino-2,2,6,6-tetramethylpiperidine, and a hindered amine structure is introduced into the side chain of the modified polyester molecule, and the introduction of the hindered amine structure can give the degradable plastic excellent anti-aging properties.

[0022] Secondly, the bamboo alkali lignin is purified and then reacted with melamine to obtain pretreated bamboo lignin; the pretreated bamboo lignin is reacted with diethyl phosphite to obtain premodified bamboo lignin; a large amount of phosphorus and nitrogen elements are introduced into the premodified bamboo lignin to give the biodegradable plastic excellent flame retardant properties; the premodified bamboo lignin is reacted with 3-mercaptopropanol to obtain modified bamboo lignin; the alcohol hydroxyl group on the mercaptopropanol is ester-exchanged with the phosphate bond on the premodified bamboo lignin to introduce a thiol group into the modified bamboo lignin, and the thiol group introduced into the modified bamboo lignin can undergo addition reaction with the carbon-carbon double bond on the modified polyester molecular chain to form a cross-linked network, thereby inhibiting the relative slip between the polyester molecular chains and giving the biodegradable plastic excellent mechanical properties.

[0023] Finally, the modified polyester and modified bamboo lignin are melt-plasticized and then calendered to produce degradable plastics. Bamboo lignin is a natural biomass material. After being discarded, it can be decomposed into carbon dioxide and water by microorganisms in nature, and then absorbed and utilized by plants, participating in the carbon cycle. It is biodegradable. Adding bamboo lignin to modified polyester can give the degradable plastics excellent degradable properties. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1

[0025] A method for preparing a degradable plastic, the method comprising the following steps:

[0026] (1) Diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol were mixed uniformly in a molar ratio of 1:0.4:1:0.4, tetrabutyl titanate (0.05 times the mass of diethyl terephthalate) was added, and the mixture was stirred at 175°C and 300 r / min for 3 h under a nitrogen atmosphere. The mixture was heated to 220°C and stirred at 3 Pa and 300 r / min for 8 h. The mixture was cooled to room temperature to obtain a crude product. The crude product was Mix evenly with chloroform at a mass ratio of 1:8 to completely dissolve the crude product, then add methanol 20 times the mass of the crude product and mix evenly, let stand for 6 hours, filter, and dry at 5Pa, 40°C for 14 hours to obtain polyester; mix polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform at a mass ratio of 1:0.4:0.4:20, stir at 45°C, 300r / min for 4 hours, and dry at 5Pa, 40°C for 24 hours to obtain modified polyester;

[0027] (2) Bamboo alkali lignin was mixed with a sodium hydroxide aqueous solution with a molar concentration of 0.1 mol / L in a mass ratio of 1:9, stirred at 10°C and 300 r / min for 60 min, adjusted to pH 3 with a hydrochloric acid aqueous solution with a mass fraction of 11%, centrifuged, washed precipitate with deionized water for 3 times, dried at 5 Pa and 50°C for 8 h, and purified bamboo lignin was obtained; deionized water and 1,4-dioxane were mixed in a volume ratio of 1:4 to prepare a 1,4-dioxane aqueous solution; purified bamboo lignin, melamine, and a 1,4-dioxane aqueous solution were mixed in a mass ratio of 1:0.3:9, acetic acid (1.4 times the mass of purified bamboo lignin) and a formaldehyde aqueous solution (35% mass fraction) (0.2 times the mass of purified bamboo lignin) were added, stirred at 55°C and 300 r / min for 5 h, and purified bamboo lignin was added. The pretreated bamboo lignin, diethyl phosphite, formaldehyde and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.2:0.1:9, the pH value was adjusted to 4.9 with a hydrochloric acid aqueous solution with a mass fraction of 11%, the mixture was stirred at 65°C and 300r / min for 5h, and the mixture was dried at 5Pa and 50°C for 8h to obtain pre-modified bamboo lignin; the pre-modified bamboo lignin, 3-mercaptopropanol, p-toluenesulfonic acid and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.4:0.03:12, the mixture was stirred at 120°C and 300r / min for 5h, and the mixture was centrifuged, the precipitate was washed with deionized water for 3 times, and the mixture was dried at 5Pa and 50°C for 8h to obtain modified bamboo lignin;

