Preparation method and application of pH-reversible polysaccharide-based double-layer emulsion
The pH reversible polysaccharide double-layer emulsion prepared in a high-speed homogenizer solves the problem of low stability of the oil-in-water double-layer emulsion, and realizes droplet wrinkle recovery under pH adjustment, and has good results. The ion permeability and encapsulation function are suitable for biomimetic biomaterials.
Patent Information
- Application Number
- CN202411014929.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing oil-in-water (O/W/W) double-layer emulsion has low stability and is susceptible to pH values, resulting in irreversible damage to the structure.
Carboxy polysaccharide, chitosan and soybean oil were used for shear preparation in a high-speed homogenizer to form a polysaccharide bilayer emulsion with reversible pH. By adjusting the pH value from 5 to 11, the droplets were crimped and returned to 5. Return to normal.
It has achieved high stability and structural restorability of a polysaccharide-based bilayer emulsion with reversible pH, possesses good ion permeability and elasticity, is suitable for the encapsulation and delivery of hydrophilic substances, and has great potential in biomimetic biomaterials.
Smart Images

Figure CN119039617A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of emulsion gel preparation, and relates to a preparation method of a pH-reversible polysaccharide-based double-layer emulsion and application thereof. Background Art
[0002] Double emulsions are defined as one emulsion in the form of a dispersed phase in another emulsion, which means that oil-in-water (W / O) or water-in-oil (O / W) emulsions can be further homogenized in water and oil, respectively. Due to their unique properties, such as simultaneous encapsulation of hydrophilic and lipophilic active compounds, delaying oxidation reactions, masking flavors, inhibiting the release of undesirable ingredients, and producing low-fat products, double emulsions have attracted widespread attention in the food industry; double emulsions are mainly divided into two types: water-in-oil-in-water (W / O / W) and oil-in-water-in-oil (O / W / O). In fact, water-in-water-in-oil (O / W / W) emulsions are also a type of double emulsion. However, to the best of our knowledge, there is little information on O / W / W double emulsions.
[0003] Oil-in-water-in-water (O / W / W) is a type of double-layer emulsion, which is generally prepared by dispersing an O / W emulsion in a water-in-water emulsion (W / W) system, wherein the water-in-water (W / W) emulsion is the basis for preparing the oil-in-water-in-water (O / W / W). The water-in-water (W / W) emulsion system is formed by phase separation, wherein the phase separation process can be divided into combined phase separation or separated phase separation. At present, the preparation of oil-in-water-in-water (O / W / W) double-layer emulsion is mainly based on the separated phase separation process of the water-in-water (W / W) emulsion system, and its formation process is mainly to first form a water-in-water emulsion through two thermally incompatible macromolecules, and then add oil or oil-in-water primary emulsion for further homogenization to obtain an O / W / W double-layer emulsion. In the prior art, an O / W / W double emulsion is prepared by mixing an oil-in-water emulsion with a heat-incompatible whey protein isolate and a pectin solution; and an O / W / W double emulsion is formed by dispersing sunflower oil in a heat-incompatible mixed system of skim milk powder and guar gum, and homogenizing. However, the O / W / W double emulsion prepared by phase separation is usually less stable, and it is often necessary to select a high concentration of materials to reduce the fluidity of the continuous phase and the dispersed phase, or to add additional cross-linking agents such as enzymes or metal ions to construct a continuous phase gel, or to add particles or linear polymers to stabilize the emulsion interface. In recent years, O / W / W double emulsions have also been prepared by a combined phase separation method, where two hydrophilic polymers with opposite charges attract each other to form a precipitate or aggregate, so that the electrostatic polymer and water are separated from the two residual polymers, but this electrostatically interacting emulsion system is easily affected by pH and irreversibly destroyed, so it is of great significance to develop a pH-reversible oil-in-water-in-water (O / W / W) double emulsion. Summary of the invention
[0004] In view of the technical problem that the above-mentioned emulsion system is easily affected by pH, the present invention provides a preparation method of a pH-reversible polysaccharide-based double-layer emulsion and its application.
[0005] The invention uses carboxyl polysaccharide, chitosan and soybean oil as raw materials, and shears them in a high-speed homogenizer to prepare a polysaccharide-based double-layer emulsion with pH reversible high stability and structural recoverability.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a pH-reversible polysaccharide-based double-layer emulsion comprises the following steps:
[0008] S1. Solution preparation
[0009] Taking chitosan powder and carboxyl polysaccharide powder respectively, and preparing chitosan solution and carboxyl polysaccharide solution respectively;
[0010] S2. Preparation of polysaccharide-based primary emulsion
[0011] Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution; and shear the mixed solution in a high-speed homogenizer to obtain a polysaccharide-based primary emulsion; the volume of the soybean oil is 20% to 40% of the volume of the mixed solution, and the mass concentration of the chitosan solution is 3% to 5%;
[0012] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0013] After mixing the polysaccharide-based primary emulsion of step S2 with the carboxyl polysaccharide solution of step S1, the obtained mixture is sheared in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion; the volume of the polysaccharide-based primary emulsion is 10% to 50% of the volume of the mixture; and the mass concentration of the carboxyl polysaccharide solution is 1% to 2%.
[0014] It is further defined that in step S1, the preparation process of the chitosan solution is: adding chitosan powder to water, then adding acetic acid aqueous solution, mixing and standing for 12h to 24h; the volume of the acetic acid aqueous solution is 1% of the volume of water.
[0015] It is further defined that in step S1, the preparation process of the carboxyl polysaccharide solution is: adding carboxymethyl cellulose powder into boiling water and dissolving it for 20 minutes to 40 minutes, and then letting it stand for 12 hours to 24 hours.
[0016] It is further defined that the carboxyl polysaccharide is carboxymethyl cellulose, sodium alginate or pectin.
[0017] It is further defined that in step S2, the shearing is performed at a rotation speed of 11500 r / min to 14500 r / min for 2 min to 3 min.
[0018] It is further defined that in step S3, the shearing is performed at a rotation speed of 11500 r / min to 14500 r / min for 1 min to 2 min.
[0019] The pH-reversible polysaccharide-based double-layer emulsion is prepared by utilizing the method for preparing the pH-reversible polysaccharide-based double-layer emulsion.
[0020] It is further defined that when the pH of the pH-reversible polysaccharide-based double-layer emulsion is adjusted from 5 to 11, the double-layer emulsion droplets shrink and become smaller; when the pH is adjusted from 11 to 5, the size of the double-layer emulsion droplets returns to normal.
[0021] The application of the pH-reversible polysaccharide-based double-layer emulsion in the co-encapsulation of hydrophilic and hydrophobic substances.
[0022] Application of pH-reversible polysaccharide-based double-layer emulsion in biomimetic biomaterials.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The pH-reversible polysaccharide-based double-layer emulsion prepared by the present invention has good pH reversibility. When the double-layer emulsion droplets are adjusted from acidic conditions (pH=5) to alkaline conditions (pH=11), the double-layer emulsion droplets will shrink significantly and become smaller. When the pH is readjusted to 5, the size of the double-layer emulsion droplets returns to normal.
[0025] 2. The pH-reversible polysaccharide-based emulsion prepared by the present invention also has the function of simultaneously encapsulating and delivering hydrophilic and hydrophobic substances. In terms of refolding and stability, its emulsion interface film has good ion permeability and elasticity, and has great potential as a biomimetic biomaterial.
[0026] 3. The present invention uses chitosan and carboxyl polysaccharide as green materials, which are safe and edible, have a wide range of sources, are biodegradable, and are environmentally friendly.