[0028] (3) The modified polyester and modified bamboo lignin were added into an internal mixer at a mass ratio of 1:0.2, stirred at 150°C and 300 r / min for 10 min, and then 0.01 times the mass of azobisisobutyronitrile of the modified polyester was added and mixed evenly. The mixture was placed on a flat vulcanizer for calendering. The pressure of the flat vulcanizer was set to 9 MPa and the temperature was set to 155°C. The mixture was kept warm for 10 min and pressed into a film with a thickness of 0.9 mm to obtain a biodegradable plastic. Example 2

[0029] A method for preparing a degradable plastic, the method comprising the following steps:

[0030] (1) Diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol were mixed uniformly in a molar ratio of 1:0.5:1:0.5, tetrabutyl titanate (0.06 times the mass of diethyl terephthalate) was added, and the mixture was stirred at 180°C and 400 r / min for 2.5 h under a nitrogen atmosphere. The mixture was heated to 225°C and stirred at 4 Pa ​​and 400 r / min for 7 h. The mixture was cooled to room temperature to obtain a crude product. The crude product was Mix evenly with chloroform at a mass ratio of 1:9 to completely dissolve the crude product, then add methanol 25 times the mass of the crude product and mix evenly, let stand for 7 hours, filter, and dry at 6Pa, 45°C for 13 hours to obtain polyester; mix polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform at a mass ratio of 1:0.5:0.5:22, stir at 50°C, 400r / min for 3.5 hours, and dry at 6Pa, 45°C for 22 hours to obtain modified polyester;

[0031] (2) Bamboo alkali lignin was mixed with a sodium hydroxide aqueous solution with a molar concentration of 0.1 mol / L in a mass ratio of 1:10, stirred at 20°C and 400 r / min for 55 min, adjusted to pH 3.1 with a 12% hydrochloric acid aqueous solution, centrifuged, washed precipitate with deionized water 4 times, dried at 6 Pa and 55°C for 7.5 h, and purified bamboo lignin was obtained; deionized water and 1,4-dioxane were mixed in a volume ratio of 1:4.5 to prepare a 1,4-dioxane aqueous solution; purified bamboo lignin, melamine, and a 1,4-dioxane aqueous solution were mixed in a mass ratio of 1:0.35:10, 1.5 times the mass of purified bamboo lignin acetic acid and 0.25 times the mass of purified bamboo lignin 36% formaldehyde aqueous solution were added, stirred at 60°C and 400 r / min for 4.5 h, and purified bamboo lignin was added. The pretreated bamboo lignin, diethyl phosphite, formaldehyde and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.25:0.15:10, the pH value was adjusted to 5.0 with a 12% hydrochloric acid aqueous solution, the mixture was stirred at 70°C and 400r / min for 4.5h, and the mixture was dried at 6Pa and 55°C for 7.5h to obtain pre-modified bamboo lignin; the pre-modified bamboo lignin, 3-mercaptopropanol, p-toluenesulfonic acid and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.5:0.04:13, the mixture was stirred at 125°C and 400r / min for 4.5h, and the mixture was centrifuged, the precipitate was washed 4 times with deionized water, and the mixture was dried at 6Pa and 55°C for 7.5h to obtain modified bamboo lignin;

[0032] (3) The modified polyester and modified bamboo lignin were added into an internal mixer at a mass ratio of 1:0.25, stirred at 155°C and 400 r / min for 9 min, and then 0.02 times the mass of azobisisobutyronitrile of the modified polyester was added and mixed evenly. The mixture was placed on a flat vulcanizer for calendering. The pressure of the flat vulcanizer was set to 10 MPa and the temperature was set to 160°C. The mixture was kept warm for 9 min and pressed into a film with a thickness of 1.0 mm to obtain a biodegradable plastic. Example 3