[0027] 4. The preparation method of the present invention is simple, has low production cost and high production efficiency, and is suitable for industrial promotion and application in the food field. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The infrared absorption spectra of pH-reversible polysaccharide-based double-layer emulsions in different treatment groups (10%-50%);
[0029] Figure 2The microscopic morphology of pH-reversible polysaccharide-based double-layer emulsions in different treatment groups (10%-50%), where the scale bar is 100 μm;
[0030] Figure 3 The rheological properties of pH-reversible polysaccharide-based bilayer emulsions in different treatment groups (10%-50%);
[0031] Figure 4 The stability diagram of pH-reversible polysaccharide-based bilayer emulsions in different treatment groups (10%-50%);
[0032] Figure 5 The microscopic morphology of pH-reversible polysaccharide-based double-layer emulsions in different treatment groups at pH = 5 (10%-40%), where the scale bar is 100 μm;
[0033] Figure 6 The microscopic morphology of pH-reversible polysaccharide-based double-layer emulsions in different treatment groups at pH = 11 (10%-40%), where the scale bar is 100 μm;
[0034] Figure 7 Microscopic morphology of pH-reversible polysaccharide-based double-layer emulsions in different treatment groups when the pH was readjusted to 5 (10%-40%), where the scale bar is 100 μm. DETAILED DESCRIPTION
[0035] The technical solution protected by the present invention is described in detail below with reference to the accompanying drawings. Although the drawings show specific embodiments of the present disclosure, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein.
[0036] The present invention provides a method for preparing a pH-reversible polysaccharide-based double-layer emulsion, comprising the following steps:
[0037] S1. Solution preparation
[0038] Chitosan powder and carboxyl polysaccharide powder are taken respectively to prepare chitosan solution and carboxyl polysaccharide solution respectively.
[0039] In step S1, the preparation process of chitosan solution is: chitosan powder is added to water, and then acetic acid aqueous solution is added, mixed and allowed to stand for 12h to 24h; the volume of acetic acid aqueous solution is 1% of the volume of water.
[0040] In step S1, the preparation process of the carboxyl polysaccharide solution is: adding the carboxyl polysaccharide powder into boiling water and dissolving it for 20 minutes to 40 minutes, and then standing it for 12 hours to 24 hours.
[0041] In the present invention, the carboxyl polysaccharide is carboxymethyl cellulose, sodium alginate or pectin.
[0042] S2. Preparation of polysaccharide-based primary emulsion
[0043] Add soybean oil to the chitosan solution in step S1, mix well to obtain a mixed solution; and shear the mixed solution in a high-speed homogenizer to obtain a polysaccharide-based primary emulsion.
[0044] In step S2 of the present invention, the volume of soybean oil is 20% to 40% of the volume of the mixed solution, and the mass concentration of the chitosan solution is 3% to 5%.
[0045] Preferably, the volume of soybean oil is 20% of the volume of the mixed solution, and the mass concentration of the chitosan solution is 3%.
[0046] In step S2 of the present invention, the shearing is performed at a rotation speed of 11500 r / min to 14500 r / min for 2 min to 3 min.
[0047] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0048] The polysaccharide-based primary emulsion of step S2 is mixed with the carboxyl polysaccharide solution of step S1, and then sheared in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion.
[0049] In the steps of the present invention, the volume of the polysaccharide-based primary emulsion is 10% to 50% of the volume of the mixture; and the mass concentration of the carboxyl polysaccharide is 1% to 2%.
[0050] Preferably, the mass concentration of the carboxyl polysaccharide solution is 1.5%.
[0051] In step S3 of the present invention, the shearing is performed at a rotation speed of 11500 r / min to 14500 r / min for 1 min to 2 min.
[0052] The pH-reversible polysaccharide-based double-layer emulsion prepared by the method for preparing the pH-reversible polysaccharide-based double-layer emulsion of the present invention has great potential application value in pH response and as a biomimetic biomaterial, in that when the pH is adjusted from 5 to 11, the double-layer emulsion droplets shrink and become smaller; when the pH is adjusted from 11 to 5, the size of the double-layer emulsion droplets returns to normal.
[0053] The technical advantages of the polysaccharide-based water-in-water emulsion gel prepared by the present invention are described below through several groups of implementation methods and performance tests.
[0054] It should be noted that, unless otherwise specified, the reagents, drugs, instruments, etc. used in the following examples are all conventional products in the field purchased from the market.
[0055] Example 1
[0056] The present embodiment provides a method for preparing a pH-reversible polysaccharide-based double-layer emulsion, comprising the following steps:
[0057] S1. Solution preparation
[0058] Chitosan powder and carboxymethyl cellulose powder are taken respectively to prepare chitosan solution and carboxymethyl cellulose solution respectively.
[0059] In step S1, the preparation process of chitosan solution is: adding chitosan powder to water, then adding acetic acid aqueous solution, mixing and standing for 12 hours; the volume of acetic acid aqueous solution is 1% of the volume of water; the mass concentration of chitosan solution is 3%.
[0060] In step S1, the preparation process of the carboxymethyl cellulose solution is: adding carboxymethyl cellulose powder into boiling water and dissolving it for 30 minutes, and then standing for 12 hours to fully dissolve, to obtain a carboxymethyl cellulose solution with a mass concentration of 1.5%.
[0061] S2. Preparation of polysaccharide-based primary emulsion
[0062] Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution, wherein the volume of soybean oil is 20% of the volume of the mixed solution; and shear the mixed solution in a high-speed homogenizer at a speed of 11500r / min for 2min to obtain a polysaccharide-based primary emulsion.
[0063] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0064] The polysaccharide-based primary emulsion of step S2 and the carboxymethyl cellulose solution of step S1 are mixed, wherein the volume of the polysaccharide-based primary emulsion accounts for 10% of the total volume of the solution, and the total volume of the solution refers to the total volume of the polysaccharide-based primary emulsion and the carboxymethyl cellulose solution; the mixed solution is sheared for 1 minute at a speed of 11500 r / min in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion.
[0065] Example 2
[0066] The present embodiment provides a method for preparing a pH-reversible polysaccharide-based double-layer emulsion, comprising the following steps:
[0067] S1. Solution preparation
[0068] Chitosan powder and carboxymethyl cellulose powder are taken respectively to prepare chitosan solution and carboxymethyl cellulose solution respectively.
[0069] In step S1, the preparation process of chitosan solution is: adding chitosan powder to water, then adding acetic acid aqueous solution, mixing and standing for 12 hours; the volume of acetic acid aqueous solution is 1% of the volume of water; the mass concentration of chitosan solution is 3%.
[0070] In step S1, the preparation process of the carboxymethyl cellulose solution is: adding carboxymethyl cellulose powder into boiling water and dissolving it for 30 minutes, and then standing for 12 hours to fully dissolve, to obtain a carboxymethyl cellulose solution with a mass concentration of 1.5%.
[0071] S2. Preparation of polysaccharide-based primary emulsion
[0072] Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution, wherein the volume of soybean oil is 20% of the volume of the mixed solution; and shear the mixed solution in a high-speed homogenizer at a speed of 11500r / min for 2min to obtain a polysaccharide-based primary emulsion.
[0073] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0074] The polysaccharide-based primary emulsion of step S2 and the carboxymethyl cellulose solution of step S1 are mixed, wherein the volume of the polysaccharide-based primary emulsion accounts for 20% of the total volume of the solution, and the total volume of the solution refers to the total volume of the polysaccharide-based primary emulsion and the carboxymethyl cellulose solution; the mixed solution is sheared for 1 minute at a speed of 11500 r / min in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion.
[0075] Example 3
[0076] The present embodiment provides a method for preparing a pH-reversible polysaccharide-based double-layer emulsion, comprising the following steps:
[0077] S1. Solution preparation
[0078] Chitosan powder and carboxymethyl cellulose powder are taken respectively to prepare chitosan solution and carboxymethyl cellulose solution respectively.
[0079] In step S1, the preparation process of chitosan solution is: adding chitosan powder to water, then adding acetic acid aqueous solution, mixing and standing for 12 hours; the volume of acetic acid aqueous solution is 1% of the volume of water; the mass concentration of chitosan solution is 3%.
[0080] In step S1, the preparation process of the carboxymethyl cellulose solution is: adding carboxymethyl cellulose powder into boiling water and dissolving it for 30 minutes, and then standing for 12 hours to fully dissolve, to obtain a carboxymethyl cellulose solution with a mass concentration of 1.5%.