[0033] A method for preparing a degradable plastic, the method comprising the following steps:

[0034] (1) Diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol were mixed uniformly in a molar ratio of 1:0.6:1:0.6, tetrabutyl titanate (0.07 times the mass of diethyl terephthalate) was added, and the mixture was stirred at 185°C and 500 r / min for 2 h under a nitrogen atmosphere. The mixture was heated to 230°C and stirred at 5 Pa and 500 r / min for 6 h. The mixture was cooled to room temperature to obtain a crude product. The crude product was mixed with Chloroform was mixed evenly at a mass ratio of 1:10 to completely dissolve the crude product, and then methanol 30 times the mass of the crude product was added and mixed evenly, allowed to stand for 8 hours, filtered, and dried at 7Pa, 50°C for 12 hours to obtain polyester; polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform were mixed evenly at a mass ratio of 1:0.6:0.6:24, stirred at 55°C, 500r / min for 3 hours, and dried at 7Pa, 50°C for 20 hours to obtain modified polyester;

[0035] (2) Bamboo alkali lignin was mixed with a sodium hydroxide aqueous solution with a molar concentration of 0.1 mol / L in a mass ratio of 1:11, stirred at 30°C and 500 r / min for 50 min, adjusted to pH 3.2 with a 13% hydrochloric acid aqueous solution, centrifuged, washed 5 times with deionized water, and dried at 7 Pa and 60°C for 7 h to obtain purified bamboo lignin; deionized water and 1,4-dioxane were mixed in a volume ratio of 1:5 to prepare a 1,4-dioxane aqueous solution; purified bamboo lignin, melamine, and a 1,4-dioxane aqueous solution were mixed in a mass ratio of 1:0.4:11, 1.6 times the mass of purified bamboo lignin acetic acid and 0.3 times the mass of purified bamboo lignin A 37% formaldehyde aqueous solution were added, stirred at 65°C and 500 r / min for 4 h, and purified bamboo was added. The pretreated bamboo lignin was prepared by mixing the pretreated bamboo lignin with deionized water 30 times the mass of lignin, centrifuging, and drying the precipitate at 7Pa and 55°C for 6 hours; the pretreated bamboo lignin, diethyl phosphite, formaldehyde, and N,N-dimethylformamide were mixed at a mass ratio of 1:0.3:0.2:11, adjusting the pH to 5.1 with a 13% hydrochloric acid aqueous solution, stirring at 75°C and 500r / min for 4 hours, and drying at 7Pa and 60°C for 7 hours to obtain pre-modified bamboo lignin; the pre-modified bamboo lignin, 3-mercaptopropanol, p-toluenesulfonic acid, and N,N-dimethylformamide were mixed at a mass ratio of 1:0.5:0.04:14, stirring at 130°C and 500r / min for 4 hours, centrifuging, washing the precipitate with deionized water for 5 times, and drying at 7Pa and 60°C for 7 hours to obtain modified bamboo lignin;

[0036] (3) The modified polyester and modified bamboo lignin were added into an internal mixer at a mass ratio of 1:0.3, stirred at 160°C and 500 r / min for 8 min, and then 0.03 times the mass of azobisisobutyronitrile of the modified polyester was added and mixed evenly. The mixture was placed on a flat vulcanizer for calendering. The pressure of the flat vulcanizer was set to 11 MPa and the temperature was set to 165°C. The mixture was kept warm for 10 min and pressed into a film with a thickness of 1.1 mm to obtain a biodegradable plastic.

[0037] Comparative Example 1

[0038] The difference between the preparation method of the degradable plastic of Comparative Example 1 and Example 2 lies in the difference in step (1). Step (1) is modified as follows: diethyl terephthalate, diethyl adipate, 1,4-butanediol and 1,4-butene glycol are mixed uniformly in a molar ratio of 1:0.5:1:0.5, tetrabutyl titanate with a mass of 0.06 times that of diethyl terephthalate is added, and the mixture is stirred at 180°C and 400 r / min for 2.5 h under a nitrogen atmosphere, and the mixture is heated to 225°C and stirred at 4 Pa ​​and 400 r / min for 7 h. , cooled to room temperature to obtain a crude product, the crude product and chloroform were mixed evenly at a mass ratio of 1:9 to completely dissolve the crude product, and then methanol 25 times the mass of the crude product was added to mix evenly, allowed to stand for 7 hours, filtered, and dried at 6Pa, 45°C for 13 hours to obtain polyester; polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform were mixed evenly at a mass ratio of 1:0.5:0.5:22, stirred at 50°C, 400r / min for 3.5 hours, and dried at 6Pa, 45°C for 22 hours to obtain modified polyester. The remaining steps are the same as in Example 2.

[0039] Comparative Example 2

[0040] The preparation method of the degradable plastic of Comparative Example 2 is different from that of Example 2 in that step (1) is different. Step (1) is modified as follows: diethyl terephthalate, 1,4-butanediol and 1,4-butenediol are mixed uniformly in a molar ratio of 1:0.5:0.5, tetrabutyl titanate in an amount of 0.06 times the mass of diethyl terephthalate is added, and the mixture is stirred at 180°C and 400 r / min for 2.5 h under a nitrogen atmosphere, and the mixture is heated to 225°C, and the mixture is stirred at 4 Pa ​​and 400 r / min for 7 h, and then cooled to room temperature. The crude product was mixed with chloroform at a mass ratio of 1:9 to make the crude product completely dissolved, and then methanol 25 times the mass of the crude product was added to mix evenly, and the mixture was allowed to stand for 7 hours, filtered, and dried at 6Pa, 45°C for 13 hours to obtain polyester; polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform were mixed evenly at a mass ratio of 1:0.5:0.5:22, stirred at 50°C, 400r / min for 3.5 hours, and dried at 6Pa, 45°C for 22 hours to obtain modified polyester. The remaining steps are the same as those in Example 2.

[0041] Comparative Example 3

[0042] The preparation method of the degradable plastic of Comparative Example 3 is different from that of Example 2 only in step (1). Step (1) is modified as follows: diethyl terephthalate, dimethyl 2,5-dibromoadipate and 1,4-butanediol are mixed uniformly in a molar ratio of 1:0.5:1.5, tetrabutyl titanate with a mass of 0.06 times that of diethyl terephthalate is added, and the mixture is stirred at 180°C and 400 r / min for 2.5 h under a nitrogen atmosphere, and the mixture is heated to 225°C, and the mixture is stirred at 4 Pa ​​and 400 r / min for 7 h, and then cooled. Cool to room temperature to obtain a crude product, mix the crude product with chloroform at a mass ratio of 1:9 to dissolve the crude product completely, add 25 times the mass of methanol to mix evenly, let stand for 7 hours, filter, and dry at 6Pa, 45°C for 13 hours to obtain polyester; mix polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform at a mass ratio of 1:0.5:0.5:22, stir at 50°C, 400r / min for 3.5 hours, and dry at 6Pa, 45°C for 22 hours to obtain modified polyester. The remaining steps are the same as in Example 2.

[0043] Comparative Example 4

[0044] The preparation method of the degradable plastic of Comparative Example 4 is different from that of Example 2 only in step (1). Step (1) is modified as follows: diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol are mixed uniformly in a molar ratio of 1:0.5:1:0.5, tetrabutyl titanate (0.06 times the mass of diethyl terephthalate) is added, and the mixture is stirred at 180°C and 400 r / min for 2.5 h under a nitrogen atmosphere, and the mixture is heated to 225°C, and the mixture is stirred at 4 Pa ​​and 400 r / min for 7 h, and the mixture is cooled to room temperature to obtain a crude product, and the crude product is mixed uniformly with chloroform in a mass ratio of 1:9 to completely dissolve the crude product, and then methanol (25 times the mass of the crude product) is added to mix the mixture uniformly, and the mixture is allowed to stand for 7 h, filtered, and dried at 6 Pa and 45°C for 13 h to obtain a modified polyester. The remaining steps are the same as those of Example 2.