[0081] S2. Preparation of polysaccharide-based primary emulsion
[0082] Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution, wherein the volume of soybean oil is 20% of the volume of the mixed solution; and shear the mixed solution in a high-speed homogenizer at a speed of 11500r / min for 2min to obtain a polysaccharide-based primary emulsion.
[0083] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0084] The polysaccharide-based primary emulsion of step S2 and the carboxymethyl cellulose solution of step S1 are mixed, wherein the volume of the polysaccharide-based primary emulsion accounts for 30% of the total volume of the solution, and the total volume of the solution refers to the total volume of the polysaccharide-based primary emulsion and the carboxymethyl cellulose solution; the mixed solution is sheared for 1 minute at a speed of 11500 r / min in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion.
[0085] Example 4
[0086] The present embodiment provides a method for preparing a pH-reversible polysaccharide-based double-layer emulsion, comprising the following steps:
[0087] S1. Solution preparation
[0088] Chitosan powder and carboxymethyl cellulose powder are taken respectively to prepare chitosan solution and carboxymethyl cellulose solution respectively.
[0089] In step S1, the preparation process of chitosan solution is: adding chitosan powder to water, then adding acetic acid aqueous solution, mixing and standing for 12 hours; the volume of acetic acid aqueous solution is 1% of the volume of water; the mass concentration of chitosan solution is 3%.
[0090] In step S1, the preparation process of the carboxymethyl cellulose solution is: adding carboxymethyl cellulose powder into boiling water and dissolving it for 30 minutes, and then standing for 12 hours to fully dissolve, to obtain a carboxymethyl cellulose solution with a mass concentration of 1.5%.
[0091] S2. Preparation of polysaccharide-based primary emulsion
[0092] Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution, wherein the volume of soybean oil is 20% of the volume of the mixed solution; and shear the mixed solution in a high-speed homogenizer at a speed of 11500r / min for 2min to obtain a polysaccharide-based primary emulsion.
[0093] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0094] The polysaccharide-based primary emulsion of step S2 and the carboxymethyl cellulose solution of step S1 are mixed, wherein the volume of the polysaccharide-based primary emulsion accounts for 40% of the total volume of the solution, and the total volume of the solution refers to the total volume of the polysaccharide-based primary emulsion and the carboxymethyl cellulose solution; the mixed solution is sheared for 1 minute at a speed of 11500 r / min in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion.
[0095] Example 5
[0096] The present embodiment provides a method for preparing a pH-reversible polysaccharide-based double-layer emulsion, comprising the following steps:
[0097] S1. Solution preparation
[0098] Chitosan powder and carboxymethyl cellulose powder are taken respectively to prepare chitosan solution and carboxymethyl cellulose solution respectively.
[0099] In step S1, the preparation process of chitosan solution is: adding chitosan powder to water, then adding acetic acid aqueous solution, mixing and standing for 12 hours; the volume of acetic acid aqueous solution is 1% of the volume of water; the mass concentration of chitosan solution is 3%.
[0100] In step S1, the preparation process of the carboxymethyl cellulose solution is: adding carboxymethyl cellulose powder into boiling water and dissolving it for 30 minutes, and then standing for 12 hours to fully dissolve, to obtain a carboxymethyl cellulose solution with a mass concentration of 1.5%.
[0101] S2. Preparation of polysaccharide-based primary emulsion
[0102] Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution, wherein the volume of soybean oil is 20% of the volume of the mixed solution; and shear the mixed solution in a high-speed homogenizer at a speed of 11500r / min for 2min to obtain a polysaccharide-based primary emulsion.
[0103] S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion
[0104] The polysaccharide-based primary emulsion of step S2 and the carboxymethyl cellulose solution of step S1 are mixed, wherein the volume of the polysaccharide-based primary emulsion accounts for 50% of the total volume of the solution, and the total volume of the solution refers to the total volume of the polysaccharide-based primary emulsion and the carboxymethyl cellulose solution; the mixed solution is sheared for 1 minute at a speed of 11500 r / min in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion.
[0105] The following performance analysis tests were conducted on the pH-reversible polysaccharide-based double-layer emulsions prepared in Examples 1 to 5 above.