[0045] Comparative Example 5

[0046] The preparation method of the degradable plastic of Comparative Example 5 differs from that of Example 2 only in step (2), where step (2) is modified as follows: bamboo alkali lignin and a sodium hydroxide aqueous solution having a molar concentration of 0.1 mol / L are uniformly mixed at a mass ratio of 1:10, stirred at 20° C. and 400 r / min for 55 min, the pH value is adjusted to 3.1 with a hydrochloric acid aqueous solution having a mass fraction of 12%, centrifuged, the precipitate is washed 4 times with deionized water, and dried at 6 Pa and 55° C. for 7.5 h to obtain modified bamboo lignin. The remaining steps are the same as those of Example 2.

[0047] Comparative Example 6

[0048] The preparation method of the degradable plastic of Comparative Example 6 is different from that of Example 2 in that step (2) is not performed, and step (3) is modified as follows: adding the modified polyester to an internal mixer, stirring at 155° C. and 400 r / min for 9 min, placing it on a flat vulcanizer for calendering, setting the pressure of the flat vulcanizer to 10 MPa and the temperature to 160° C., keeping the temperature for 9 min, pressing it into a film with a thickness of 1.0 mm, and preparing the degradable plastic. The remaining steps are the same as those of Example 2.

[0049] Test Example 1

[0050] Flame retardant performance test

[0051] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T2406.2, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 1.

[0052] Table 1

[0053]

[0054] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the degradable plastics prepared by the present invention have good flame retardant properties.

[0055] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Examples 4 to 5, indicating that the bamboo alkali lignin is purified and then reacted with melamine to obtain pretreated bamboo lignin; the pretreated bamboo lignin is reacted with diethyl phosphite to obtain pre-modified bamboo lignin; and a large amount of phosphorus and nitrogen elements are introduced into the pre-modified bamboo lignin, giving the degradable plastic excellent flame retardant properties.

[0056] Test Example 2

[0057] Testing of mechanical properties and anti-aging properties

[0058] Test method: The tensile strength of the embodiment and the comparative example was tested on an electronic universal testing machine according to GB / T1040.3, and then the unstretched original sample was irradiated with a xenon arc lamp for 72 hours. The tensile strength of the embodiment and the comparative example after ultraviolet aging treatment was tested on an electronic universal testing machine according to GB / T1040.3, and the change rate of the tensile strength of the embodiment and the comparative example before and after ultraviolet aging treatment was calculated, tensile strength change rate = (tensile strength after ultraviolet aging treatment / original tensile strength of sample) × 100%. The results are shown in Table 2.

[0059] Table 2

[0060]

[0061] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the degradable plastics prepared by the present invention have good mechanical properties and anti-aging properties.

[0062] By comparison, the tensile strength of Examples 1 to 3 is greater than that of Comparative Example 3, indicating that polyester is prepared by melt polycondensation of diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol, and 1,4-butenediol, and carbon-carbon double bonds are introduced into the main chain of the polyester molecule. The carbon-carbon double bonds introduced into the main chain of the polyester molecule can react with the thiol groups on the modified bamboo lignin to form a cross-linked network, thereby inhibiting the relative slip between the polyester molecular chains and giving the degradable plastic excellent mechanical properties.

[0063] By comparison, the tensile strength of Examples 1 to 3 is greater than that of Comparative Examples 4 to 5, indicating that the bamboo alkali lignin is purified and then reacted with melamine to obtain pretreated bamboo lignin; the pretreated bamboo lignin is reacted with diethyl phosphite to obtain premodified bamboo lignin; the premodified bamboo lignin is reacted with 3-mercaptopropanol to obtain modified bamboo lignin; the alcoholic hydroxyl groups on the mercaptopropanol are ester-exchanged with the phosphate bonds on the premodified bamboo lignin to introduce thiol groups on the modified bamboo lignin, and the thiol groups introduced on the modified bamboo lignin can undergo addition reaction with the carbon-carbon double bonds on the modified polyester molecular chains to form a cross-linked network, thereby inhibiting the relative slip between the polyester molecular chains and giving the degradable plastic excellent mechanical properties.

[0064] By comparison, the change rate of tensile strength of Examples 1 to 3 is smaller than that of Comparative Examples 1, 2 and 4, indicating that polyester is prepared by melt polycondensation of diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol, and bromine atoms are introduced into the side chains of polyester molecules; the bromine atoms on the side chains of polyester molecules react with the amino groups on 4-amino-2,2,6,6-tetramethylpiperidine to introduce hindered amine structures into the side chains of modified polyester molecules, and the introduction of hindered amine structures can give the degradable plastics excellent anti-aging properties.

[0065] Test Example 3

[0066] Degradability testing

[0067] Test method: Cut the examples and comparative examples into 100×30 mm 2 The samples were weighed and recorded as m1. The samples were placed in glass jars containing 400 ml of phosphate PBS buffer solution (PH = 7.4), in which the lipase activity was 15000u / g and the enzyme concentration in the solution was 18u / ml. The enzyme degradation experiment was carried out in a 37°C constant temperature drying oven. After 1 month, the samples were taken out, washed with distilled water 5 times, and vacuum dried at 37°C for 3 days. The weight was recorded as m2, and the degradation rate of the samples was (m1-m2) / m1×100%. The results are shown in Table 3.

[0068] Table 3

[0069]

[0070] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 3, it can be found that the degradable plastics prepared by the present invention have good degradability.

[0071] By comparison, the degradation rates of Examples 1 to 3 are greater than that of Comparative Example 2, indicating that polyester is prepared by melt polycondensation of diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol, and aliphatic ester bonds are introduced into the main chain of the polyester molecule. The aliphatic ester bonds introduced into the main chain of the polyester molecule are biodegradable and can give the degradable plastic excellent degradable properties.

[0072] By comparison, the degradation rates of Examples 1 to 3 are greater than that of Comparative Example 6. Bamboo lignin is a natural biomass material. After being discarded, it can be decomposed into carbon dioxide and water by microorganisms in nature, and then absorbed and utilized by plants, participating in the carbon cycle, and has biodegradability. The degradable plastic obtained by adding bamboo lignin to modified polyester, melt plasticizing, and calendering can give the degradable plastic excellent degradable properties.

[0073] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A degradable plastic, characterized in that: The degradable plastic is prepared by reacting polyester with 4-amino-2,2,6,6-tetramethylpiperidine to obtain modified polyester; reacting pre-modified bamboo lignin with 3-mercaptopropanol to obtain modified bamboo lignin; and calendering the modified polyester and the modified bamboo lignin after melt plasticization. The polyester is prepared by melt polycondensation of diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol; The pre-modified bamboo lignin is prepared by reacting pre-treated bamboo lignin with diethyl phosphite; The pretreated bamboo lignin is prepared by reacting the purified bamboo alkali lignin with melamine.