[0106] Test 1: Infrared spectroscopy analysis
[0107] Test samples: five groups of polysaccharide-based double-layer emulsions prepared in Examples 1 to 5, carboxymethyl cellulose (CMC) and chitosan (CS).
[0108] Test method: FTIR spectrometer (BRUKER, Vertex70, Karlsruhe Germany) was used to measure the -1 Resolution recording wavelength at 4000cm -1 ~400cm -1 Chitosan, carboxymethyl cellulose and different internal phases O / W 1 / W2 Infrared spectra of emulsions.
[0109] See also Figure 1 Compared with the hydroxyl peaks in the two polysaccharides (chitosan and carboxymethyl cellulose), the hydroxyl peaks in the water-in-water-in-oil double emulsion are significantly narrowed, indicating that a large number of hydroxyl groups are involved in the formation of the water-in-water-in-oil double emulsion. In addition, in the water-in-water-in-oil double emulsion, the characteristic peaks of amide I and amide II in chitosan and the asymmetric carboxyl peak in carboxymethyl cellulose disappear. -1 (10%~40%) and 1583cm -1 A new peak appeared at (50%), indicating that the amino groups in chitosan and the carboxyl groups in carboxymethyl cellulose had electrostatic interactions. -1 The intensity of the peaks near 2924 cm-1 decreases, which is due to the fact that more protonated amino groups in the internal phase interact with the carboxyl groups of carboxymethyl cellulose in the continuous phase. -1 、2855cm -1 and 1745cm -1 The peaks at 40° and 100° belong to the typical spectral bands of triglycerides in soybean oil. In summary, electrostatic interaction and hydrogen bonding are the main driving forces for the formation of water-in-water-in-oil bilayer emulsions.
[0110] Experiment 2: Microstructure Observation
[0111] Test samples: five groups of polysaccharide-based double-layer emulsions prepared in Examples 1 to 5.
[0112] Experimental method: For CLSM observation, 1 mL of O / W / W double-layer emulsion was stained with 50 μL of 0.1% Nile red solution (dissolved in 1,2-isopropanol, w / v) and 50 μL of a mixed fluorescent dye solution containing calcofluor white dye (w / v, 0.1%) and Nile red dye (w / v, 0.1%) in a 1:1 ratio. The stained sample was then dropped onto a glass slide and inverted onto the platform. Afterwards, the excitation wavelength of the laser was adjusted to the excitation wavelength of polysaccharides (405 nm) and the excitation wavelength of oil (488 nm). Finally, the sample was observed and recorded under a 10x magnifying glass.
[0113] See also Figure 2As shown, the green signal represents the oil droplets in the primary emulsion, and the blue signal represents the W / W interface formed by the electrostatic interaction of polysaccharides. It can be seen that the large blue droplets encapsulate the small green droplets, confirming the formation of the water-in-water-in-oil emulsion. This water-in-water-in-oil bilayer emulsion structure determines the function of the O / W / W bilayer emulsion to simultaneously encapsulate hydrophilic and hydrophobic substances. As the internal phase increases from 10% to 40%, the water-in-water-in-oil emulsion droplets increase. When the internal phase increases to 50%, the W / W interface breaks, and the primary emulsion in the bilayer emulsion flows into the continuous phase. This is mainly because there is not enough carboxyl in the continuous phase and amino in the dispersed phase to form a W / W interface.
[0114] Test 3: Rheological properties analysis
[0115] Test samples: five groups of polysaccharide-based double-layer emulsions prepared in Examples 1 to 5.
[0116] Test method: O / W was measured using a PP25 geometry rheometer (MCR 302, Anton Paar, Austria). 1 / W 2 Double emulsion and O / W with different pH values 1 / W 2 The double-layer emulsion was subjected to a frequency sweep test at a strain of 0.1%, and the frequency sweep range was 0.1-10 Hz.