2. A method for preparing a degradable plastic, characterized in that: The method comprises the following preparation steps: (1) Diethyl terephthalate, dimethyl 2,5-dibromoadipate, 1,4-butanediol and 1,4-butenediol were mixed in a molar ratio of 1:(0.4-0.6):1:(0.4-0.6), and tetrabutyl titanate (0.05-0.07 times the mass of diethyl terephthalate) was added. In a nitrogen atmosphere, the mixture was stirred at 175-185°C and 300-500 r / min for 2-3 h. The mixture was heated to 220-230°C and heated at 3-5 Pa and 300-50 0r / min, continue stirring the reaction for 6-8h, cool to room temperature to obtain a crude product, and purify the crude product to obtain polyester; mix polyester, 4-amino-2,2,6,6-tetramethylpiperidine, triethylamine, and chloroform in a mass ratio of 1:(0.4-0.6):(0.4-0.6):(20-24), stir and react at 45-55°C, 300-500r / min for 3-4h, and dry at 5-7Pa, 40-50°C for 20-24h to obtain modified polyester; (2) Purified bamboo lignin, melamine, and 1,4-dioxane aqueous solution were mixed at a mass ratio of 1:(0.3-0.4):(9-11), and acetic acid (1.4-1.6 times the mass of purified bamboo lignin) and formaldehyde aqueous solution (35-37% by mass) (0.2-0.3 times the mass of purified bamboo lignin) were added, and the mixture was stirred at 55-65°C and 300-500 r / min for 4-5 h. Deionized water (20-30 times the mass of purified bamboo lignin) was added and mixed evenly, and the mixture was centrifuged. The precipitate was dried at 5-7 Pa and 45-55°C for 6-7 h to obtain pretreated bamboo lignin. Pretreated bamboo lignin, diethyl phosphite, formaldehyde, and N,N-dimethylformamide were mixed at a mass ratio of 1:(0.2-0.3):(0.1-0 .2):(9~11) are mixed evenly, and the pH value is adjusted to 4.9~5.1 with a hydrochloric acid aqueous solution with a mass fraction of 11~13%, and the mixture is stirred at 65~75℃ and 300~500r / min for 4~5h, and dried at 5~7Pa and 50~60℃ for 7~8h to obtain pre-modified bamboo lignin; the pre-modified bamboo lignin, 3-mercaptopropanol, p-toluenesulfonic acid, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(0.4~0.6):(0.03~0.05):(12~14), and the mixture is stirred at 120~130℃ and 300~500r / min for 4~5h, and centrifuged, and the precipitate is washed with deionized water for 3~5 times, and dried at 5~7Pa and 50~60℃ for 7~8h to obtain modified bamboo lignin; (3) Add the modified polyester and modified bamboo lignin in a mass ratio of 1:(0.2~0.3) into an internal mixer, stir at 150~160℃ and 300~500r / min for 8~10min, then add 0.01~0.03 times the mass of azobisisobutyronitrile of the modified polyester, mix well, place on a flat vulcanizer for calendering, and press into a film with a thickness of 0.9~1.1mm to obtain a biodegradable plastic.

3. The method for preparing a degradable plastic according to claim 2, characterized in that: The purification process of the crude product in step (1) is as follows: the crude product is mixed evenly with chloroform in a mass ratio of 1:(8-10) to completely dissolve the crude product, and then 20-30 times the mass of methanol of the crude product is added to mix evenly, allowed to stand for 6-8 hours, filtered, and dried at 5-7 Pa, 40-50° C. for 12-14 hours.

4. The method for preparing a degradable plastic according to claim 2, characterized in that: The purified bamboo lignin in step (2) is prepared by uniformly mixing bamboo alkali lignin with a sodium hydroxide aqueous solution having a molar concentration of 0.1 mol / L in a mass ratio of 1:(9-11), stirring at 10-30° C. and 300-500 r / min for 50-60 min, adjusting the pH to 3-3.2 with a hydrochloric acid aqueous solution having a mass fraction of 11-13%, centrifuging, washing the precipitate with deionized water for 3-5 times, and drying at 5-7 Pa and 50-60° C. for 7-8 h.

5. The method for preparing a degradable plastic according to claim 2, characterized in that: The 1,4-dioxane aqueous solution in step (2) is prepared by mixing deionized water and 1,4-dioxane in a volume ratio of 1:4-5.

6. The method for preparing a degradable plastic according to claim 2, characterized in that: The process parameters of the calendering molding in step (3) are: the pressure of the flat vulcanizing machine is 9-11 MPa, the temperature is 155-165° C., and the insulation time is 8-10 min.

Citation Information

Patent Citations

  • Stabilized thermoplastic copolyesters

    CN101755000A

  • Unsaturated aliphatic-aromatic-polylactic acid block copolymer

    CN105622911A