[0117] See also Figure 3 It can be seen that as the internal phase increases from 10% to 40%, the storage modulus and loss modulus are also increasing; especially when the internal phase reaches 40%, the storage modulus and loss modulus reach the highest value, and the storage modulus is higher than the loss modulus, which is mainly because a large number of water-in-water-in-oil emulsion droplets form a dense gel network structure under this internal phase. When the internal phase continues to increase to 50%, the storage modulus and loss modulus decrease, which is mainly due to the primary emulsion flowing to the continuous phase after the water-in-water-in-oil double emulsion breaks, which reduces the viscoelasticity of the entire emulsion system.
[0118] Test 4: Stability analysis
[0119] Test samples: five groups of polysaccharide-based double-layer emulsions prepared in Examples 1 to 5.
[0120] Experimental method: In order to test the centrifugal stability, O / W with different internal phases were prepared in centrifuge tubes. 1 / W 2 Double emulsion. After the double emulsion was stored at room temperature for 12 hours, it was centrifuged at 3000 rpm for 10 minutes, and then the emulsion after centrifugation was imaged. 1 / W 2 The centrifugal stability was evaluated by the creaming index (CI) of the emulsion samples.
[0121] See also Figure 4 As shown in the figure, as the internal phase increases from 10% to 40%, the creaming index decreases continuously, indicating that the stability of the double emulsion continues to improve. In particular, when the internal phase is 40%, the creaming index reaches the lowest, indicating that the stability of the double emulsion is the highest at this internal phase, which is mainly due to the dense network structure formed, which hinders the separation of water and oil. Although the creaming index also reaches the lowest when the internal phase is 50%, the double emulsion flocculates after centrifugation, indicating that the stability of the double emulsion is poor at this internal phase, which is mainly due to the destruction of the network structure of the emulsion after demulsification.
[0122] Experiment 5: Microstructure of double-layer emulsions at different pH values (pH = 5 / 11 / 5)
[0123] Test samples: five groups of polysaccharide-based double-layer emulsions prepared in Examples 1 to 5.
[0124] Experimental method: First, adjust the pH of the O / W / W double emulsion (10%-40%) with different internal phases to 5; then adjust the pH of the O / W / W double emulsion from 5 to 11 with NaOH solution (0.5 mol / L), and finally adjust the pH of the O / W / W double emulsion from 11 to 5 with HCl solution (0.5 mol / L). During this process, observe the microstructure of the gel material, such as Figure 5 to Figure 7 In the figure, A to D are gel materials of Examples 1 to 4, respectively, and the subscripts 1 to 3 indicate that 1 is a double channel staining image, 2 is a single polysaccharide image in 1, and 3 is a single oil image in 1.
[0125] See also Figure 5 As shown, there is no difference between the microstructure of the double-layer emulsion at pH 5 and the microstructure of the double-layer emulsion that has not been pH-controlled. This is mainly because the pH of the double-layer emulsion is around 5.
[0126] See also Figure 6 As shown in the figure, at pH 11, all the bilayer emulsions shrank and the water content in the continuous phase increased. This was mainly because the hydroxide ions passed through the W / W interface into the O / W / W emulsion droplets and reacted with the chitosan in the dispersed phase to generate a large amount of water. This water passed through the W / W interface into the continuous phase of the O / W / W bilayer emulsion, increasing the volume of the continuous phase. Hydroxyl ions can smoothly pass through the W / W interface from the continuous phase of the O / W / W emulsion into the dispersed phase of the O / W / W emulsion, and water can pass through the W / W interface from the dispersed phase of the O / W / W emulsion into the continuous phase of the O / W / W emulsion, indicating that the W / W interface has a certain permeability.
[0127] See also Figure 7As shown in Figure 5, when the pH was adjusted from 11 to 5, the size of the O / W / W emulsion structure of the bilayer emulsion returned to normal. The O / W / W bilayer emulsion swelled, which may be because a large number of hydrogen ions entered the dispersed phase of the O / W / W bilayer emulsion from the continuous phase through the W / W interface, causing the chitosan in the internal phase to be recharged and dissolved in the W / W droplets, once again confirming the permeability of the W / W interfacial film.
[0128] In summary, the pH-reversible O / W / W bilayer emulsion has the structural property of encapsulating both hydrophilic and hydrophobic substances, and has potential application value in the encapsulation and delivery of hydrophilic and hydrophobic substances. In addition, the pH-reversible O / W / W bilayer emulsion has good structural recovery. The emulsion droplets shrink under strong alkaline conditions (pH 11). When the emulsion system returns to acidity (pH 5), the emulsion droplets swell and return to their normal size, indicating that the O / W / W bilayer emulsion has great application potential in acid-base pH response, and also shows that the W / W emulsion interface film has good structural shrinkage. In addition, since hydrogen ions and hydroxides can smoothly pass through the W / W interface, it shows that the W / W interface film has good permeability, so it has great application potential in biomimetic biomaterials.
[0129] In the embodiments of the present invention, the carboxyl polysaccharide used is carboxymethyl cellulose. When sodium alginate or pectin is used to replace carboxymethyl cellulose, the pH-reversible polysaccharide-based double-layer emulsion formed also has the same or similar properties and is used in biomimetic biomaterials.
[0130] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a pH-reversible polysaccharide-based double-layer emulsion, It is characterized in that The following steps are involved: S1. Solution preparation Taking chitosan powder and carboxyl polysaccharide powder respectively, and preparing chitosan solution and carboxyl polysaccharide solution respectively; S2. Preparation of polysaccharide-based primary emulsion Add soybean oil to the chitosan solution of step S1, mix well to obtain a mixed solution; and shear the mixed solution in a high-speed homogenizer to obtain a polysaccharide-based primary emulsion; the volume of the soybean oil is 20% to 40% of the volume of the mixed solution, and the mass concentration of the chitosan solution is 3% to 5%; S3. Preparation of pH-reversible polysaccharide-based double-layer emulsion After mixing the polysaccharide-based primary emulsion of step S2 with the carboxyl polysaccharide solution of step S1, the obtained mixture is sheared in a high-speed homogenizer to obtain a pH-reversible polysaccharide-based double-layer emulsion; the volume of the polysaccharide-based primary emulsion is 10% to 50% of the volume of the mixture; and the mass concentration of the carboxyl polysaccharide solution is 1% to 2%.
2. The method for preparing the pH-reversible polysaccharide-based double-layer emulsion according to claim 1, It is characterized in that In step S1, the preparation process of chitosan solution is: chitosan powder is added to water, and then acetic acid aqueous solution is added, mixed and allowed to stand for 12h to 24h; the volume of acetic acid aqueous solution is 1% of the volume of water.
3. The method for preparing the pH-reversible polysaccharide-based double-layer emulsion according to claim 1, It is characterized in that In step S1, the preparation process of the carboxyl polysaccharide solution is: adding the carboxyl polysaccharide powder into boiling water and dissolving it for 20 minutes to 40 minutes, and then standing it for 12 hours to 24 hours.
4. The method for preparing a polysaccharide-based water-in-water emulsion gel based on combined phase separation according to claim 3, It is characterized in that The carboxyl polysaccharide is carboxymethyl cellulose, sodium alginate or pectin.
5. The method for preparing the pH-reversible polysaccharide-based double-layer emulsion according to claim 1, It is characterized in that In the step S2, the shearing is performed at a rotation speed of 11500 r / min to 14500 r / min for 2 min to 3 min.
6. The method for preparing the pH-reversible polysaccharide-based double-layer emulsion according to claim 1, It is characterized in that In step S3, the shearing is performed at a rotation speed of 11500 r / min to 14500 r / min for 1 min to 2 min.
7. A pH-reversible polysaccharide-based double-layer emulsion prepared by the method for preparing a pH-reversible polysaccharide-based double-layer emulsion according to any one of claims 1 to 6.
8. The pH-reversible polysaccharide-based double-layer emulsion according to claim 7, It is characterized in that When the pH of the pH-reversible polysaccharide-based double-layer emulsion is adjusted from 5 to 11, the double-layer emulsion droplets shrink and become smaller; when the pH is adjusted from 11 to 5, the size of the double-layer emulsion droplets returns to normal.
9. Use of the pH-reversible polysaccharide-based double-layer emulsion as claimed in claim 7 in the co-encapsulation of hydrophilic and hydrophobic substances.